Flame-retardant waterborne polyurethane coating as well as preparation method and application thereof

By modifying the combination of water-based polyurethane resin and other materials, water-based polyurethane coatings with excellent flame retardant properties and thermal stability are prepared, which solves the problems of poor heat resistance of water-based polyurethane coatings and unenvironmental halogen flame retardants, and achieves environmental protection, High performance coating preparation.

CN118995030AInactive Publication Date: 2024-11-22BEIJING EONZEAL WATERPROOF MATERIAL CO LTD

Patent Information

Application Number
CN202411388396.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing water-based polyurethane coatings have poor heat resistance, and the addition of flame retardants such as halogen is not environmentally friendly, which is prone to toxic gases and endanger human health.

Method used

The flame-retardant water-based polyurethane coating is prepared through specific mixing and treatment methods to improve its flame-retardant water-based polyurethane coatings. Flame retardant properties, thermal stability and mechanical properties.

Benefits of technology

It significantly improves the flame retardant properties, thermal stability and mechanical properties of water-based polyurethane coatings, reduces the harm to the environment and the human body, and is suitable for decoration materials and other applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of waterborne polyurethane coatings, and discloses a flame-retardant waterborne polyurethane coating as well as a preparation method and application thereof. The flame-retardant waterborne polyurethane coating is prepared from the following raw materials in parts by mass: 50 to 70 parts of modified waterborne polyurethane resin, 1.5 to 3 parts of hollow glass beads, 0.5 to 1.5 parts of cellulose nanocrystals, 6 to 12 parts of gelatin, 6 to 8 parts of polysiloxane, 2 to 10 parts of filler and 2 to 5 parts of modified graphene oxide. The flame retardant property of the waterborne polyurethane coating is improved under the mutual effect and common influence of various raw materials, the use of harmful flame retardants such as halogen is avoided, and the generation of harmful gases is reduced. Meanwhile, the waterborne polyurethane coating provided by the invention also has excellent water resistance and paint film adhesion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterborne polyurethane coatings, and in particular to a flame retardant waterborne polyurethane coating and a preparation method and application thereof. Background Art

[0002] Coating is a material specially used for coating on the surface of protected or decorated objects, which can form a firmly attached continuous film. Coating is also called paint in China. It is a liquid or solid material that can be coated on the surface of an object to form a continuous and solid film. It is usually mainly composed of resin, oil, and emulsion, with or without pigments and fillers, and corresponding additives. Coatings can be classified in many ways according to their uses, film-forming substances, etc., such as art-specified pigments, paints, and cosmetic products. In the field of construction, coatings can be used for wall decoration, protection, and heat insulation. In the field of household goods, coatings can be used for surface decoration and protection of furniture, floors, and kitchen and bathroom products. In the field of automobiles and ships, coatings are used to improve aesthetics and extend service life. In the industrial field, coatings can be used for the protection and beautification of mechanical equipment, packaging, and electronic products. With the improvement of environmental protection laws and regulations in various countries and the enhancement of people's environmental awareness, the emission of volatile organic compounds and harmful air pollutants in traditional solvent-based coatings has been subject to increasingly stringent restrictions. Therefore, the development of low-pollution, high-performance, and multi-functional environmentally friendly water-based coatings has become the main direction of coating technology development.

[0003] Polyurethane coatings include solvent-based polyurethane coatings and water-based polyurethane coatings. Solvent-based polyurethane coatings are widely used in daily life due to their excellent wear resistance, mechanical properties, water resistance, etc. However, due to the volatilization of a large amount of organic solvents (toluene, xylene, etc.), they cause irreversible damage to the environment and its construction workers, and their application is limited. Waterborne polyurethane (WPU) is a new type of polyurethane system that uses water instead of organic solvents as a dispersion medium, also known as water-dispersed polyurethane, water-based polyurethane or water-based polyurethane. Waterborne polyurethane uses water as a solvent and has the advantages of being pollution-free, safe and reliable, having excellent mechanical properties, good compatibility, and easy to modify. There are many types of waterborne polyurethanes, which have the advantages of strong functionality, weak volatility, low odor, and good wear resistance, and are widely used in all walks of life. However, due to the poor water resistance, heat resistance, and flame retardancy of waterborne polyurethane, the development of waterborne polyurethane is limited to a certain extent.

[0004] At present, in order to improve the flame retardancy of waterborne polyurethane coatings, two basic flame retardant systems have been designed: halogen flame retardant system and non-halogen flame retardant system. Waterborne polyurethane materials added with halogen flame retardants will produce thick smoke and harmful substances such as hydrogen halides when burned, which can cause suffocation. In terms of non-halogen flame retardant systems, metal hydroxide flame retardants are added in large amounts and have poor dispersibility, and high filling amounts cause serious damage to mechanical properties; phosphorus-nitrogen flame retardants such as aluminum hypophosphite have high flame retardant efficiency, but phosphorus flame retardants are flammable and have poor compatibility. They are easy to migrate and precipitate in waterborne coatings, affecting the appearance and comprehensive performance of the products, which to a certain extent limits their scope of application and application effects. Therefore, how to prepare an environmentally friendly and flame-retardant waterborne polyurethane coating has become a technical problem that needs to be solved at present. Summary of the invention

[0005] In view of this, the present invention proposes a flame retardant waterborne polyurethane coating and a preparation method and application thereof, so as to solve the problems in the prior art that the waterborne polyurethane coating has poor heat resistance, the addition of flame retardants such as halogen is not environmentally friendly, and it is easy to produce toxic gases and endanger human health.

[0006] The present invention provides a flame retardant waterborne polyurethane coating, which is prepared from raw materials containing the following parts by weight: 50-70 parts of modified waterborne polyurethane resin, 1.5-3 parts of hollow glass beads, 0.5-1.5 parts of cellulose nanocrystals, 6-12 parts of gelatin, 6-8 parts of polysiloxane, 2-10 parts of filler and 2-5 parts of modified graphene oxide.

[0007] Furthermore, the modified waterborne polyurethane resin comprises the following raw materials in parts by mass: 55-65 parts of organophosphorus polyester polyol, 36-45 parts of trimethylene diisocyanate, 3-4.5 parts of neopentyl glycol, 2-5 parts of sodium ethylenediamine sulfonate, 3-4 parts of pentaerythritol, 0.8-1.2 parts of sodium o-phenylphenol, 3-4 parts of N-ethyldiethanolamine, and 5-6 parts of bis(2-hydroxypropyl)aniline.

[0008] Furthermore, the preparation method of the modified waterborne polyurethane resin comprises the following steps: (a) mixing organophosphorus polyester polyol, trimethylene diisocyanate, neopentyl glycol, sodium ethylenediamine sulfonate, pentaerythritol, sodium o-phenylphenol and N,N-dimethylformamide uniformly to obtain a mixture; (b) The mixed material, N-ethyldiethanolamine and bis(2-hydroxypropyl)aniline are mixed and the pH is adjusted to neutral to obtain a modified waterborne polyurethane resin.

[0009] Furthermore, the filler comprises the following raw materials in parts by weight: 2-8 parts of tourmaline powder, 10-15 parts of talc, 5-8 parts of kaolin, 5-10 parts of expanded perlite, and 10-15 parts of diatomaceous earth.

[0010] Furthermore, the modified graphene oxide is obtained by the following preparation method: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 are mixed by ultrasound, and then sodium acetate solution is added to the system and heated and stirred to obtain modified graphene oxide.

[0011] Furthermore, the temperature of the mixed ultrasound is 55-70°C, and the time of the mixed ultrasound is 30-60min; The heating and stirring temperature is 150-195° C., and the heating and stirring time is 15-25 h.

[0012] Furthermore, the molar ratio of the 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine, La(NO3)3 and the sodium acetate in the sodium acetate solution is 1:1-1.4:1.2-1.5.

[0013] The present invention also provides a method for preparing the flame retardant waterborne polyurethane coating, comprising the following steps: The flame-retardant waterborne polyurethane coating is obtained by mixing modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide.

[0014] Furthermore, the mixing temperature is 60-80° C., and the mixing time is 2-3 hours.

[0015] The present invention also provides application of the flame-retardant water-based polyurethane coating in decoration materials.

[0016] Compared with the prior art, the present invention has the following beneficial effects: The invention provides a flame retardant waterborne polyurethane coating, which is prepared from the following raw materials in parts by mass: 50-70 parts of modified waterborne polyurethane resin, 1.5-3 parts of hollow glass beads, 0.5-1.5 parts of cellulose nanocrystals, 6-12 parts of gelatin, 6-8 parts of polysiloxane, 2-10 parts of filler and 2-5 parts of modified graphene oxide.

[0017] The modified waterborne polyurethane of the present invention has long carbon side chains and phosphorus-containing groups of organic phosphorus polyester polyol and trimethylene diisocyanate, and the side chain groups are intertwined with each other, thereby improving the mechanical strength of the waterborne polyurethane, especially increasing the toughness and tensile strength of the waterborne polyurethane, and alleviating the problem of softening of the coating and reduced adhesion due to the phosphorus-containing groups. At the same time, the trimethylene diisocyanate has isocyanurate hexacyclic ring and organosilicon group, has a strong electron-withdrawing effect, improves the crosslinking degree, further improves the adhesion of the waterborne polyurethane coating, and has phosphorus-containing groups, thereby improving the flame retardancy of the waterborne polyurethane coating; the four hydroxyl groups in pentaerythritol react with -NCO, promote further crosslinking of the waterborne polyurethane, generate a polyurethane with a crosslinked network structure, and improve the mechanical strength and thermal stability of the waterborne polyurethane. At the same time, a large crosslinking degree makes the intermolecular gap smaller, and it is difficult for water molecules to enter the interior of the polyurethane molecules, thereby improving the water resistance of the waterborne polyurethane coating.

[0018] The present invention also adds hollow glass beads, tourmaline powder, talcum powder, kaolin, expanded perlite and diatomaceous earth, which cooperate with each other to greatly improve the strength, wear resistance and corrosion resistance of the waterborne polyurethane coating. At the same time, these materials have a lower thermal conductivity, which further improves the flame retardant performance of the waterborne polyurethane coating. And by utilizing its large specific surface area and open-pore structure, the obtained waterborne polyurethane coating has a strong adsorption capacity, can adsorb harmful dust and purify the air.

[0019] The present invention also adds cellulose nanocrystals and gelatin to improve the mechanical properties of the waterborne polyurethane coating, especially the tensile strength and thermal stability of the coating. Polysiloxane is also added to further improve the flame retardancy of the coating.

[0020] The present invention also adds modified graphene oxide, which has a porous crystal structure and can promote heat conduction. The graphene oxide has excellent thermal conductivity, which greatly improves the thermal conduction and thermal stability of the waterborne polyurethane coating. The modified graphene oxide will thermally decompose at high temperature to produce rare earth metal lanthanum oxide, which promotes the catalytic performance of the carbonization reaction. At the same time, a dense carbon layer will be formed on the surface of the graphene oxide during the combustion process. Under the combined action of the two, the dense graphitized carbon layer generated on the surface of the waterborne polyurethane coating will hinder the conduction of heat and oxygen, inhibit further combustion, and thus increase the flame retardant performance of the waterborne polyurethane coating.

[0021] The flame retardant waterborne polyurethane coating provided by the invention has excellent flame retardant performance, thermal stability and tensile strength.

[0022] The present invention also provides a method for preparing a flame-retardant waterborne polyurethane coating, comprising the following steps: (1) mixing a modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, a filler, and modified graphene oxide to obtain the flame-retardant waterborne polyurethane coating. The method for preparing the waterborne polyurethane coating provided by the present invention is simple, easy to operate, suitable for large-scale production, and does not use halogen reagents, thereby significantly reducing pollution to the environment and harm to the human body. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] The present invention provides a flame retardant waterborne polyurethane coating, which is prepared from raw materials containing the following parts by weight: 50-70 parts of modified waterborne polyurethane resin, 1.5-3 parts of hollow glass beads, 0.5-1.5 parts of cellulose nanocrystals, 6-12 parts of gelatin, 6-8 parts of polysiloxane, 2-10 parts of filler and 2-5 parts of modified graphene oxide.

[0025] In one embodiment, the weight fraction of the modified waterborne polyurethane resin is preferably 50-70 parts, more preferably 55-65 parts, and more preferably 58-62 parts.

[0026] In one embodiment, the mass fraction of the hollow glass beads is preferably 1.5-3 parts, more preferably 1.8-2.7 parts, and more preferably 2-2.5 parts.

[0027] In one embodiment, the weight fraction of the cellulose nanocrystals is preferably 0.5-1.5 parts, more preferably 0.7-1.3 parts, and more preferably 0.9-1.1 parts.

[0028] In one embodiment, the mass fraction of the gelatin is preferably 6-12 parts, further preferably 7-11 parts, and more preferably 9-10 parts.

[0029] In one embodiment, the weight fraction of the polysiloxane is preferably 6-8 parts, more preferably 6.5-7.5 parts, and more preferably 6.8-7.2 parts.

[0030] In one embodiment, the weight percentage of the filler is preferably 2-10 parts, more preferably 3-9 parts, and more preferably 4-8 parts.

[0031] In one embodiment, the mass fraction of the modified graphene oxide is preferably 2-5 parts, more preferably 3-4 parts, and more preferably 3.2-3.8 parts.

[0032] In one embodiment, the modified waterborne polyurethane resin comprises the following raw materials in parts by weight: 55-65 parts of organophosphorus polyester polyol, 36-45 parts of trimethylene diisocyanate, 3-4.5 parts of neopentyl glycol, 2-5 parts of sodium ethylenediamine sulfonate, 3-4 parts of pentaerythritol, 0.8-1.2 parts of sodium o-phenylphenol, 3-4 parts of N-ethyldiethanolamine, and 5-6 parts of bis(2-hydroxypropyl)aniline.

[0033] In one embodiment, the mass fraction of the organophosphorus polyester polyol is preferably 55-65 parts, more preferably 57-63 parts, and more preferably 58-62 parts.

[0034] In one embodiment, the weight fraction of trimylene diisocyanate is preferably 36-45 parts, more preferably 38-42 parts, and more preferably 39-41 parts.

[0035] In one embodiment, the mass fraction of the neopentyl glycol is preferably 3-4.5 parts, more preferably 3.2-4.3 parts, and more preferably 3.5-4 parts.

[0036] In one embodiment, the mass fraction of the sodium ethylenediaminesulfonate is preferably 2-5 parts, more preferably 3-4 parts, and more preferably 3.2-3.8 parts.

[0037] In one embodiment, the mass fraction of pentaerythritol is preferably 3-4 parts, more preferably 3.2-3.8 parts, and more preferably 3.4-3.6 parts.

[0038] In one embodiment, the mass fraction of the sodium o-phenylphenolate is preferably 0.8-1.2 parts, more preferably 0.9-1.1 parts, and more preferably 1 part.

[0039] In one embodiment, the mass fraction of the N-ethyldiethanolamine is preferably 3-4 parts, more preferably 3.2-3.8 parts, and more preferably 3.4-3.6 parts.

[0040] In one embodiment, the weight fraction of the bis(2-hydroxypropyl)aniline is preferably 5-6 parts, more preferably 5.2-5.8 parts, and more preferably 5.4-5.6 parts.

[0041] In one embodiment, the method for preparing the organophosphorus polyester polyol comprises the following steps: After mixing 2-phospho-1,2,4-tricarboxybutane and 1,6-hexanediol, N2 is introduced as a protective gas, and then the temperature is raised to 107-110°C and kept warm for 1.5-1.8 hours. Tributyltin oxide is then added, and the temperature is raised to 165-168°C and kept warm for 4-5 hours. The organic phosphorus polyester polyol is obtained by vacuum heat preservation for 2-3 hours.

[0042] In one embodiment, the preparation method of the modified waterborne polyurethane resin comprises the following steps: (a) mixing organophosphorus polyester polyol, trimethylene diisocyanate, neopentyl glycol, sodium ethylenediamine sulfonate, pentaerythritol, sodium o-phenylphenol and N,N-dimethylformamide uniformly to obtain a mixture; (b) The mixed material, N-ethyldiethanolamine and bis(2-hydroxypropyl)aniline are mixed and the pH is adjusted to neutral to obtain a modified waterborne polyurethane resin.

[0043] In one embodiment, in step (a), the organophosphorus polyester polyol and trimerylene diisocyanate are preliminarily mixed, and then neopentyl glycol, sodium ethylenediamine sulfonate, pentaerythritol, sodium o-phenylphenol and N,N-dimethylformamide are added and mixed uniformly to obtain a mixture. The temperature of the preliminarily mixing is preferably 75° C., and the time of the preliminarily mixing is preferably 5-6 hours; the temperature of the mixing is preferably 70-80° C., and the time of the mixing is preferably 5-6 hours.

[0044] In one embodiment, the mixing temperature of the mixed material, N-ethyldiethanolamine and bis(2-hydroxypropyl)aniline in step (b) is preferably 70-75° C., and the mixing time is preferably 4-5 h.

[0045] In one embodiment, the filler comprises the following raw materials in parts by weight: 2-8 parts of tourmaline powder, 10-15 parts of talc, 5-8 parts of kaolin, 5-10 parts of expanded perlite, and 10-15 parts of diatomaceous earth.

[0046] In one embodiment, the mass fraction of the tourmaline powder is preferably 2-8 parts, more preferably 3-7 parts, and more preferably 4-6 parts.

[0047] In one embodiment, the mass fraction of the talc powder is preferably 10-15 parts, more preferably 11-14 parts, and more preferably 12-13 parts.

[0048] In one embodiment, the mass fraction of the kaolin is preferably 5-8 parts, more preferably 6-7 parts, and more preferably 6.2-6.8 parts.

[0049] In one embodiment, the mass fraction of the expanded perlite is preferably 5-10 parts, more preferably 6-9 parts, and more preferably 7-8 parts.

[0050] In one embodiment, the mass fraction of the diatomaceous earth is preferably 10-15 parts, more preferably 11-14 parts, and more preferably 12-13 parts.

[0051] In one embodiment, the modified graphene oxide is obtained by the following preparation method: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 are mixed by ultrasound, and then sodium acetate solution is added to the system and heated and stirred to obtain modified graphene oxide.

[0052] In one embodiment, the temperature of the mixed ultrasound is preferably 55-70°C, more preferably 58-67°C, more preferably 60-65°C, and the time of the mixed ultrasound is preferably 30-60min, more preferably 35-55min, more preferably 40-50min; The heating and stirring temperature is preferably 150-195°C, more preferably 160-185°C, more preferably 165-180°C, and the heating and stirring time is preferably 15-25h, more preferably 18-22h, more preferably 19-21h.

[0053] In one embodiment, the molar ratio of the 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine, La(NO3)3 and sodium acetate in the sodium acetate solution is preferably 1:1-1.4:1.2-1.5, further preferably 1:1.1-1.3:1.3-1.4, and more preferably 1:1.2:1.35.

[0054] The present invention also provides a method for preparing the flame retardant waterborne polyurethane coating, comprising the following steps: The flame-retardant waterborne polyurethane coating is obtained by mixing modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide.

[0055] In one embodiment, the mixing temperature is preferably 60-80°C, more preferably 65-75°C, more preferably 68-72°C, and the mixing time is preferably 2-3h, more preferably 2.2-2.8h, more preferably 2.4-2.6h.

[0056] The present invention also provides application of the flame-retardant water-based polyurethane coating in decoration materials.

[0057] The technical solution of the present invention will be explained and illustrated through specific embodiments below. Example 1

[0058] A flame retardant waterborne polyurethane coating is prepared from the following raw materials in parts by weight: 50 parts of modified waterborne polyurethane resin, 1.5 parts of hollow glass beads, 0.5 parts of cellulose nanocrystals, 6 parts of gelatin, 6 parts of polysiloxane, 2 parts of filler, and 2 parts of modified graphene oxide; Among them, the filler includes: 2 parts of tourmaline powder, 10 parts of talc, 5 parts of kaolin, 5 parts of expanded perlite, and 10 parts of diatomaceous earth.

[0059] Preparation of organophosphorus polyester polyols: After mixing 2-phospho-1,2,4-tricarboxybutane and 1,6-hexanediol, N2 was introduced as a protective gas, and then the temperature was raised to 107°C and kept warm for 1.5 hours. Tributyltin oxide was then added, and the temperature was raised to 165°C and kept warm for 4 hours. The organic phosphorus polyester polyol was obtained by vacuum heat preservation for 2 hours.

[0060] Preparation of modified waterborne polyurethane resin: (a) 55 parts of organophosphorus polyester polyol and 36 parts of trimethylene diisocyanate were preliminarily mixed at 75°C for 5 hours, then the system was cooled to 40°C, and then 3 parts of neopentyl glycol, 2 parts of sodium ethylenediamine sulfonate, 3 parts of pentaerythritol, 0.8 parts of sodium o-phenylphenol and N,N-dimethylformamide were added and mixed at 70°C for 5 hours to obtain a uniform mixture.

[0061] (b) The mixed material system was cooled to 40° C., 3 parts of N-ethyldiethanolamine and 5 parts of bis(2-hydroxypropyl)aniline were added, and then mixed at 70° C. for 4 hours to obtain a modified waterborne polyurethane resin.

[0062] Modified graphene oxide: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 were mixed and ultrasonicated at 55°C for 30 minutes, and then sodium acetate solution was added to the system, the temperature was raised to 150°C, and the modified graphene oxide was obtained by heating and stirring for 15 hours.

[0063] Among them, the molar ratio of 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine, La(NO3)3 and sodium acetate in the sodium acetate solution is preferably 1:1:1.2.

[0064] Preparation of flame retardant waterborne polyurethane coating: The flame-retardant waterborne polyurethane coating is obtained by mixing the modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide at a temperature of 60° C. for 2 hours. Example 2

[0065] A flame retardant waterborne polyurethane coating is prepared from the following raw materials in parts by weight: 70 parts of modified waterborne polyurethane resin, 3 parts of hollow glass beads, 1.5 parts of cellulose nanocrystals, 12 parts of gelatin, 8 parts of polysiloxane, 10 parts of filler, and 5 parts of modified graphene oxide; Wherein, the filler comprises: 8 parts of tourmaline powder, 15 parts of talc, 8 parts of kaolin, 10 parts of expanded perlite, and 15 parts of diatomaceous earth.

[0066] Preparation of organophosphorus polyester polyols: After mixing 2-phospho-1,2,4-tricarboxybutane and 1,6-hexanediol, N2 was introduced as a protective gas, and then the temperature was raised to 110°C and kept warm for 1.8 hours. Tributyltin oxide was then added, and the temperature was raised to 168°C and kept warm for 4 hours. The organic phosphorus polyester polyol was obtained by vacuum heat preservation for 2 hours.

[0067] Preparation of modified waterborne polyurethane resin: (a) 65 parts of organophosphorus polyester polyol and 45 parts of trimethylene diisocyanate were preliminarily mixed at 75°C for 5 hours, then the system was cooled to 40°C, and then 4.5 parts of neopentyl glycol, 5 parts of sodium ethylenediamine sulfonate, 3 parts of pentaerythritol, 1 part of sodium o-phenylphenol and N,N-dimethylformamide were added and mixed at 70°C for 5 hours to obtain a uniform mixture.

[0068] (b) The mixed material system was cooled to 40° C., 3 parts of N-ethyldiethanolamine and 5 parts of bis(2-hydroxypropyl)aniline were added, and then mixed at 70° C. for 4 hours to obtain a modified waterborne polyurethane resin.

[0069] Modified graphene oxide: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 were mixed and ultrasonicated at 55°C for 30 minutes, and then sodium acetate solution was added to the system, the temperature was raised to 150°C, and the modified graphene oxide was obtained by heating and stirring for 15 hours.

[0070] Among them, the molar ratio of 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine, La(NO3)3 and sodium acetate in the sodium acetate solution is preferably 1:1.4:1.5.

[0071] Preparation of flame retardant waterborne polyurethane coating: The flame-retardant waterborne polyurethane coating is obtained by mixing the modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide at a temperature of 75° C. for 3 hours. Example 3

[0072] A flame retardant waterborne polyurethane coating is prepared from the following raw materials in parts by weight: 65 parts of modified waterborne polyurethane resin, 2 parts of hollow glass beads, 1 part of cellulose nanocrystals, 8 parts of gelatin, 7 parts of polysiloxane, 5 parts of filler, and 4 parts of modified graphene oxide; Wherein, the filler comprises: 6 parts of tourmaline powder, 12 parts of talc, 7 parts of kaolin, 8 parts of expanded perlite, and 12 parts of diatomaceous earth.

[0073] Preparation of organophosphorus polyester polyols: After mixing 2-phospho-1,2,4-tricarboxybutane and 1,6-hexanediol, N2 was introduced as a protective gas, and then the temperature was raised to 110°C and kept warm for 1.8 hours. Tributyltin oxide was then added, and the temperature was raised to 168°C and kept warm for 4 hours. The organic phosphorus polyester polyol was obtained by vacuum heat preservation for 2 hours.

[0074] Preparation of modified waterborne polyurethane resin: (a) 58 parts of organophosphorus polyester polyol and 40 parts of trimethylene diisocyanate were preliminarily mixed at 75°C for 5 hours, then the system was cooled to 40°C, and then 4 parts of neopentyl glycol, 4 parts of sodium ethylenediamine sulfonate, 3.5 parts of pentaerythritol, 1.2 parts of sodium o-phenylphenol and N,N-dimethylformamide were added and mixed at 70°C for 5 hours to obtain a uniform mixture.

[0075] (b) The mixed material system was cooled to 40° C., 4 parts of N-ethyldiethanolamine and 6 parts of bis(2-hydroxypropyl)aniline were added, and then mixed at 70° C. for 4 hours to obtain a modified waterborne polyurethane resin.

[0076] Modified graphene oxide: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 were mixed and ultrasonicated at 55°C for 30 minutes, and then sodium acetate solution was added to the system, the temperature was raised to 150°C, and the modified graphene oxide was obtained by heating and stirring for 15 hours.

[0077] Among them, the molar ratio of 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine, La(NO3)3 and sodium acetate in the sodium acetate solution is preferably 1:1.2:1.5.

[0078] Preparation of flame retardant waterborne polyurethane coating: The flame-retardant waterborne polyurethane coating is obtained by mixing the modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide at a temperature of 80° C. for 2.5 hours.

[0079] Performance Testing The flame retardant waterborne polyurethane coatings obtained in Examples 1-3 were subjected to performance tests, and the specific results are shown in Table 1: Among them, the oxygen index is tested according to GB / T2406-1993; the vertical burning performance test is carried out according to GB / T2408-1994; the water resistance test is carried out according to GB / T6753.3-1986; and the paint adhesion test is carried out according to GB / T1720-1989.

[0080] Table 1 Performance test results of flame retardant waterborne polyurethane coatings obtained in Examples 1-3 Oxygen Index Total burning time Flame retardant grade Water resistance Paint film adhesion Example 1 33.4 2s V-0 No abnormality Level 1 Example 2 35.2 2s V-0 No abnormality Level 1 Example 3 36.5 2s V-0 No abnormality Level 1 It can be seen from Table 1 that the flame retardant waterborne polyurethane coating provided by the present invention has excellent flame retardancy, water resistance and paint surface adhesion. The oxygen index is in the range of 33.4-36.5, the total burning time is 2s, the flame retardancy grade is V-0, and the paint surface adhesion is grade 1.

[0081] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A flame retardant waterborne polyurethane coating, characterized in that: Prepared from the following raw materials in parts by weight: 50-70 parts of modified waterborne polyurethane resin, 1.5-3 parts of hollow glass beads, 0.5-1.5 parts of cellulose nanocrystals, 6-12 parts of gelatin, 6-8 parts of polysiloxane, 2-10 parts of filler and 2-5 parts of modified graphene oxide.

2. A flame retardant waterborne polyurethane coating according to claim 1, characterized in that: The modified waterborne polyurethane resin comprises the following raw materials in parts by mass: 55-65 parts of organophosphorus polyester polyol, 36-45 parts of trimethylene diisocyanate, 3-4.5 parts of neopentyl glycol, 2-5 parts of sodium ethylenediamine sulfonate, 3-4 parts of pentaerythritol, 0.8-1.2 parts of sodium o-phenylphenol, 3-4 parts of N-ethyldiethanolamine, and 5-6 parts of bis(2-hydroxypropyl)aniline.

3. A flame retardant waterborne polyurethane coating according to claim 2, characterized in that: The preparation method of the modified waterborne polyurethane resin comprises the following steps: (a) mixing organophosphorus polyester polyol, trimethylene diisocyanate, neopentyl glycol, sodium ethylenediamine sulfonate, pentaerythritol, sodium o-phenylphenol and N,N-dimethylformamide uniformly to obtain a mixture; (b) The mixed material, N-ethyldiethanolamine and bis(2-hydroxypropyl)aniline are mixed and the pH is adjusted to neutral to obtain a modified waterborne polyurethane resin.

4. A flame retardant waterborne polyurethane coating according to claim 2 or 3, characterized in that: The filler comprises the following raw materials in parts by weight: 2-8 parts of tourmaline powder, 10-15 parts of talc, 5-8 parts of kaolin, 5-10 parts of expanded perlite, and 10-15 parts of diatomaceous earth.

5. A flame retardant waterborne polyurethane coating according to claim 4, characterized in that: The modified graphene oxide is obtained by the following preparation method: N,N-dimethylformamide solvent, graphene oxide, 2,4,6-tris[(p-carboxyphenyl)amino]-1,3,5-triazine and La(NO3)3 are mixed by ultrasound, and then sodium acetate solution is added to the system and heated and stirred to obtain modified graphene oxide.

6. The flame retardant waterborne polyurethane coating according to claim 5, characterized in that: The temperature of the mixed ultrasound is 55-70°C, and the time of the mixed ultrasound is 30-60min; The heating and stirring temperature is 150-195° C., and the heating and stirring time is 15-25 h.

7. A flame retardant waterborne polyurethane coating according to claim 5 or 6, characterized in that: The molar ratio of the 2,4,6-tris[(p-carboxylphenyl)amino]-1,3,5-triazine, La(NO3)3 and the sodium acetate in the sodium acetate solution is 1:1-1.4:1.2-1.

5.

8. The method for preparing a flame retardant waterborne polyurethane coating according to any one of claims 1 to 7, characterized in that: It includes the following steps: The flame-retardant waterborne polyurethane coating is obtained by mixing modified waterborne polyurethane resin, hollow glass beads, cellulose nanocrystals, gelatin, polysiloxane, filler and modified graphene oxide.

9. The method for preparing a flame retardant waterborne polyurethane coating according to claim 8, characterized in that: The mixing temperature is 60-80° C., and the mixing time is 2-3 hours.

10. Use of the flame retardant waterborne polyurethane coating according to any one of claims 1 to 7 in decoration materials.

Citation Information

Patent Citations

  • Flame-retardant water-based polyurethane paint

    CN105505180A

  • Flame-retardant waterborne polyurethane coating

    CN109705719A

  • High-flame-retardant waterborne polyurethane coating and preparation method thereof

    CN111500175A

  • Flame-retardant and heat-resistant waterborne polyurethane coating and preparation method thereof

    CN111777887A

Cited By

  • Waterborne polyurethane wear-resistant coating and preparation method thereof

    CN119859463A