High-conductivity, stable-shape, high-heat-conductivity, leakage-proof and joule-heating photoelectric double-trigger phase change material based on copper net and preparation method thereof

By using materials such as copper mesh and carbon nanotubes in phase change materials, combined with the flexible support of SEBS, the problems of poor thermal conductivity and easy leakage are solved, and photoelectricity with high conductivity, high thermal conductivity, stable shape, leakage prevention and Joule heating are achieved Dual trigger phase change material, suitable for complex application scenarios.

CN118995145APending Publication Date: 2024-11-22LIAONING UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411095191.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing phase change materials have defects in poor thermal conductivity and easy leakage, which is difficult to meet the needs of complex application scenarios for high conductivity, stable shape, high thermal conductivity, anti-leakage, and Joule heating.

Method used

The copper mesh is used as the conductive and thermal network, and carbon nanotubes, polyethanol 10000 and styrene-butene-butadiene-styrene copolymer SEBS are introduced to achieve effective packaging through the flexible support of the copper-based three-dimensional network and SEBS. The high conductivity and high thermal conductivity of copper mesh and carbon nanotubes realize the dual functions of Joule heating and photothermal conversion.

Benefits of technology

It improves the conductivity, thermal conductivity, shape stability and leakage resistance of phase change materials, realizes Joule heating and light-heat conversion functions, and is suitable for applications such as battery preheating and personal thermal management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004987710830000011
    Figure HDA0004987710830000011
  • Figure HDA0004987710830000012
    Figure HDA0004987710830000012
  • Figure HDA0004987710830000021
    Figure HDA0004987710830000021
Patent Text Reader

Abstract

The invention belongs to the field of organic materials, and particularly relates to a photoelectric double-trigger phase change material which is based on a copper net, high in conductivity, stable in shape, high in heat conductivity, leakproof and Joule-heating and a preparation method of the photoelectric double-trigger phase change material. The photoelectric double-trigger phase change material provided by the invention takes a copper net as a substrate, and carbon nanotubes (CNTs), polyethylene glycol 10000 (PEG10000) and a styrene-butylene-butadiene-styrene copolymer (SEBS) are introduced on the basis of the copper net to obtain the photoelectric double-trigger phase change material which is high in conductivity, stable in shape, high in heat conductivity, leakproof and Joule-heating. According to the preparation method, raw materials are easy to obtain, operation is easy and convenient, and the obtained phase change material has the performance of high electric conductivity, stable shape, high heat conductivity, leakage prevention, Joule heating and the like and has certain application prospects in the fields of battery preheating, personal heat management and the like in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of organic materials, and in particular relates to a copper mesh-based photoelectric dual-trigger phase change material with high conductivity, stable shape, high thermal conductivity, leakage prevention, and Joule heating, and a preparation method thereof. Background Art

[0002] With the rapid development of technologies such as thermal management, portable smart wearables, and solar energy utilization, and the frequent occurrence of large temperature difference workplaces and extreme weather, active solar thermal management, passive Joule thermal management, and thermal energy storage and conversion have received extensive attention from researchers. Phase change materials (PCMs), as a type of energy storage material that can absorb and release heat through a phase change process, have long been used in the field of device thermal management. However, the inherent defects of PCMs, such as poor thermal conductivity and easy leakage, limit their further application. Many studies are dedicated to solving these two inherent problems.

[0003] In recent years, porous support scaffolds have been increasingly used to achieve PCM composites with high encapsulation efficiency and stable morphology. However, some porous scaffolds, such as polymer or silica scaffolds, are not suitable for energy conversion due to poor electrical conductivity and light absorption despite their good encapsulation efficiency. On the other hand, metal-based three-dimensional network structures are widely used in both aspects. However, the synergistic integration of efficient thermal conductivity and excellent heat storage remains a major challenge for PCM. In recent years, the thermal conductivity of composite PCMs has been improved by adding high thermal conductivity fillers, constructing thermal conductive channels, and reducing interfacial thermal resistance, but the heat storage capacity will inevitably be lost. Therefore, there is an urgent need to develop photothermal dual-triggered phase change materials with high electrical conductivity, stable shape, high thermal conductivity, leakage prevention, and Joule heating to meet complex and diverse application scenarios. Summary of the invention

[0004] The purpose of the present invention is to provide a photoelectric dual-trigger phase change material with easily available raw materials and high electrical conductivity, stable shape, high thermal conductivity, leakage prevention and Joule heating.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A photoelectric dual-trigger phase change material based on a copper mesh with high conductivity, shape stability, high thermal conductivity, leakage prevention, and Joule heating. The copper mesh is used as the conductive and thermal conductive network, and carbon nanotubes (CNTs), polyethylene glycol 10000 (PEG10000) and styrene-butylene-butadiene-styrene copolymer (SEBS) are introduced on the basis of the copper mesh.

[0007] Furthermore, the above-mentioned copper mesh-based photoelectric dual-trigger phase change material with high conductivity, shape stability, high thermal conductivity, leakage prevention, and Joule heating is based on a copper-based three-dimensional network and uses SEBS as a flexible support to achieve effective dual packaging of PEG10000.

[0008] Furthermore, the above-mentioned copper mesh-based photoelectric dual-triggered phase change material with high conductivity, shape stability, high thermal conductivity, leakage prevention, and Joule heating uses CNTs as light absorbers, and simultaneously utilizes the high conductivity and high thermal conductivity of copper mesh and CNTs to achieve the dual functions of Joule heating and photothermal conversion.

[0009] The method for preparing the photoelectric dual-trigger phase change material with high conductivity, shape stability, high thermal conductivity, leakage prevention and Joule heating based on the copper mesh described in any one of the above comprises the following steps:

[0010] 1) First, the copper mesh was washed with water for 2 h to remove impurities on the surface, and then the copper mesh was immersed in PEG10000 for 24 h by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface;

[0011] 2) dissolving SEBS in n-hexane at 50° C., adding CNTs and stirring evenly; then adding the adsorption-saturated copper mesh obtained in step 1), stirring slowly for 2 h, and finally drying in a forced air drying oven for 2 h to remove excess solvent.

[0012] Preferably, in the above preparation method, in step 2), CNTs are added at a mass percentage of 10%, 30% or 50%.

[0013] The beneficial effects of the present invention are:

[0014] 1. The present invention has readily available raw materials and is easy to operate, and improves the inherent defects of phase change materials such as low thermal conductivity, leakage, and rigidity.

[0015] 2. The packaging method of the phase change material of the present invention is based on a copper-based three-dimensional network and SEBS polymer as a flexible support to achieve effective double packaging of PEG10000.

[0016] 3. The photoelectric dual trigger function of the present invention uses carbon nanotubes as light absorbers and simultaneously utilizes the high electrical conductivity and high thermal conductivity of the copper mesh and carbon nanotubes themselves to achieve the dual functions of Joule heating and photothermal conversion.

[0017] 4. The phase change material of the present invention has comprehensive properties such as high conductivity, shape stability, high thermal conductivity, leakage prevention, Joule heating and photothermal conversion, and has certain application value in battery preheating and personal thermal management. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1This is the DSC curve of enthalpy change of Cu@PCM10000 prepared in Example 5.

[0019] Figure 2 This is a diagram showing the anti-leakage and shape stability effects of Cu@PCM10000@SEBS prepared in Example 7.

[0020] Figure 3 This is the electrothermal conversion diagram of Cu@PCM10000@SEBS@CNTs-30% prepared in Example 9. DETAILED DESCRIPTION

[0021] Example 1Cu@PCM2000

[0022] The preparation method is as follows:

[0023] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG2000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a forced air drying oven to remove excess PEG2000 on the surface, recorded as Cu@PCM2000.

[0024] Example 2Cu@PCM4000

[0025] The preparation method is as follows:

[0026] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG4000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a forced air drying oven to remove excess PEG4000 on the surface, recorded as Cu@PCM4000.

[0027] Example 3Cu@PCM6000

[0028] The preparation method is as follows:

[0029] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG6000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a forced air drying oven to remove excess PEG6000 on the surface, recorded as Cu@PCM6000.

[0030] Example 4Cu@PCM8000

[0031] The preparation method is as follows:

[0032] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG8000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a forced air drying oven to remove excess PEG8000 on the surface, recorded as Cu@PCM8000.

[0033] Example 5Cu@PCM10000

[0034] The preparation method is as follows:

[0035] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG10000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a forced air drying oven to remove excess PEG10000 on the surface, recorded as Cu@PCM10000.

[0036] Example 6Cu@PCM20000

[0037] The preparation method is as follows:

[0038] The commercially available copper mesh was first washed with water for 2 h to remove impurities on the surface, and then immersed in PEG20000 for 24 h by vacuum adsorption to achieve saturated adsorption, and placed in a blast drying oven to remove excess PEG20000 on the surface, recorded as Cu@PCM20000.

[0039] Example 7Cu@PCM10000@SEBS

[0040] The preparation method is as follows:

[0041] First, the commercial copper mesh was washed with water for 2 hours to remove impurities on the surface, and then it was immersed in PEG10000 for 24 hours by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface. SEBS was dissolved in 50°C n-hexane, then added to the adsorption-saturated copper mesh and slowly stirred for 2 hours, and finally dried in a forced air drying oven for 2 hours to remove excess solvent.

[0042] Example 8Cu@PCM10000@SEBS@CNTs-10%

[0043] The preparation method is as follows:

[0044] First, the commercial copper mesh was washed with water for 2 hours to remove impurities on the surface, and then it was immersed in PEG10000 for 24 hours by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface. SEBS was dissolved in 50°C n-hexane, CNTs were added at a mass percentage of 10%, and stirred evenly, and then the adsorption saturated copper mesh was added and slowly stirred for 2 hours, and finally dried in a forced air drying oven for 2 hours to remove excess solvent.

[0045] Example 9Cu@PCM10000@SEBS@CNTs-30%

[0046] The preparation method is as follows:

[0047] First, the commercial copper mesh was washed with water for 2 hours to remove impurities on the surface, and then it was immersed in PEG10000 for 24 hours by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface. SEBS was dissolved in 50°C n-hexane, CNTs were added at a mass percentage of 30%, and stirred evenly, and then the adsorption saturated copper mesh was added and slowly stirred for 2 hours, and finally dried in a forced air drying oven for 2 hours to remove excess solvent.

[0048] Example 10Cu@PCM10000@SEBS@CNTs-50%

[0049] The preparation method is as follows:

[0050] First, the commercial copper mesh was washed with water for 2 hours to remove impurities on the surface, and then it was immersed in PEG10000 for 24 hours by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface. SEBS was dissolved in 50°C n-hexane, and CNTs were added at a mass percentage of 50%, stirred evenly, and then the adsorption-saturated copper mesh was added and slowly stirred for 2 hours, and finally dried in a forced air drying oven for 2 hours to remove excess solvent.

[0051] Figure 1 The enthalpy change diagram of Cu@PCM10000 is shown. It is not difficult to find that its melting enthalpy and solidification enthalpy are as high as 102.6 J / g and 89.56 J / g respectively. The high enthalpy change value also brings excellent energy storage behavior to the phase change material.

[0052] Figure 2 The figure shows the excellent anti-leakage and shape stability of the Cu@PCM10000@SEBS dual-encapsulation phase change material. As can be seen from the figure, PEG10000 leaked after heating for 1 minute, and PEG10000 completely leaked after 5 minutes. However, Cu@PCM10000@SEBS had no leakage at all after heating for 30 minutes, and its shape did not change at all, showing extremely strong anti-leakage and shape stability.

[0053] Figure 3 The electrothermal conversion of Cu@PCM10000@SEBS@CNTs-30% is shown. As can be seen from the figure, the temperature of Cu@PCM10000@SEBS@CNTs-30% rises rapidly with the start of the load voltage, showing a sensitive Joule heating function. When the load voltage is turned off, the temperature drops rapidly. The results show that the prepared Cu@PCM10000@SEBS@CNTs-30% has excellent electrothermal function and has certain application prospects in the field of personal thermal management in the future.

[0054] In summary, the phase change material of the present invention has comprehensive properties such as high conductivity, shape stability, high thermal conductivity, leakage prevention, Joule heating and photothermal conversion, and is expected to have certain application value in battery preheating and personal thermal management in the future.

Claims

1. A photoelectric dual-trigger phase change material based on copper mesh with high conductivity, shape stability, high thermal conductivity, leakage prevention, and Joule heating, characterized in that: The photoelectric dual-trigger phase change material uses a copper mesh as a conductive and thermal conductive network, and introduces CNTs, PEG10000 and SEBS on the basis of the copper mesh.

2. According to claim 1, a copper mesh-based photoelectric dual-trigger phase change material with high electrical conductivity, shape stability, high thermal conductivity, leakage prevention, and Joule heating, characterized in that: The photoelectric dual-trigger phase change material is based on a copper-based three-dimensional network and uses SEBS as a flexible support to achieve effective dual packaging of PEG10000.

3. The photoelectric dual-trigger phase change material based on copper mesh with high conductivity, shape stability, high thermal conductivity, leakage prevention and Joule heating according to claim 1, characterized in that: The photoelectric dual-trigger phase change material uses CNTs as light absorbers and simultaneously utilizes the high electrical conductivity and high thermal conductivity of copper mesh and CNTs to achieve the dual functions of Joule heating and photothermal conversion.

4. The method for preparing the photoelectric dual-trigger phase change material with high conductivity, shape stability, high thermal conductivity, leakage prevention and Joule heating based on copper mesh according to any one of claims 1 to 3, characterized in that: The steps include: 1) First, the copper mesh was washed with water for 2 h to remove impurities on the surface, and then the copper mesh was immersed in PEG10000 for 24 h by vacuum adsorption to achieve saturated adsorption and remove excess PEG10000 on the surface; 2) dissolving SEBS in n-hexane at 50° C., adding CNTs and stirring evenly; then adding the adsorption-saturated copper mesh obtained in step 1), stirring slowly for 2 h, and finally drying in a forced air drying oven for 2 h to remove excess solvent.

5. The preparation method according to claim 4, characterized in that: In step 2), CNTs are added at a mass percentage of 10%, 30% or 50%.