Functional surfactant for oil and gas fields and preparation method thereof

By modifying the combination of nanoparticles, nitrogen-containing heterocyclic hydrocarbons and silicone surfactants, a functional surfactant with a three-dimensional network structure is formed, and the surfactant in the prior art is solved in the high temperature and high salt environment. The problem of insufficient tolerance significantly improves the recovery rate.

CN118995178AActive Publication Date: 2024-11-22SHAANXI BANGXI CHEM

Patent Information

Application Number
CN202411269514.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-22
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

Existing surfactants have poor resistance to high temperature and high salt environments, resulting in low recovery rates.

Method used

Using a combination of modified nanoparticles, nitrogen-containing heterocycloalkanes and silicone surfactants, a nucleophilic substitution reaction of sulfonic acid-based modified nanosilica and cage-type oligosilsesquioxane is formed to form a three-dimensional network. Functional surfactants with a structure enhance their rheology and temperature and salt resistance.

Benefits of technology

It significantly improves the stability of the surfactant and its resistance to high temperature and high salt, effectively reduces the interfacial tension of oil and water, and improves the recovery rate of oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995178A_ABST
    Figure CN118995178A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of surfactants for oil and gas fields, in particular to a functional surfactant for an oil and gas field and a preparation method of the functional surfactant. The modified nano particles are sulfonic modified nano silicon dioxide; the nitrogen-containing heterocyclic alkane is macrocycloalkane composed of C-N, C-O or C-C bonds; and the organic silicon surfactant is polyhedral oligomeric silsesquioxane. According to the functional surfactant for the oil and gas field and the preparation method of the functional surfactant, the prepared surfactant is good in stability, has better rheological property and temperature resistance and salt resistance, and can effectively reduce oil-water interfacial tension and improve the recovery rate of petroleum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surfactants for oil and gas fields, in particular to a functional surfactant for oil and gas fields and a preparation method thereof. Background Art

[0002] Petroleum, also known as crude oil, is an oily substance formed by organic matter under pressure and high temperature conditions deep in the earth's crust for millions of years. It is a mixture of various alkanes, cycloalkanes, and aromatic hydrocarbons. Like coal, it is a fossil fuel. Crude oil extraction can be divided into three stages: ① The primary oil recovery stage in which oil is extracted by self-flowing under the pressure of the internal formation. This stage is also the easiest stage to extract; ② The secondary oil recovery stage in which water or gas injection is used to increase the formation pressure. This stage usually achieves a recovery rate of about 30%; ③ In order to effectively utilize the remaining reserves in the formation, scholars have proposed a tertiary oil recovery stage based on more advanced technical means such as chemical drive, microbial drive, and mixed drive. Among them, surfactant flooding technology in chemical drive is the fastest-growing and most promising research direction.

[0003] Surfactants play an important role in chemical flooding. By injecting surfactants into the reservoir, the interaction between crude oil and rock surface is changed, the interfacial tension between oil and water is reduced, the displacement of crude oil is promoted, and the recovery rate is improved. Surfactants are mainly divided into anionic, cationic, zwitterionic and non-ionic surfactants and other types of surfactants. Among anionic surfactants, sulfonate surfactants are low in price and have good water solubility. They show good interfacial activity when used in combination and can obtain lower interfacial tension under low concentration conditions, so they are widely used.

[0004] However, the surfactants in the prior art have poor resistance to high and low temperatures and salt, which leads to low recovery rates. Summary of the invention

[0005] The purpose of the present invention is to provide a functional surfactant for oil and gas fields and a preparation method thereof. The prepared surfactant has good stability, good rheological properties and temperature and salt resistance, can effectively reduce oil-water interfacial tension, and improve the recovery rate of oil.

[0006] To achieve the above-mentioned purpose, the present invention provides a functional surfactant for oil and gas fields, comprising modified nanoparticles, nitrogen-containing heterocycloalkane and organosilicon surfactant; the modified nanoparticles are sulfonic acid group-modified nanosilica; the nitrogen-containing heterocycloalkane is a macrocycloalkane composed of CN, CO or CC bonds; the organosilicon surfactant is a cage-type oligomeric silsesquioxane, wherein the molar ratio of the nitrogen-containing heterocycloalkane to the organosilicon surfactant is 1:1 to 1:20, and the mass percentage of the modified nanoparticles is 1 to 2wt% based on the total mass of the nitrogen-containing heterocycloalkane and the organosilicon surfactant.

[0007] Preferably, the nitrogen-containing heterocycloalkane is selected from one or more of 1,4,7-triazacyclononane, 1,4,7,10-tetraazacyclododecane, and 1,4,7,10,13-pentaazacyclopentadecane.

[0008] Preferably, the cage oligomeric silsesquioxane is monochloropropylheptaisobutyl oligomeric cage oligomeric silsesquioxane.

[0009] The method for preparing the functional surfactant for oil and gas fields comprises the following steps:

[0010] S1, preparing sulfonic acid group-modified nano-silica;

[0011] S2, dissolving the nitrogen-containing heterocycloalkane in solvent 1, then adding a base, and stirring under nitrogen to obtain a nitrogen-containing heterocycloalkane solution;

[0012] S3, dissolving the cage-type oligomeric silsesquioxane in solvent 1, then transferring it to a constant pressure dropping funnel, and dropping it into the nitrogen-containing heterocycloalkane solution in S2, heating the reaction, filtering and retaining the filtrate, washing the filtrate and then rotating and concentrating it to obtain a concentrated solution;

[0013] S4, adding the sulfonic acid group-modified nano-silica of S1 into the concentrated solution of S3, reacting under ultrasonic stirring conditions, and obtaining a functional surfactant for oil and gas fields.

[0014] Preferably, S1 comprises the following steps,

[0015] S1.1. Preparation of amino-modified nano-silica

[0016] Dissolving nano-silica and aminosilane coupling agent in solvent 2, performing ultrasonic dispersion, stirring and reflux reaction at constant temperature, cooling to room temperature, and centrifuging to obtain amino-modified nano-silica;

[0017] S1.2, modifying the amino-modified nano-silica with sulfonic acid groups

[0018] Sodium 3-chloro-2-hydroxypropanesulfonate is dissolved in deionized water. After it is completely dissolved, the amino-modified nano-silica prepared in S1.1 is added. After ultrasonic dispersion, the mixture is heated in an oil bath for reaction to obtain a dispersion of sulfonic acid group-modified nano-silica. The dispersion of sulfonic acid group-modified nano-silica is separated and purified, and then vacuum dried to obtain a powder of sulfonic acid group-modified nano-silica.

[0019] Preferably, in S1.1, the mass ratio of the aminosilane coupling agent to the nano-silica is 1:0.5-1.

[0020] Preferably, in S1.1, the second solvent comprises one or both of ethanol and toluene; the reaction temperature of the constant temperature stirring reflux reaction is 60 to 120° C., and the constant temperature reaction time is 18 to 24 hours.

[0021] Preferably, in S1.2, the ultrasonic dispersion time is 5 min, the oil bath heating reaction is carried out at 70° C. for 24 h, and the separation and purification is firstly performed by rotary concentration and then purified by dialysis bag.

[0022] Preferably, the solvent in S2 and S3 is chloroform, and the base in S2 is sodium hydroxide.

[0023] Preferably, in S2, the stirring is carried out at room temperature for 30 min.

[0024] Preferably, in S3, the dripping is completed slowly within 30 minutes; the heating reaction is carried out by stirring at room temperature for 15 minutes, then heating to 65° C. and reacting for 16 to 32 hours; and the washing is carried out by washing three times with distilled water to remove unreacted nitrogen-containing heterocycloalkane.

[0025] Preferably, in S3, the molar ratio of the nitrogen-containing heterocycloalkane to the cage-type oligomeric silsesquioxane is 1 to 20:1.

[0026] Preferably, in S4, based on the concentrated solution, the mass percentage of the sulfonic acid group-modified nano-silica is 0.05-2.0 wt %.

[0027] Mechanism of the Invention

[0028] The nitrogen atom of the nitrogen-containing heterocycloalkane contains a lone pair of electrons, which is easy to introduce other functional groups for modification; the cage-type oligomeric silsesquioxane has high biocompatibility and surface activity due to the stable bond energy of the silicon-oxygen bond, easy rotation, large bond angle and long bond length, and can also withstand high and low temperatures; the sulfonic acid group-modified nano-silica obtained by functional modification has good anti-aggregation and anti-interference capabilities under high temperature and high salt environments; the present invention uses nitrogen-containing heterocycloalkane as a hydrophilic group and cage-type oligomeric silsesquioxane as a hydrophobic group to prepare a functional surfactant for oil and gas fields through a nucleophilic substitution reaction, and at the same time introduces sulfonic acid group-modified nano-silica to be grafted with nitrogen-containing heterocycloalkane and cage-type oligomeric silsesquioxane to form a three-dimensional network structure, which increases the rheological properties of the surfactant while also increasing its high and low temperature resistance and salt resistance, and shows the ability to effectively reduce the oil-water interfacial tension.

[0029] Beneficial effects of the present invention:

[0030] The functional surfactant for oil and gas fields provided by the present invention has good stability, good rheological properties and temperature and salt resistance, good wettability to rocks, can effectively reduce oil-water interfacial tension, and improve the recovery rate of oil.

[0031] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the infrared spectrum of the functional surfactant for oil and gas fields in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0034] Example 1

[0035] The present invention provides a functional surfactant for oil and gas fields, which is prepared by the following steps:

[0036] S1. Preparation of sulfonic acid modified nano-silica

[0037] S1.1. Preparation of amino-modified nano-silica

[0038] 5g of nano-silica and 10g of KH-550 were dissolved in ethanol, and the temperature was raised to 60°C after ultrasonic dispersion. The mixture was stirred and refluxed at a constant temperature for 18h, and then cooled to room temperature and centrifuged to obtain amino-modified nano-silica.

[0039] S1.2, modifying the amino-modified nano-silica with sulfonic acid groups

[0040] Dissolve 7.9 g of sodium 3-chloro-2-hydroxypropanesulfonate in 100 mL of deionized water. After it is completely dissolved, add 2 g of

[0041] The amino-modified nano-silica prepared in S1.1 was ultrasonically dispersed for 5 minutes, heated to 70°C in an oil bath and reacted for 24 hours to obtain a dispersion of sulfonic acid-modified nano-silica. The dispersion of sulfonic acid-modified nano-silica was first rotary concentrated and then purified using a dialysis bag. The solvent was then completely evaporated and vacuum dried to obtain a powder of sulfonic acid-modified nano-silica.

[0042] S2, dissolving 1.723 g of 1,4,7,10-tetraazacyclododecane in 50 mL of chloroform, then adding 0.8 g of sodium hydroxide, and stirring under nitrogen for 30 min to obtain a nitrogen-containing heterocycloalkane solution;

[0043] S3, dissolving 0.525g of monochloropropyl heptaisobutyl oligomeric cage-type silsesquioxane in 5mL of chloroform, then transferring to a constant pressure dropping funnel, and dropping into the nitrogen-containing heterocycloalkane solution of S2, slowly dropping within 30min, stirring at room temperature for 15min, heating to 65°C, reacting for 16h, filtering and retaining the filtrate after the reaction is completed, washing the filtrate three times with distilled water to remove unreacted nitrogen-containing heterocycloalkane, and rotating and concentrating to obtain a concentrate;

[0044] S4. Based on the total mass of the nitrogen-containing heterocycloalkane and the organosilicon surfactant, the sulfonic acid group-modified nano-silica of S1 is added to the concentrated solution of S3 at a mass percentage of 1.0wt%, and reacted under ultrasonic stirring to obtain a functional surfactant for oil and gas fields.

[0045] Example 2

[0046] The present invention provides a functional surfactant for oil and gas fields, which is prepared by the following steps:

[0047] S1. Preparation of sulfonic acid modified nano-silica

[0048] S1.1. Preparation of amino-modified nano-silica

[0049] 8g of nano-silica and 15g of KH-550 were dissolved in toluene, and the mixture was ultrasonically dispersed and heated to 100°C. The mixture was stirred and refluxed at a constant temperature for 20h, and then cooled to room temperature and centrifuged to obtain amino-modified nano-silica.

[0050] S1.2, modifying the amino-modified nano-silica with sulfonic acid groups

[0051] Dissolve 7.9 g of sodium 3-chloro-2-hydroxypropanesulfonate in 100 mL of deionized water. After it is completely dissolved, add 2 g of

[0052] The amino-modified nano-silica prepared in S1.1 was ultrasonically dispersed for 5 minutes, heated to 70°C in an oil bath and reacted for 24 hours to obtain a dispersion of sulfonic acid-modified nano-silica. The dispersion of sulfonic acid-modified nano-silica was first rotary concentrated and then purified using a dialysis bag. The solvent was then completely evaporated and vacuum dried to obtain a powder of sulfonic acid-modified nano-silica.

[0053] S2, dissolving 1.292 g of 1,4,7-triazacyclononane in 50 mL of chloroform, then adding 0.8 g of sodium hydroxide, and stirring for 30 min under nitrogen to obtain a nitrogen-containing heterocycloalkane solution;

[0054] S3, dissolving 0.525g of monochloropropyl heptaisobutyl oligomeric cage-type silsesquioxane in 5mL of chloroform, then transferring to a constant pressure dropping funnel, and dropping into the nitrogen-containing heterocycloalkane solution of S2, slowly dropping within 30min, stirring at room temperature for 15min, heating to 65°C, reacting for 24h, filtering and retaining the filtrate after the reaction is completed, washing the filtrate three times with distilled water to remove unreacted nitrogen-containing heterocycloalkane, and rotating and concentrating to obtain a concentrate;

[0055] S4. Based on the total mass of the nitrogen-containing heterocycloalkane and the organosilicon surfactant, the sulfonic acid group-modified nano-silica of S1 is added to the concentrated solution of S3 at a mass percentage of 1.5wt%, and reacted under ultrasonic stirring to obtain a functional surfactant for oil and gas fields.

[0056] Example 3

[0057] The present invention provides a functional surfactant for oil and gas fields, which is prepared by the following steps:

[0058] S1. Preparation of sulfonic acid modified nano-silica

[0059] S1.1. Preparation of amino-modified nano-silica

[0060] Dissolve 10g of nano-silica and 20g of KH-550 in a mixed solution of ethanol and toluene, disperse by ultrasonication, heat to 120°C, stir and reflux at constant temperature for 24h, then cool to room temperature, centrifuge and separate to obtain amino-modified nano-silica;

[0061] S1.2, modifying the amino-modified nano-silica with sulfonic acid groups

[0062] Dissolve 7.9 g of sodium 3-chloro-2-hydroxypropanesulfonate in 100 mL of deionized water. After it is completely dissolved, add 2 g of

[0063] The amino-modified nano-silica prepared in S1.1 was ultrasonically dispersed for 5 minutes, heated to 70°C in an oil bath and reacted for 24 hours to obtain a dispersion of sulfonic acid-modified nano-silica. The dispersion of sulfonic acid-modified nano-silica was first rotary concentrated and then purified using a dialysis bag. The solvent was then completely evaporated and vacuum dried to obtain a powder of sulfonic acid-modified nano-silica.

[0064] S2, dissolving 2.153 g of 1,4,7,10,13-pentaazacyclopentadecane in 50 mL of chloroform, then adding 0.8 g of sodium hydroxide, and stirring for 30 min under nitrogen to obtain a nitrogen-containing heterocycloalkane solution;

[0065] S3, dissolving 0.525g of monochloropropyl heptaisobutyl oligomeric cage-type silsesquioxane in 5mL of chloroform, then transferring to a constant pressure dropping funnel, and dropping into the nitrogen-containing heterocycloalkane solution of S2, slowly dropping within 30min, stirring at room temperature for 15min, heating to 65°C, reacting for 32h, filtering and retaining the filtrate after the reaction is completed, washing the filtrate three times with distilled water to remove unreacted nitrogen-containing heterocycloalkane, and rotating and concentrating to obtain a concentrate;

[0066] S4. Based on the total mass of the nitrogen-containing heterocycloalkane and the organosilicon surfactant, the sulfonic acid group-modified nano-silica of S1 is added to the concentrated solution of S3 at a mass percentage of 2.0wt%, and reacted under ultrasonic stirring to obtain a functional surfactant for oil and gas fields.

[0067] Comparative Example 1

[0068] It is dodecyl betaine purchased from Shandong Jiapeng New Materials Co., Ltd.

[0069] Performance Testing

[0070] Figure 1 This is the infrared spectrum of the functional surfactant for oil and gas fields in Example 1 of the present invention. As shown in the figure, the infrared spectrum is at 3330cm -1 The absorption peak of NH appeared at 2972 ​​cm -1The absorption peak of -CH3 appeared at 1120cm -1 The absorption peak of Si-O-Si appears at 1190 cm -1 、1093cm -1 、617cm -1 、535cm -1 The absorption peak of sulfonic acid group appeared at , indicating that the target product was synthesized in Example 1 of the present invention.

[0071] Salt resistance test

[0072] In the oil industry, due to cost constraints, local groundwater is often used to prepare crude oil displacement fluids, but NaCl in groundwater is often not effectively separated. Therefore, in order to function normally in highly salinized crude oil displacement fluids, the tolerance of surfactants to NaCl is particularly important. In order to explore the effect of sodium chloride concentration on the ability of surfactants to reduce oil-water interfacial tension, a salt tolerance test was conducted.

[0073] The surfactants prepared in Examples 1-3 and Comparative Example 1 were added to NaCl solutions of different concentrations (10 g / L, 20 g / L, 30 g / L, 50 g / L) at 25°C to test the surface tension of the system. The test results are shown in Table 1.

[0074] Table 1 Interfacial tension of different concentrations of NaCl solution after adding different surfactants (unit: mN / m)

[0075]

[0076] It can be seen from Table 1 that in the NaCl solution with the same concentration, the surface tension of the surfactant system added to Examples 1-3 is less than the surface tension of the surfactant system added to Comparative Example 1, indicating that the ability of the surfactants prepared in Examples 1-3 of the present invention to reduce interfacial tension is better than that of Comparative Example 1.

[0077] As the concentration of NaCl solution increases, the surface tension of the surfactant systems added to Examples 1-3 does not change much and shows a downward trend, indicating that the surfactants prepared in Examples 1-3 of the present invention have good salt resistance. However, the surface tension of the surfactant system added to Comparative Example 1 increases as the concentration of NaCl solution increases, indicating that its salt resistance is poor.

[0078] Temperature resistance test

[0079] The surfactants of Examples 1-3 and Comparative Example 1 were prepared into solutions with a concentration of 5 g / L, and their surface tensions were tested at temperatures of 60° C., 70° C., 80° C., and 90° C., respectively. The test results are shown in Table 2.

[0080] Table 2 Interfacial tension of different surfactants at different temperatures (unit: mN / m)

[0081]

[0082]

[0083] As can be seen from Table 2, as the temperature increases, the surface tension of the surfactant systems added to Examples 1-3 does not change much and shows a downward trend, indicating that the surfactants prepared in Examples 1-3 of the present invention have good high temperature resistance. However, the surface tension of the surfactant system added to Comparative Example 1 increases as the temperature increases, indicating that its high temperature resistance is poor.

[0084] Test for reducing interfacial tension

[0085] The surfactants of Examples 1-3 and Comparative Example 1 were prepared into solutions with a concentration of 5 g / L, and then mixed with crude oil (the crude oil was provided by the Second Oil Production Plant of Qinghai Oilfield). After standing for 30 minutes, the oil-water interfacial tension after mixing was tested. The results are shown in Table 3.

[0086] Table 3 Oil-water interfacial tension after mixing different surfactants with crude oil (unit: mN / m)

[0087]

[0088] It can be seen from Table 3 that the interfacial tension of the oil-water mixture mixed with the surfactants prepared in Examples 1-3 of the present invention is much smaller than the interfacial tension of the oil-water mixture mixed with Comparative Example 1, indicating that the surfactants prepared in Examples 1-3 of the present invention have a strong ability to reduce interfacial tension.

[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A functional surfactant for oil and gas fields, characterized in that: The invention comprises modified nanoparticles, nitrogen-containing heterocycloalkane and organosilicon surfactant; the modified nanoparticles are sulfonic acid group-modified nano-silica; the nitrogen-containing heterocycloalkane is a macrocyclic alkane composed of CN, CO or CC bonds; the organosilicon surfactant is a cage-type oligomeric silsesquioxane, wherein the molar ratio of the nitrogen-containing heterocycloalkane to the organosilicon surfactant is 1:1 to 1:20, and the mass percentage of the modified nanoparticles is 1 to 2 wt % based on the total mass of the nitrogen-containing heterocycloalkane and the organosilicon surfactant.

2. A functional surfactant for oil and gas fields according to claim 1, characterized in that: The nitrogen-containing heterocycloalkane is selected from one or more of 1,4,7-triazacyclononane, 1,4,7,10-tetraazacyclododecane and 1,4,7,10,13-pentaazacyclopentadecane.

3. A functional surfactant for oil and gas fields according to claim 1, characterized in that: The cage type oligomeric silsesquioxane is monochloropropyl heptaisobutyl oligomeric cage type silsesquioxane.

4. A method for preparing a functional surfactant for oil and gas fields according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1, preparing sulfonic acid group-modified nano-silica; S2, dissolving the nitrogen-containing heterocycloalkane in solvent 1, then adding a base, and stirring under nitrogen to obtain a nitrogen-containing heterocycloalkane solution; S3, dissolving the cage-type oligomeric silsesquioxane in solvent 1, then transferring it to a constant pressure dropping funnel, and dropping it into the nitrogen-containing heterocycloalkane solution in S2, heating the reaction, filtering and retaining the filtrate, washing the filtrate and then rotating and concentrating it to obtain a concentrated solution; S4, adding the sulfonic acid group-modified nano-silica of S1 into the concentrated solution of S3, reacting under ultrasonic stirring conditions, and obtaining a functional surfactant for oil and gas fields.

5. The method for preparing a functional surfactant for oil and gas fields according to claim 4, characterized in that: S1 includes the following steps, S1.

1. Preparation of amino-modified nano-silica Dissolving nano-silica and aminosilane coupling agent in solvent 2, performing ultrasonic dispersion, stirring and reflux reaction at constant temperature, cooling to room temperature, and centrifuging to obtain amino-modified nano-silica; S1.2, modifying the amino-modified nano-silica with sulfonic acid groups Sodium 3-chloro-2-hydroxypropanesulfonate is dissolved in deionized water. After it is completely dissolved, the amino-modified nano-silica prepared in S1.1 is added. After ultrasonic dispersion, the mixture is heated in an oil bath for reaction to obtain a dispersion of sulfonic acid group-modified nano-silica. The dispersion of sulfonic acid group-modified nano-silica is separated and purified, and then vacuum dried to obtain a powder of sulfonic acid group-modified nano-silica.

6. The method for preparing a functional surfactant for oil and gas fields according to claim 5, characterized in that: In S1.1, the second solvent includes one or both of ethanol and toluene; the reaction temperature of the constant temperature stirring reflux reaction is 60 to 120° C., and the constant temperature reaction time is 18 to 24 hours.

7. The method for preparing a functional surfactant for oil and gas fields according to claim 5, characterized in that: In S1.2, the ultrasonic dispersion time is 5 minutes, the oil bath heating reaction is carried out at 70°C for 24 hours, and the separation and purification is first performed by rotary concentration and then purification using a dialysis bag.

8. The method for preparing a functional surfactant for oil and gas fields according to claim 4, characterized in that: The solvent in both S2 and S3 is chloroform, and the base in S2 is sodium hydroxide.

9. The method for preparing a functional surfactant for oil and gas fields according to claim 4, characterized in that: In S2, stirring is performed at room temperature for 30 min.

10. The method for preparing a functional surfactant for oil and gas fields according to claim 4, characterized in that: In S3, the dripping is completed slowly within 30 minutes; the heating reaction is stirred at room temperature for 15 minutes, then the temperature is raised to 65° C. and the reaction is carried out for 16 to 32 hours; and the washing is washed three times with distilled water to remove unreacted nitrogen-containing heterocycloalkane.

Citation Information

Patent Citations

  • Active nano tackifier and preparation method thereof

    CN118562477A

  • Chemical oil displacement agent

    CN1696240A

  • Sulfonate-functional coatings and methods

    US20120273000A1

  • Nanoparticle modified fluids and methods of manufacture thereof

    US20180030332A1

  • Compositions and methods for improving thermal and brine stability of nanoparticles

    US20230332041A1

Cited By

  • Multifunctional blocking remover for oil extraction and acidification in oil field and preparation method of multifunctional blocking remover

    CN122104190A