Micro-fracture network interface modified far-end strong sand-carrying fracturing fluid and preparation method thereof

By modifying the distal strong sand-carrying fracturing liquid using micro-slit mesh interface in shale fracturing, modifying the rock surface with titanate coupling agent and bimini cationic surfactant, combining the reaction of zirconium oxychloride and sodium lactate, the solution is solved The problems of fine crack blockage and sand carrying capacity caused by traditional fracturing fluid are achieved, and efficient oil and gas production increase and stable production are achieved.

CN118995182AActive Publication Date: 2024-11-22成都昱葵科技有限公司

Patent Information

Application Number
CN202411093301.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22
Estimated Expiration
2044-08-09

AI Technical Summary

Technical Problem

During shale fracturing, traditional oil-based fracturing fluid leads to blockage of fine fractures and reduces sand carrying capacity, resulting in a decrease in oil and gas production rate. The weak hydrophilicity of reservoir rocks makes water easy to adsorb and block fractures, increasing flow resistance .

Method used

The distal strong sand-carrying fracturing liquid is modified by the interface of the micro-slit mesh, and the rock surface is modified by titanate coupling agent and bimini cationic surfactant to form a hydrophobic film, enhance sand-carrying performance, and pass through the oxychlorine in the intermediate S Zirconium lactate reacts with sodium lactate to synthesize zirconium lactate, delaying the release rate of metal ions, improving the complexity of cross-linking reactions, and enhancing sand carrying capacity.

Benefits of technology

The fracturing fluid with high resistance reduction, low damage, and strong sand carrying capacity has been achieved, which has improved the production of oil and gas wells, reduced the blockage of micro channels, and improved the oil and gas recovery rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987171500000091
    Figure BDA0004987171500000091
  • Figure BDA0004987171500000101
    Figure BDA0004987171500000101
Patent Text Reader

Abstract

The invention discloses a micro-fracture network interface modified far-end strong sand-carrying fracturing fluid and a preparation method thereof, and relates to the technical field of oil and gas field exploitation. The fracturing fluid is prepared from the following components in parts by weight: 20 to 50 parts of low molecular weight polyacrylamide, 10 to 30 parts of polyhydroxyethyl acrylamide, 30 to 75 parts of diethylene glycol monoethyl ether acetate, 2 to 10 parts of fumed silica, 3 to 12 parts of a titanate coupling agent, 2 to 7 parts of a gemini cationic surfactant, 2 to 7 parts of alkyl polyoxyethylene ether and 2 to 7 parts of an intermediate S, the intermediate S comprises the following components in parts by weight: 10-25 parts of zirconium oxychloride and 5-25 parts of sodium lactate; and 65-85 parts of diethylene glycol monoethyl ether acetate. The preparation method comprises the following steps: S1, preparing an intermediate S; and S2, preparing a finished product R. The fracturing fluid has the characteristics of high resistance reduction, low damage and strong sand carrying capacity, and can realize gas guiding and oil increasing and improve the yield of an oil and gas well by modifying the surface characteristics of reservoir rocks.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil and gas field exploitation, and in particular to a micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method thereof. Background Art

[0002] As the oil and gas industry conducts in-depth research on unconventional shale fracturing methods, creating a larger and more complex fracture network has become an important reservoir transformation goal and a key means to increase oil and gas production.

[0003] In many shale fracturing processes, a large number of secondary fracture networks based on induced fractures and natural fractures have appeared. These secondary fracture networks will absorb up to 90% of the total liquid volume during hydraulic fracturing. The white oil and surfactants in the traditional oil-based fracturing fluid system can easily lead to blockage and damage of micro-fractures. At the same time, due to the flow attenuation of the fracturing fluid at the far end of the micro-fractures and in the branch fractures, the sand carrying capacity decreases, and the proppant gradually settles, making it difficult to effectively lay in the deep fractures. Under the action of ground stress, due to the lack of effective support, the branch fractures gradually close, and the micro-fractures are blocked by organic harmful components in the broken gel residue of the fracturing fluid, which has an extremely adverse effect on increasing and stabilizing production. In response to such problems, current research and reports mainly focus on reducing damage by breaking the fracturing fluid and increasing the sand-carrying capacity of polymer fracturing fluid (such as patents CN105219372B and CN103756664A), and often ignore the modification of the surface characteristics of reservoir rocks; since untreated rocks are weakly hydrophilic, water in the reservoir is easily adsorbed on the cracks and rock surfaces, blocking the discharge channels of crude oil and natural gas; at the same time, affected by the Jamin effect and capillary action, the flow resistance of hydrophobic crude oil and natural gas in the pores increases, and the actual recovery rate is further reduced. Therefore, the technical development trend to solve the above problems is to adopt comprehensive means and methods to introduce the modification and optimization of rock wettability, while improving the remote sand-carrying performance of the fracturing fluid and reducing the damage performance of the fracturing fluid breaking. Summary of the invention

[0004] The present invention provides a micro-fracture network interface modified remote strong sand-carrying fracturing fluid and a preparation method thereof, which not only has the characteristics of high resistance reduction, low damage and strong sand-carrying, but also can realize gas conduction and oil increase and improve the production of oil and gas wells by modifying the surface characteristics of reservoir rocks.

[0005] The present invention is achieved through the following technical scheme: a micro-fracture network interface modified distal strong sand-carrying fracturing fluid, which comprises, by weight, 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S; the intermediate S comprises, by weight, 10-25 parts of zirconium oxychloride, 5-25 parts of sodium lactate, and 65-85 parts of diethylene glycol ethyl ether acetate.

[0006] Furthermore, the effective content of sodium lactate is greater than 99%.

[0007] Furthermore, the molecular weight of the low molecular weight polyacrylamide is 3 million to 8 million, and the molecular weight of the polyhydroxyethyl acrylamide is 5 million to 30 million.

[0008] Furthermore, the titanate coupling agent is one or more of isopropyl tri(dioctyl pyrophosphate) titanate, isopropyl triisostearate titanate, and bistriethanolamine diisopropyl titanate, and the gemini cationic surfactant is one or more of didodecyl dimethyl ammonium chloride, didhexadecyl dimethyl ammonium chloride, and didetracetyl dimethyl ammonium chloride.

[0009] Furthermore, the alkyl polyoxyethylene ether is one or more of octadecylamino polyoxyethylene ether, dodecylamino polyoxyethylene ether, and hexadecylamino polyoxyethylene ether.

[0010] A method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid comprises the following steps:

[0011] S1 Preparation of intermediate S: The preparation of intermediate S comprises the following steps:

[0012] A1: By weight, 5-25 parts of sodium lactate and 10-25 parts of zirconium oxychloride are mixed and added to 65-85 parts of diethylene glycol ethyl ether acetate, heated to 50±5°C under stirring, and reacted for 2-3h to obtain intermediate A;

[0013] A2: Add pH regulator to intermediate A several times, sample 0.1% aqueous solution of intermediate A every 30 minutes to measure pH value, until pH value is 4-5, keep material temperature at 50±5℃, react for 4-5h, cool to room temperature to obtain intermediate S, the weight ratio of pH regulator added each time to intermediate A is 1:1000;

[0014] S2 Preparation of finished product R: The preparation of the finished product R comprises the following steps:

[0015] B1: Add low molecular weight polyacrylamide, polyhydroxyethyl acrylamide and fumed silica to diethylene glycol ethyl ether acetate in a certain proportion, mix them evenly under high-speed stirring, and let them stand for 1h-1.5h to obtain intermediate B;

[0016] B2: Add titanate coupling agent and gemini cationic surfactant to intermediate B and stir evenly at high speed, let stand for 1-1.5 hours to obtain intermediate C;

[0017] B3: Add alkyl polyoxyethylene ether to intermediate C and stir evenly at high speed, and let stand for 1-2 hours to obtain intermediate D;

[0018] B4: Add intermediate S to intermediate D, mix well under high-speed stirring to obtain finished product R;

[0019] The addition amount of the above reaction materials is calculated by weight: 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S;

[0020] Preparation of S3 strong sand-carrying fracturing fluid: The finished product R is configured into a solution with a content of 0.1wt% to obtain a micro-fracture network interface modified low-damage distal enhanced sand-carrying fracturing fluid.

[0021] Furthermore, in step A2, the pH regulator is an ethanol solution of diethanolamine with a mass fraction of 10.0 wt%.

[0022] Furthermore, in the step A1, the stirring speed is 300-1000 r / min.

[0023] Furthermore, in the preparation step of the S2 finished product R, the high-speed stirring speed is 1500-2500r / min.

[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0025] 1. A micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method of the present invention, wherein a titanate coupling agent is added, and its hydrolysis is utilized to perform adsorption with the hydroxyl groups on the rock surface, so as to form a hydrophobic film on the proppant and the fracture surface, and at the same time, the fracture network modification component is attached to the proppant and the fracture surface through intermolecular forces;

[0026] 2. The present invention discloses a micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method thereof. Gemini cationic surfactant is used as a modified component to perform hydrophobic transformation on reservoir rocks. Water in the reservoir is not easily adsorbed on the rock and fracture base surface, and a channel conducive to oil and gas production can be created. At the same time, part of the natural gas is in the form of adsorbed gas when it is produced. The hydrophobic treatment of the pores is accompanied by the discharge of formation water in the reservoir. Under the influence of the pressure difference, the adsorbed gas deep in the fracture will also be discharged, further improving the natural gas recovery rate. The titanate coupling agent is used to perform surface treatment on the proppant, adjusting the proppant from a weakly hydrophilic structure to a hydrophobic structure, changing the wettability of the proppant surface, improving the suspension ability of the proppant in the fracturing fluid, slowing down the sedimentation, achieving a long sand transport distance, reducing the near-well settlement, achieving the support effect on the distal fractures, and further improving the production.

[0027] 3. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid and preparation method of the present invention adopt alkyl polyoxyethylene ether as the modification component, which can promote the dispersion of heavy components such as asphaltenes and colloids in crude oil to form an oil-water dispersion, improve the liquid replacement efficiency, and further improve the recovery rate of crude oil.

[0028] 4. The present invention discloses a micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method thereof. Zirconium lactate is synthesized by the reaction of zirconium oxychloride and sodium lactate in an intermediate S. The zirconium ions in zirconium lactate are chelated and bound by lactate, and the release rate of the zirconium ions becomes slow and controllable. After the swelling and stretching of the polymer in the fracturing fluid are completed, the carboxyl hydroxyl reaction sites in the polymer structure are combined with the zirconium ions to form a cross-linked network structure through coordination bonds, thereby enhancing the sand-carrying performance of the system, thereby avoiding the problems of too fast zirconium ion release, poor polymer swelling, poor cross-linking effect, and poor sand-carrying performance; it also solves the problem of too slow zirconium ion release and the inability of the polymer to cross-link.

[0029] 5. The invention discloses a micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method thereof, which adopts a ligand and delays the release rate of metal ions during use, so that the local polymer undergoes a cross-linking reaction 5-15 minutes after the fracturing fluid enters the ground, and the structural complexity is improved, so as to achieve the purpose of enhancing the sand-carrying capacity of the fracturing fluid at the distal end and branch fractures at low flow rates;

[0030] 6. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid and preparation method of the present invention adopt low molecular weight polyacrylamide, which can achieve good debonding effect under the action of conventional debonding agents, has good compatibility with commercially available debonding agents, and has low viscosity and low residue after debonding;

[0031] 7. The present invention discloses a micro-fracture network interface modified distal strong sand-carrying fracturing fluid and a preparation method. On the one hand, the fracturing fluid can timely enhance the sand-carrying capacity of the distal end and branch fractures at low flow rates. On the other hand, an oil-conducting and gas-conducting fracturing fluid system is used to infiltrate from the cracks to modify the interface of the micro-channels, thereby reducing the strong adsorption of oil, gas and water by the micro-channels, and ensuring the smoothness of the micro-guiding channels, thereby achieving the purpose of improving the oil and gas recovery rate. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with the embodiments and test examples. The following embodiments and test examples are only several specific implementations of the present invention, but the design concept of the present invention is not limited thereto, and any non-substantial changes made to the present invention using this concept shall be deemed as acts that infringe the protection scope of the present invention.

[0033] Example

[0034] In one embodiment, a micro-fracture network interface modified distal strong sand-carrying fracturing fluid comprises, by weight, 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S; the intermediate S comprises, by weight, 10-25 parts of zirconium oxychloride, 5-25 parts of sodium lactate, and 65-85 parts of diethylene glycol ethyl ether acetate.

[0035] In one embodiment, the effective content of sodium lactate is greater than 99%.

[0036] In one embodiment, the molecular weight of the low molecular weight polyacrylamide is 3 million to 8 million, and the molecular weight of the polyhydroxyethyl acrylamide is 5 million to 30 million.

[0037] In one embodiment, the titanate coupling agent is one or more of isopropyl tri(dioctyl pyrophosphate) titanate, isopropyl triisostearate titanate, and bistriethanolamine diisopropyl titanate, and the gemini cationic surfactant is one or more of didodecyl dimethyl ammonium chloride, didhexadecyl dimethyl ammonium chloride, and didetracetyl dimethyl ammonium chloride.

[0038] In one embodiment, the alkyl polyoxyethylene ether is one or more of octadecylamino polyoxyethylene ether, dodecylamino polyoxyethylene ether, and hexadecylamino polyoxyethylene ether.

[0039] In one embodiment, a method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid comprises the following steps:

[0040] S1 Preparation of intermediate S: The preparation of intermediate S comprises the following steps:

[0041] A1: By weight, 5-25 parts of sodium lactate and 10-25 parts of zirconium oxychloride are mixed and added to 65-85 parts of diethylene glycol ethyl ether acetate, heated to 50±5°C under stirring, and reacted for 2-3h to obtain intermediate A;

[0042] A2: Add pH regulator to intermediate A several times, sample 0.1% aqueous solution of intermediate A every 30 minutes to measure pH value, until pH value is 4-5, keep material temperature at 50±5℃, react for 4-5h, cool to room temperature to obtain intermediate S, the weight ratio of pH regulator added each time to intermediate A is 1:1000;

[0043] S2 Preparation of finished product R: The preparation of the finished product R comprises the following steps:

[0044] B1: Add low molecular weight polyacrylamide, polyhydroxyethyl acrylamide and fumed silica to diethylene glycol ethyl ether acetate in a certain proportion, mix them evenly under high-speed stirring, and let them stand for 1h-1.5h to obtain intermediate B;

[0045] B2: Add titanate coupling agent and gemini cationic surfactant to intermediate B and stir evenly at high speed, let stand for 1-1.5 hours to obtain intermediate C;

[0046] B3: Add alkyl polyoxyethylene ether to intermediate C and stir evenly at high speed, and let stand for 1-2 hours to obtain intermediate D;

[0047] B4: Add intermediate S to intermediate D, mix well under high-speed stirring to obtain finished product R;

[0048] The addition amount of the above reaction materials is calculated by weight: 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S;

[0049] Preparation of S3 strong sand-carrying fracturing fluid: The finished product R is configured into a solution with a content of 0.1 wt % to obtain a micro-fracture network interface modified low-damage distal enhanced sand-carrying fracturing fluid.

[0050] In one embodiment, the pH regulator in step A2 is an ethanol solution of diethanolamine with a mass fraction of 10.0 wt%.

[0051] In one embodiment, the stirring speed in step A1 is 300-1000 r / min.

[0052] In one embodiment, in the step of preparing the S2 finished product R, the high-speed stirring speed is 1500-2500 r / min

[0053] Test example

[0054] The test example aims to obtain test data of the technical solution of the present invention by conducting specific tests and index evaluation on the technical solution of the present invention.

[0055] The test examples are conducted based on the implementation methods of the above-mentioned embodiments, and specific operable test parameters are given. Six test examples are set up, and the differences among the six test examples lie in the differences in the compatible components and raw materials. The test parameters and the test group component formulas will be specifically described below.

[0056] Formula: All six test examples include low molecular weight polyacrylamide, polyhydroxyethyl acrylamide, diethylene glycol ethyl ether acetate, fumed silica, titanate coupling agent, gemini cationic surfactant, alkyl polyoxyethylene ether, and intermediate S; intermediate S includes zirconium oxychloride and sodium lactate; diethylene glycol ethyl ether acetate.

[0057] Components: The strong sand-carrying fracturing fluid of the present invention is a solution prepared from the finished product R. The total weight of the material of the finished product R is set to 100g, and the actual amount added is calculated according to the number of components.

[0058] Test method:

[0059] S1 Preparation of intermediate S: The preparation of intermediate S comprises the following steps:

[0060] A1: Sodium lactate and zirconium oxychloride were mixed and added to diethylene glycol ethyl ether acetate, heated to 55°C under stirring, and reacted for 2.5 hours to obtain intermediate A; the effective content of sodium lactate was 99.5;

[0061] A2: Add pH regulator to intermediate A several times, sample 0.1% aqueous solution of intermediate A every 30 minutes to measure pH value, until pH value is 4.5, keep material temperature at 55°C, react for 5 hours, cool to room temperature to obtain intermediate S;

[0062] S2 Preparation of finished product R: The preparation of the finished product R comprises the following steps:

[0063] B1: According to a certain ratio, low molecular weight polyacrylamide, polyhydroxyethyl acrylamide and fumed silica are added to diethylene glycol ethyl ether acetate, mixed evenly under high-speed stirring, and allowed to stand for 1 hour to obtain intermediate B; the molecular weight of the low molecular weight polyacrylamide is 500, and the molecular weight of the polyhydroxyethyl acrylamide is 15 million.

[0064] B2: Add titanate coupling agent and gemini cationic surfactant to intermediate B and stir evenly at high speed, let stand for 1.5 hours to obtain intermediate C;

[0065] B3: Add alkyl polyoxyethylene ether to intermediate C and stir evenly at high speed, let stand for 2 hours to obtain intermediate D;

[0066] B4: Add intermediate S to intermediate D, mix well under high-speed stirring to obtain finished product R;

[0067] Preparation of S3 strong sand-carrying fracturing fluid: The finished product R is configured into a solution with a content of 0.1 wt % to obtain a micro-fracture network interface modified low-damage distal enhanced sand-carrying fracturing fluid.

[0068] More specifically, the pH regulator in step A2 is an ethanol solution of diethanolamine with a mass fraction of 10.0 wt%.

[0069] More specifically, the stirring speed in step A1 is 800 r / min.

[0070] More specifically, in the preparation step of the S2 finished product R, the high-speed stirring speed is 2200 r / min.

[0071] The present invention sets 6 specific test examples, and the test example formula components are as follows:

[0072] Test Example 1:

[0073] The intermediate S component includes 15 parts of zirconium oxychloride, 20 parts of sodium lactate, and 70 parts of diethylene glycol ethyl ether acetate;

[0074] The finished product R component includes 30 parts of polyacrylamide, 25 parts of polyhydroxyethyl acrylamide, 65 parts of diethylene glycol ethyl ether acetate, 5 parts of fumed silica, 5 parts of isopropyl triisostearate titanate, 5 parts of didodecyl dimethyl ammonium chloride, 5 parts of dodecylamino polyoxyethylene ether, and 5 parts of intermediate S.

[0075] Test Example 2:

[0076] The intermediate S component includes 10 parts of zirconium oxychloride, 20 parts of sodium lactate, and 70 parts of diethylene glycol ethyl ether acetate;

[0077] The finished product R component includes 20 parts of polyacrylamide, 30 parts of polyhydroxyethyl acrylamide, 65 parts of diethylene glycol ethyl ether acetate, 5 parts of fumed silica, 5 parts of isopropyl triisostearate titanate, 5 parts of didodecyl dimethyl ammonium chloride, 5 parts of dodecylamino polyoxyethylene ether, and 5 parts of intermediate S.

[0078] Test Example 3:

[0079] The intermediate S component includes 15 parts of zirconium oxychloride, 25 parts of sodium lactate, and 70 parts of diethylene glycol ethyl ether acetate;

[0080] The finished product R component includes 30 parts of polyacrylamide, 30 parts of polyhydroxyethyl acrylamide, 65 parts of diethylene glycol ethyl ether acetate, 2 parts of fumed silica, 3 parts of bistriethanolamine diisopropyl titanate, 2 parts of didodecyl dimethyl ammonium chloride, 5 parts of dodecylamino polyoxyethylene ether, and 5 parts of intermediate S.

[0081] Test example 4:

[0082] The intermediate S component includes 15 parts of zirconium oxychloride, 25 parts of sodium lactate, and 65 parts of diethylene glycol ethyl ether acetate;

[0083] The finished product R component includes 30 parts of polyacrylamide, 30 parts of polyhydroxyethyl acrylamide, 65 parts of diethylene glycol ethyl ether acetate, 2 parts of fumed silica, 7 parts of isopropyl titanate triisostearate, 7 parts of ditetradecyl dimethyl ammonium chloride, 5 parts of dodecylamino polyoxyethylene ether, and 5 parts of intermediate S.

[0084] Test Example 5:

[0085] The intermediate S component includes 15 parts of zirconium oxychloride, 25 parts of sodium lactate, and 80 parts of diethylene glycol ethyl ether acetate;

[0086] The finished product R component includes 30 parts of polyacrylamide, 30 parts of polyhydroxyethyl acrylamide, 75 parts of diethylene glycol ethyl ether acetate, 10 parts of fumed silica, 5 parts of isopropyl titanate triisostearate, 5 parts of didodecyl dimethyl ammonium chloride, 5 parts of dodecylamino polyoxyethylene ether, and 5 parts of intermediate S.

[0087] Test Example 6:

[0088] The intermediate S component includes 25 parts of zirconium oxychloride, 25 parts of sodium lactate, and 80 parts of diethylene glycol ethyl ether acetate;

[0089] The finished product R component includes 30 parts of polyacrylamide, 10 parts of polyhydroxyethyl acrylamide, 50 parts of diethylene glycol ethyl ether acetate, 5 parts of fumed silica, 5 parts of isopropyl titanate triisostearate, 5 parts of didodecyl dimethyl ammonium chloride, 5 parts of hexadecylamino polyoxyethylene ether, and 10 parts of intermediate S.

[0090] Conclusion: A series of indexes were measured in the above test examples 1-6, as shown in Table 1. Compared with the index requirements, test examples 1-6 all meet the requirements and show good comprehensive performance indicators. Test example 1 is the best formula, and the 0.1wt% liquid viscosity, sand carrying capacity, residue content and interfacial tension of this formula are the best.

[0091] Table 1 Test example evaluation data table

[0092]

[0093]

[0094] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A micro-fracture network interface modified distal strong sand-carrying fracturing fluid, characterized in that: The invention comprises, by weight, 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S; the intermediate S comprises, by weight, 10-25 parts of zirconium oxychloride and 5-25 parts of sodium lactate; 65-85 parts of diethylene glycol ethyl ether acetate.

2. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 1, characterized in that: The effective content of sodium lactate is greater than 99%.

3. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 1, characterized in that: The molecular weight of the low molecular weight polyacrylamide is 3 million to 8 million, and the molecular weight of the polyhydroxyethyl acrylamide is 5 million to 30 million.

4. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 1, characterized in that: The titanate coupling agent is one or more of isopropyl tri(dioctyl pyrophosphate) titanate, isopropyl triisostearate titanate, and bistriethanolamine diisopropyl titanate, and the gemini cationic surfactant is one or more of didodecyl dimethyl ammonium chloride, dihexadecyl dimethyl ammonium chloride, and ditetradecyl dimethyl ammonium chloride.

5. The micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 1, characterized in that: The alkyl polyoxyethylene ether is one or more of octadecylamino polyoxyethylene ether, dodecylamino polyoxyethylene ether, and hexadecylamino polyoxyethylene ether.

6. A method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to any one of claims 1 to 5, characterized in that: The steps include: S1 Preparation of intermediate S: The preparation of intermediate S comprises the following steps: A1: By weight, 5-25 parts of sodium lactate and 10-25 parts of zirconium oxychloride are mixed and added to 65-85 parts of diethylene glycol ethyl ether acetate, heated to 50±5°C under stirring, and reacted for 2-3h to obtain intermediate A; A2: Add pH regulator to intermediate A several times, sample 0.1% aqueous solution of intermediate A every 30 minutes to measure pH value, until pH value is 4-5, keep material temperature at 50±5℃, react for 4-5h, cool to room temperature to obtain intermediate S, the weight ratio of pH regulator added each time to intermediate A is 1:1000; S2 Preparation of finished product R: The preparation of the finished product R comprises the following steps: B1: Add low molecular weight polyacrylamide, polyhydroxyethyl acrylamide and fumed silica to diethylene glycol ethyl ether acetate in a certain proportion, mix them evenly under high-speed stirring, and let them stand for 1h-1.5h to obtain intermediate B; B2: Add titanate coupling agent and gemini cationic surfactant to intermediate B and stir evenly at high speed, let stand for 1-1.5 hours to obtain intermediate C; B3: Add alkyl polyoxyethylene ether to intermediate C and stir evenly at high speed, and let stand for 1-2 hours to obtain intermediate D; B4: Add intermediate S to intermediate D, mix well under high-speed stirring to obtain finished product R; The addition amount of the above reaction materials is calculated by weight: 20-50 parts of low molecular weight polyacrylamide, 10-30 parts of polyhydroxyethyl acrylamide, 30-75 parts of diethylene glycol ethyl ether acetate, 2-10 parts of fumed silica, 3-12 parts of titanate coupling agent, 2-7 parts of gemini cationic surfactant, 2-7 parts of alkyl polyoxyethylene ether, and 2-7 parts of intermediate S; Preparation of S3 strong sand-carrying fracturing fluid: The finished product R is configured into a solution with a content of 0.1wt% to obtain a micro-fracture network interface modified low-damage distal enhanced sand-carrying fracturing fluid.

7. The method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 6, characterized in that: In the step A2, the pH regulator is an ethanol solution of diethanolamine with a mass fraction of 10.0 wt%.

8. The method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 6, characterized in that: The stirring speed in step A1 is 300-1000 r / min.

9. The method for preparing a micro-fracture network interface modified distal strong sand-carrying fracturing fluid according to claim 6, characterized in that: In the preparation step of the S2 finished product R, the high-speed stirring speed is 1500-2500r / min.

Citation Information

Patent Citations

  • Densifier and fracturing fluid for shale gas fracturing fluid, preparation method and application thereof

    CN103756664A

  • A multifunctional composite fracturing fluid system

    CN105219372B

  • Ultra-temperature organic zirconium crosslinker suitable for polymer crosslinking and prepared fracturing solutions of ultra-temperature organic zirconium crosslinker

    CN102838781A

  • Fracturing fluid and preparation method thereof

    CN110699060A

  • Direct adding type suspending agent for real-time modification of proppant in fracturing process and application of direct adding type suspending agent

    CN116064026A

Cited By

  • Integrated composite transformation liquid and preparation method thereof

    CN119529812A

  • Integrated composite transformation liquid and preparation method thereof

    CN120118676A