Red fluorescent material, preparation method and application thereof, energy down-conversion film and preparation thereof

By coating the surface of the solar cell with red fluorescent material and energy conversion film, converting ultraviolet or blue light in sunlight into near-red light, the problem of poor spectral response of solar cells is solved, and the photoelectric conversion efficiency and spectral utilization rate are improved .

CN118995206AActive Publication Date: 2024-11-22LANZHOU UNIV

Patent Information

Application Number
CN202411035747.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22
Estimated Expiration
2044-07-31

Smart Images

  • Figure CN118995206A_ABST
    Figure CN118995206A_ABST
Patent Text Reader

Abstract

The invention provides a red fluorescent material, a preparation method and application thereof, an energy down-conversion film and preparation thereof, and belongs to the technical field of luminescent materials. The chemical composition of the red fluorescent material is Ba < 1-x > Mg < 1-y > Al < 10-z > O < 17 >: xEu < 2 + >, yMn < 2 + >, zCr < 3 + >, wherein 0 lt; x is less than or equal to 0.5, 0lt; y is less than or equal to 0.5, 0lt; the material has a wide excitation spectrum coverage area, can be excited by ultraviolet light or blue light in sunlight so as to emit near-red light or red light, and can directly convert ultraviolet light with the wavelength of 300-400nm into red light with the wavelength of 650-750nm, so that the problem of spectrum mismatch of a solar cell is solved, the light utilization rate of the solar cell is improved, and the photoelectric conversion efficiency of a solar device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of luminescent materials, and in particular to a red fluorescent material and a preparation method and application thereof, an energy down-conversion film and a preparation thereof. Background Art

[0002] Among the common renewable energy sources, solar energy stands out from many clean energy sources such as ocean energy, wind energy, geothermal energy, and biomass energy due to its abundant sources, unlimited "storage capacity", environmental friendliness, and easy clean utilization. In recent years, solar energy has become the top priority of clean energy development with its own incomparable advantages, and has gradually become active in various fields of energy utilization.

[0003] For the utilization of solar energy, solar cells are the most common device that can convert sunlight energy into electricity for human production and life through the photovoltaic effect. It is also a long-term sustainable way of energy production with many advantages such as green and low carbon. Although the technology of crystalline silicon solar cells is very mature, the maximum photoelectric conversion rate of existing crystalline silicon solar cells on the market is only 26%. Fundamentally, the low photoelectric conversion rate of silicon solar cells is due to the poor response of silicon solar cells to the spectrum of sunlight and the short penetration depth of short-wavelength photons in silicon materials. The band gap of silicon is about 1.1eV, corresponding to a wavelength of 1100nm. Therefore, photons with energy less than the band gap (wavelength>1100nm) cannot generate carriers, while photons with wavelengths much less than 1100nm have energy much greater than 1.1eV, and excess energy will be dissipated in the form of heat, causing energy waste. Therefore, silicon solar cells have a good spectral response in the red to near-infrared part (600nm~1100nm), and a weak spectral response in the 200nm~600nm band, and there is a spectral mismatch problem.

[0004] In view of the spectrum mismatch problem of solar cells, researchers have found that the spectrum conversion effect can be used to effectively utilize the solar spectrum, that is, the band light that is poorly absorbed by silicon-based solar cells is converted into a band light that can be effectively absorbed by spectrum conversion, thereby improving the spectrum utilization rate of solar cells. In most existing studies, one method for applying phosphors to solar cells is to directly cover the phosphors on the surface of silicon-based solar cells by spin coating. However, the problems of the phosphors and solar cells in this method are unstable efficiency, low improvement in solar cell photoelectric conversion efficiency, low light source energy utilization efficiency, and unsuitability for industrial large-scale production, which limit the application of this method. Another application method is to mix phosphors with copolymers to make a spectrum transfer film (CN113078223A). Although this method can be more directly applied to the surface of solar cells and better overcome the lower spectral response in the short-wave region, its biggest disadvantage is that due to the easier reflection of short-wavelength light, a considerable part of short-wavelength photons are reflected into the air without being absorbed by the battery, thus resulting in a lower photoelectric conversion rate. Summary of the invention

[0005] The object of the present invention is to provide a red fluorescent material and a preparation method and application thereof, an energy down-conversion film and its preparation. The red fluorescent material can be excited by ultraviolet light or blue light in sunlight to emit near-red light or red light. The EDC film prepared using the red fluorescent material improves the utilization rate of sunlight by solar cells by converting ultraviolet or blue light in sunlight into near-red light or red light that is easily absorbed by solar cells, thereby improving the photoelectric conversion rate.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a red fluorescent material, the chemical composition of which is Ba 1-x Mg 1-y Al 10-z O 17 :xEu 2+ ,yMn 2+ ,zCr 3 + ; Among them, 0 <x≤0.5,0<y≤0.5,0<z≤0.05。

[0008] Preferably, x=0.3, y=0.3 and z=0.03.

[0009] The present invention provides a method for preparing the red fluorescent material described in the above technical solution, comprising the following steps:

[0010] The Ba source, Mg source, Al source, Eu source, Mn source, Cr source and flux are ground and mixed, the obtained mixture is sintered in a reducing atmosphere, and the surface sample is removed to obtain a red fluorescent material.

[0011] Preferably, the Ba source includes BaO, BaCO3, Ba(OH)2·8H2O, Ba(NO3)2, BaSO4 or BaCl2;

[0012] The Mg source includes MgO, MgCO3, Mg(OH)2, Mg(NO3)2·6H2O or MgCl2;

[0013] The Al source includes Al2O3, Al(OH)3, AlOOH, Al(NO3)3·9H2O, Al2(SO4)3 or AlCl3;

[0014] The Eu source includes Eu2O3, Eu2(SO4)3, Eu(NO3)3·6H2O, EuCl2, EuCl3 or EuF3;

[0015] The Mn source includes MnO, MnO2, Mn2O3, Mn3O4, MnCO3, Mg(OH)2, Mn(NO3)2·6H2O or MnCl2·4H2O;

[0016] The Cr source includes Cr2O3, Cr(NO3)3·9H2O, CrCl2·6H2O or CrF3;

[0017] The flux includes AlF3, KF, LiF, NaF, BaF2, NH4Cl or H3BO3.

[0018] Preferably, the mass of the flux is 0-7wt% of the total mass of the Ba source, Mg source, Al source, Eu source, Mn source and Cr source and is not 0; the reducing atmosphere is a N2+H2 mixed atmosphere, and the volume ratio of N2 to H2 is 9:1; the sintering temperature is 1450-1600°C, and the time is 2-6h.

[0019] The present invention provides the use of the red fluorescent material described in the above technical solution or the red fluorescent material prepared by the preparation method described in the above technical solution in a solar cell.

[0020] The present invention provides a method for preparing an energy down-conversion film, comprising the following steps:

[0021] Mixing an organic polymer with an organic solvent, and mixing the obtained colloidal polymer with a red fluorescent material to obtain a colloidal powder mixture; the red fluorescent material is the red fluorescent material described in the above technical solution or the red fluorescent material prepared by the preparation method described in the above technical solution;

[0022] Coat the powdered rubber mixture on the surface of the solar cell and dry it to obtain an energy down-conversion thin film.

[0023] Preferably, the organic polymer includes ethylene-vinyl acetate copolymer, polyvinylpyrrolidone, ethylene-octene copolymer or epoxy resin.

[0024] Preferably, the dosage ratio of the organic polymer to the organic solvent is 3 g:10 mL to 1 g:20 mL; the mass ratio of the red fluorescent material to the colloidal polymer is 1:10 to 100.

[0025] The present invention provides an energy down-conversion thin film prepared by the preparation method described in the above technical solution.

[0026] The present invention provides a red fluorescent material with a chemical composition of Ba 1-x Mg 1-y Al 10-z O 17 :xEu 2+ ,yMn 2+ ,zCr 3 + ; wherein, 0 < x ≤ 0.5, 0 < y ≤ 0.5, 0 < z ≤ 0.05. This red fluorescent material contains Eu 2+ ,Mn 2+ ,Cr 3+ triple activators, wherein Eu 2+ is a parity and spin-allowed transition, and the emission is located at 400 - 500 nm; Mn 2+ is a parity and spin-forbidden transition, and the emission is located at 480 - 560 nm; Cr 3+ is a parity-forbidden transition, and there may also be a spin-forbidden transition or a spin-allowed transition, and the emission is located at 650 - 750 nm. The present invention incorporates three activator ions into the BaMgAl 10 O 17 matrix. The multiple energy transfers between Eu 2+ -Mn 2+ -Cr 3+ ions can not only effectively enhance the emission intensity of each ion, thereby enhancing the emission intensity of BaMgAl 10 O 17 , but also greatly broaden the spectral range. Therefore, the excitation spectrum of this red fluorescent material covers a wide range and can be excited by ultraviolet light or blue light in sunlight to emit near-red light or red light, directly converting ultraviolet light with a wavelength of 300 - 400 nm into red light with a wavelength of 650 - 750 nm (corresponding to the optimal response wavelength region of the solar cell), thereby improving the spectral mismatch problem of the solar cell, enhancing the light utilization rate of the solar cell, and improving the photoelectric conversion efficiency of the solar device.

[0027] The red fluorescent material of the present invention is prepared by a high-temperature solid phase method combined with sintering in a reducing atmosphere. The preparation method of the present invention is simple and easy to operate, does not produce harmful substances, is green, environmentally friendly and pollution-free, has low cost and can stably improve the sunlight utilization rate of silicon-based solar cells, and has broad application prospects.

[0028] The present invention introduces a red fluorescent material into an organic polymer as a light conversion agent and is coated on the surface of a solar cell to prepare an energy down-conversion film, thereby realizing the synergistic coupling between the organic polymer light conversion film and the solar cell. The prepared energy down-conversion film improves the absorption capacity of the solar cell spectrum by effectively converting ultraviolet or blue light with poor photoelectric response in sunlight into near-red light or red light that is easily absorbed by silicon-based solar cells, and can effectively enhance the absorption efficiency of solar cells in the near-ultraviolet region, improve the utilization rate of sunlight, and further improve the photoelectric conversion efficiency, thereby realizing effective coupling. Therefore, the red fluorescent material of the present invention has a high quantum efficiency, and can overcome the problem of low conversion rate caused by mixing phosphors with copolymers to prepare spectrum down-conversion films.

[0029] The spectrum of the red fluorescent material of the present invention has a high degree of matching with the solar spectrum, and can better achieve spectral response with solar cells. When the energy down-conversion film prepared from the fluorescent material is effectively coupled with the silicon-based solar cell, the silicon-based solar cell can absorb more red light, thereby maximizing the utilization of solar energy and improving the photoelectric conversion efficiency of the solar cell.

[0030] Furthermore, the present invention adopts EVA organic polymer to prepare the energy down-conversion film, which not only has good light transmittance and does not physically hinder sunlight, but also has high adhesion performance and is not prone to falling off, and can be applied on a large scale. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 is Ba in Example 1 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ XRD pattern of phosphor;

[0032] Figure 2 is Ba in Example 1 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr3+ EDS image of phosphor;

[0033] Figure 3 is Ba in Example 1 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ Excitation and emission spectra of phosphors;

[0034] Figure 4 is Ba in Example 1 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ Quantum efficiency diagram of phosphors;

[0035] Figure 5 is Ba in Example 1 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ Particle size distribution of phosphor;

[0036] Figure 6 This is a comparison chart of the luminous intensity of the phosphors obtained in Example 1 and Comparative Example 1;

[0037] Figure 7 Schematic diagram of the model combining silicon solar cell with phosphor-energy down-conversion film;

[0038] Figure 8 This is a comparison diagram of IV curves of a silicon-based solar cell with a BAM-EVA light-conversion film coating and a bare solar cell in Example 1;

[0039] Fig. 9 The quantum efficiency curves of the silicon-based solar cell with the BAM-EVA light conversion film coating and the bare solar cell in Example 1;

[0040] Fig.10 This is a comparison chart of the luminous intensity of the phosphors prepared in Example 1 and Examples 6 to 10. DETAILED DESCRIPTION

[0041] The present invention provides a red fluorescent material, the chemical composition of which is Ba 1-x Mg 1-yAl 10-z O 17 :xEu 2+ ,yMn 2+ ,zCr 3 + ; wherein, 0 < x ≤ 0.5, 0 < y ≤ 0.5, 0 < z ≤ 0.05.

[0042] In the present invention, x, y, and z are in turn the 2+ Eu 2+ , Mn 3+ and Cr

[0043] In the present invention, preferably 0.1 < x ≤ 0.4, more preferably 0.2 < x ≤ 0.35; preferably 0.1 < y ≤ 0.4, more preferably 0.2 < y ≤ 0.35; preferably 0.01 < z ≤ 0.04, more preferably 0.02 < z ≤ 0.03.

[0044] As a preferred embodiment of the present invention, x = 0.3, y = 0.3 and z = 0.03, and the chemical composition of the corresponding red fluorescent material is Ba 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ .

[0045] The present invention provides a method for preparing the red fluorescent material described in the above technical solution, comprising the following steps:

[0046] Grind and mix a Ba source, a Mg source, an Al source, a Eu source, a Mn source, a Cr source, and a flux, sinter the obtained mixed material in a reducing atmosphere, and then remove the surface sample to obtain the red fluorescent material.

[0047] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well-known to those skilled in the art.

[0048] In the present invention, the Ba source preferably includes BaO, BaCO3, Ba(OH)2·8H2O, Ba(NO3)2, BaSO4 or BaCl2.

[0049] In the present invention, the Mg source preferably includes MgO, MgCO3, Mg(OH)2, Mg(NO3)2·6H2O or MgCl2.

[0050] In the present invention, the Al source preferably includes Al2O3, Al(OH)3, AlOOH, Al(NO3)3·9H2O, Al2(SO4)3 or AlCl3.

[0051] In the present invention, the Eu source preferably includes Eu2O3, Eu2(SO4)3, Eu(NO3)3·6H2O, EuCl2, EuCl3 or EuF3.

[0052] In the present invention, the Mn source preferably includes MnO, MnO2, Mn2O3, Mn3O4, MnCO3, Mg(OH)2, Mn(NO3)2·6H2O or MnCl2·4H2O.

[0053] In the present invention, the Cr source preferably includes Cr2O3, Cr(NO3)3·9H2O, CrCl2·6H2O or CrF3.

[0054] The molar ratio of the Ba source, Mg source, Al source, Eu source, Mn source and Cr source in the present invention only needs to satisfy the chemical composition of the red fluorescent material.

[0055] In the present invention, the flux preferably includes AlF3, KF, LiF, NaF, BaF2, NH4Cl or H3BO3, and more preferably AlF3; the mass of the flux is preferably 0 to 7 wt% of the total mass of the Ba source, Mg source, Al source, Eu source, Mn source and Cr source and is not 0, and more preferably 0.3 to 3 wt%.

[0056] The present invention preferably weighs Ba source, Mg source, Al source, Eu source, Mn source, Cr source and flux according to the chemical composition, adds anhydrous ethanol to grind in an agate mortar, and then puts them into an alumina crucible, and places the alumina crucible in a high-temperature tube furnace for sintering. The present invention has no special limitation on the amount of anhydrous ethanol used, and can be adjusted according to demand to ensure sufficient grinding.

[0057] In the present invention, the reducing atmosphere is preferably a N2+H2 mixed atmosphere, and the volume ratio of N2 to H2 is preferably 9:1.

[0058] In the present invention, the sintering temperature is preferably 1450-1600° C., more preferably 1500-1550° C., and further preferably 1525° C., and the sintering time is preferably 2-6 h, more preferably 3-5 h, and further preferably 4 h.

[0059] During the sintering process, part of the flux is completely volatilized during the sintering process, and the non-volatile flux exists on the surface of the sample after sintering. The flux can be removed by removing the surface sample, which will not affect the purity of the product.

[0060] After the sintering is completed, the present invention preferably takes out the obtained product and grinds it again with a porcelain mortar and dries it to obtain a red fluorescent material. The present invention has no special limitation on the grinding and drying, and can be carried out according to the process well known in the art.

[0061] The present invention provides the use of the red fluorescent material described in the above technical solution or the red fluorescent material prepared by the preparation method described in the above technical solution in a solar cell.

[0062] The present invention provides a method for preparing an energy down-conversion film, comprising the following steps:

[0063] Mixing an organic polymer with an organic solvent, and mixing the obtained colloidal polymer with a red fluorescent material to obtain a colloidal powder mixture; the red fluorescent material is the red fluorescent material described in the above technical solution or the red fluorescent material prepared by the preparation method described in the above technical solution;

[0064] The rubber powder mixture is coated on the surface of the solar cell and dried to obtain an energy down-conversion film.

[0065] In the present invention, the organic polymer includes ethylene-vinyl acetate copolymer (EVA), polyvinyl pyrrolidone, ethylene-octene copolymer (POE) or epoxy resin. The present invention has no particular limitation on the source and type of the organic polymer, and any commercially available product known in the art can be used.

[0066] In the present invention, the organic solvent is preferably toluene; the usage ratio of the organic polymer to the organic solvent is preferably 3g:10mL to 1g:20mL, more preferably 1g:4mL.

[0067] In the present invention, the mass ratio of the red fluorescent material to the colloidal polymer is preferably 1:10-100, more preferably 1:15-80, and further preferably 1:20-50.

[0068] The present invention preferably mixes the colloidal polymer and the red fluorescent material, and then stirs them in a vacuum degassing machine for 5 minutes (stirring allows the red fluorescent material to be evenly dispersed in the colloidal polymer to avoid bubbles and segregation) to obtain a glue powder mixture, and uses a glue spreader to coat the glue powder mixture on the surface of the solar cell at room temperature at a rate of 1200 to 2000 rpm / s (more preferably 1600 rpm / s) until the surface is smooth, removes the cell, and naturally air-dries to obtain an energy down-conversion film.

[0069] The present invention has no particular limitation on the solar cell, and any commercially available product known in the art may be used.

[0070] The present invention has no special limitation on the coating method, and any method known in the art may be used, and spin coating is more preferred. The thickness of the film formed by the glue powder mixture on the surface of the solar cell is preferably 0.005-0.030 mm, more preferably 0.013-0.016 mm, which can avoid affecting the light transmittance or the phosphor being unable to function.

[0071] The present invention provides an energy down-conversion film prepared by the preparation method described in the above technical solution.

[0072] Silicon-based solar cells generally have a weak photoelectric response in the ultraviolet range (300-400nm), and a strong photoelectric response in the visible light to red light and near-infrared range (600-1100nm). The energy down-conversion film can absorb ultraviolet or blue light, emit visible light or near-infrared light that is beneficial for silicon-based solar cells to absorb, and reduce scattered light, thereby improving its utilization of sunlight. Therefore, the energy down-conversion film of the present invention will transmit more red light, which will be absorbed by the solar cell, thereby improving the photoelectric conversion efficiency of the solar cell.

[0073] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0074] Example 1

[0075] According to the required chemical composition, 0.1379gBaCO3, 0.0280gMgO, 0.5085gAl2O3, 0.0528gEu2O3, 0.0345gMnCO3, 0.0023Cr2O3 and 0.0229gAlF3 were weighed, 5mL of anhydrous ethanol was added to an agate mortar for grinding, and then put into an alumina crucible, which was placed in a high-temperature tube furnace and sintered for 4h at a high temperature environment of 1525℃ and a reducing atmosphere of N2+H2 (the volume ratio of N2 to H2 was 9:1) to obtain Ba 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ Phosphor, i.e. z = 0.03;

[0076] According to the mass ratio of ethylene-vinyl acetate copolymer (EVA): phosphor is 15:1 and the amount ratio of ethylene-vinyl acetate copolymer (EVA): toluene is 1g:4mL, 2.5g ethylene-vinyl acetate copolymer (EVA), 10.0mL toluene and 0.1667g Ba were weighed respectively. 0.7 Mg 0.7 Al 9.97 O17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ The phosphor and EVA were placed in a vacuum degassing machine for vacuum stirring for 5 minutes to obtain a glue powder mixture, and the glue powder mixture was spin-coated on the surface of a silicon-based solar cell (a heterojunction HJT cell) at a rate of 1600 rpm / s using a glue homogenizer at room temperature (e.g. Figure 7 As shown), remove the battery after the surface is smooth, and naturally air-dry to obtain a silicon-based solar cell with a BAM-EVA energy conversion thin film coating.

[0077] Example 2

[0078] The only difference from Example 1 is that 2.5 g of ethylene-vinyl acetate copolymer (EVA), 10.0 mL of toluene, and 0.25 g of Ba are weighed respectively according to the mass ratio of ethylene-vinyl acetate copolymer (EVA) to phosphor powder of 10:1. 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.03Cr 3+ Phosphor, according to the same spin coating steps as in Example 1, a silicon-based solar cell with a BAM-EVA energy down-conversion thin film coating was prepared.

[0079] Example 3

[0080] The only difference from Example 1 is that 2.5 g of ethylene-vinyl acetate copolymer (EVA), 10.0 mL of toluene, and 0.125 g of Ba are weighed respectively according to the mass ratio of ethylene-vinyl acetate copolymer (EVA) to phosphor powder of 20:1. 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2 + ,0.3Mn 2+ ,0.03Cr 3+ Phosphor, according to the same spin coating steps as in Example 1, a silicon-based solar cell with a BAM-EVA energy down-conversion thin film coating was prepared.

[0081] Example 4

[0082] The only difference from Example 1 is: weigh the same raw material ratio as in Example 1, put the phosphor and EVA into a vacuum degassing machine for vacuum stirring for 5 minutes to obtain a glue powder mixture, change the rotation speed of the glue spreader during spin coating, and spin coat the glue powder mixture on the surface of the silicon-based solar cell at a rate of 1200 rpm / s to prepare a silicon-based solar cell with a BAM-EVA energy conversion thin film coating.

[0083] Example 5

[0084] The only difference from Example 1 is: weigh the same raw material ratio as in Example 1, put the phosphor and EVA into a vacuum degassing machine for vacuum stirring for 5 minutes to obtain a glue powder mixture, change the rotation speed of the glue spreader during spin coating, and spin coat the glue powder mixture on the surface of the silicon-based solar cell at a rate of 2000 rpm / s to prepare a silicon-based solar cell with a BAM-EVA energy conversion thin film coating.

[0085] Example 6

[0086] The only difference from Example 1 is that: z = 0.001, and Ba is obtained. 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.001Cr 3+ Phosphor, specific dosage of raw materials is shown in Table 1.

[0087] Example 7

[0088] The only difference from Example 1 is that: z = 0.005, Ba is obtained 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.005Cr 3+ Phosphor, specific dosage of raw materials is shown in Table 1.

[0089] Example 8

[0090] The only difference from Example 1 is that: z = 0.01, and Ba is obtained. 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.01Cr 3+ Phosphor, specific dosage of raw materials is shown in Table 1.

[0091] Example 9

[0092] The only difference from Example 1 is that z = 0.02, and Ba is obtained. 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.02Cr 3+ Phosphor, specific dosage of raw materials is shown in Table 1.

[0093] Example 10

[0094] The only difference from Example 1 is that: z = 0.05, Ba is obtained 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2+ ,0.05Cr 3+ Phosphor, specific dosage of raw materials is shown in Table 1.

[0095] The amounts of raw materials used in Examples 1 and 6 to 10 are shown in Table 1.

[0096] Table 1 Amount of raw materials used in Example 1 and Examples 6 to 10 (g)

[0097]

[0098]

[0099] Comparative Example 1

[0100] The only difference from Example 1 is that no flux AlF3 is added, the remaining raw materials are weighed according to the same mass as in Example 1, and the sintering steps are the same as in Example 1 to obtain Ba 0.7 Mg 0.7 Al 9.97 O 17 :0.3Eu 2+ ,0.3Mn 2 + ,0.03Cr 3+ Phosphor.

[0101] Performance Testing

[0102] 1) Figure 1 The XRD pattern of the phosphor prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the diffraction peaks of the phosphor are well matched with the standard PDF card, indicating that BaMgAl 10 O 17 phase and does not contain any other impurity phases.

[0103] Figure 2 This is the EDS image of the phosphor prepared in Example 1. Figure 2 It can be seen that the constituent elements Ba, Mg, Al, O, Eu, Mn, and Cr were successfully detected on the surface of the phosphor particles. Each element is evenly distributed on the surface of the entire sample particle, indicating that Eu, Mn, and Cr were successfully doped into BaMgAl 10 O 17 in the matrix.

[0104] 2) Figure 3 is the excitation and emission spectrum of the phosphor in Example 1, Figure 3 It can be seen that the excitation spectrum of the phosphor covers 250-400nm, with the best excitation at 335nm; the emission is a broadband emission of 450-750nm, with the best emission at 692nm, which belongs to near-infrared emission. It can be seen that the phosphor can be excited by sunlight to emit red light, which can convert the blue-violet light with poor spectral response of solar cells into red light with better response, thus realizing spectral conversion.

[0105] 3) Figure 4 is the quantum efficiency diagram of the phosphor in Example 1, Figure 4 It can be seen that the phosphor has excellent absorption coefficient and quantum efficiency. Under 365nm ultraviolet light excitation, the absorption coefficient AE is as high as 86.1%, the internal quantum efficiency (IQE) and external quantum efficiency (EQE) are 79.5% and 68.4% respectively. The excellent quantum efficiency of the phosphor ensures high light conversion efficiency.

[0106] 4) Figure 5 is the particle size distribution diagram of the phosphor in Example 1, Figure 5 It can be seen that the particle size distribution is mainly concentrated in 5-15μm, the average particle size is 10.72μm, and the particle size is at the micron level. Therefore, the size of the fluorescent material is small, which ensures the luminous intensity of the material without too much physical obstruction to the sunlight, providing a guarantee for high light conversion efficiency.

[0107] 5) Figure 6 is a comparison chart of the luminous intensity of the phosphors in Example 1 and Comparative Example 1, Figure 6 It can be seen that the luminescence performance of the phosphor can be effectively improved by adding flux AlF3.

[0108] 6) The performance of the solar cell containing the BAM-EVA energy conversion thin film coating prepared in Example 1 was tested under vertical irradiation of a solar simulator to observe the difference in photoelectric conversion efficiency of the silicon-based solar cell before and after coating. The IV curves of the bare cell and the coated solar cell were obtained as shown in the following figure: Figure 8 As shown. Figure 8 It can be seen that after coating with BAM-EVA light-converting film, the JSC There is a clear increasing trend.

[0109] 7) Verify the effect of BAM-EVA energy down-conversion film on solar cells. The external quantum efficiency (EQE) curve of the solar cell containing BAM-EVA energy down-conversion film coating prepared in Example 1 in the wavelength range of 300 to 1100 nm is as follows: Fig. 9 As shown. Fig. 9 It can be seen that in the blue light range, the external quantum efficiency of the bare cell sample is lower than that of the BAM-EVA energy conversion film coating sample, but in the rest of the spectral range, the EQE curves of the two devices are basically the same. Therefore, it can be concluded that J SC The increase is related to the application of BAM-EVA energy down-conversion film, which improves the absorption of blue-violet light by solar cells and converts it into red light with a stronger photoelectric response, effectively improving the photoelectric conversion efficiency of solar cells. Therefore, based on the light conversion effect of BAM-EVA energy down-conversion film, silicon-based solar cells with BAM-EVA energy down-conversion film coating have higher conversion efficiency than bare solar cells.

[0110] 7) The IV curves of the silicon-based solar cells in Examples 1 to 5 were tested, and the obtained parameters are shown in Table 2.

[0111] Table 2 IV curve parameters of silicon-based solar cells in Examples 1 to 5

[0112]

[0113]

[0114] The fluorescent material provided by the present invention can provide extremely long wavelength near infrared light (NIR) from the extremely short wavelength light source near ultraviolet light (NUV) in sunlight, which can greatly improve the efficiency of silicon-based solar cells. As can be seen from Table 2, Example 1 has the highest improvement in the light-to-electricity conversion efficiency of silicon-based solar cells, and the fluorescent material can increase the photoelectric conversion efficiency by up to 6.684%.

[0115] 8) Fig.10 The luminous intensity comparison diagram of the phosphors prepared in Example 1 and Examples 6 to 10; Fig.10 It can be seen that with the increase of Cr 3+ With the increase of doping concentration, Eu 2+ The blue emission peak intensity of Mn 2+ The green emission peak intensity of Cr 3+The characteristic emission peak intensity gradually increases. When z=0.03, the luminescence intensity reaches the highest, and then concentration quenching occurs and the luminescence intensity of the sample decreases.

[0116] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A red fluorescent material, characterized in that: The chemical composition is Ba 1-x Mg 1-y Al 10-z O 17 :xEu 2+ ,yMn 2+ ,zCr 3+ ; Among them, 0 <x≤0.5,0<y≤0.5,0<z≤0.05。 2. The red fluorescent material according to claim 1, characterized in that: x=0.3, y=0.3 and z=0.

03.

3. The method for preparing the red fluorescent material according to claim 1 or 2, characterized in that: The following steps are involved: The Ba source, Mg source, Al source, Eu source, Mn source, Cr source and flux are ground and mixed, the obtained mixture is sintered in a reducing atmosphere, and the surface sample is removed to obtain a red fluorescent material.

4. The preparation method according to claim 3, characterized in that: The Ba source includes BaO, BaCO3, Ba(OH)2·8H2O, Ba(NO3)2, BaSO4 or BaCl2; The Mg source includes MgO, MgCO3, Mg(OH)2, Mg(NO3)2·6H2O or MgCl2; The Al source includes Al2O3, Al(OH)3, AlOOH, Al(NO3)3·9H2O, Al2(SO4)3 or AlCl3; The Eu source includes Eu2O3, Eu2(SO4)3, Eu(NO3)3·6H2O, EuCl2, EuCl3 or EuF3; The Mn source includes MnO, MnO2, Mn2O3, Mn3O4, MnCO3, Mg(OH)2, Mn(NO3)2·6H2O or MnCl2·4H2O; The Cr source includes Cr2O3, Cr(NO3)3·9H2O, CrCl2·6H2O or CrF3; The flux includes AlF3, KF, LiF, NaF, BaF2, NH4Cl or H3BO3.

5. The preparation method according to claim 3, characterized in that: The mass of the flux is 0-7wt% of the total mass of the Ba source, Mg source, Al source, Eu source, Mn source and Cr source and is not 0; the reducing atmosphere is a N2+H2 mixed atmosphere, and the volume ratio of N2 to H2 is 9:1; the sintering temperature is 1450-1600°C, and the time is 2-6h.

6. Use of the red fluorescent material according to any one of claims 1 to 2 or the red fluorescent material prepared by the preparation method according to any one of claims 3 to 5 in solar cells.

7. A method for preparing an energy down-conversion film, characterized in that: The following steps are involved: Mixing an organic polymer with an organic solvent, and mixing the obtained colloidal polymer with a red fluorescent material to obtain a colloidal powder mixture; the red fluorescent material is the red fluorescent material according to any one of claims 1 to 2 or the red fluorescent material prepared by the preparation method according to any one of claims 3 to 5; The rubber powder mixture is coated on the surface of the solar cell and dried to obtain an energy down-conversion film.

8. The preparation method according to claim 7, characterized in that: The organic polymer includes ethylene-vinyl acetate copolymer, polyvinyl pyrrolidone, ethylene-octene copolymer or epoxy resin.

9. The preparation method according to claim 7 or 8, characterized in that: The dosage ratio of the organic polymer to the organic solvent is 3g:10mL to 1g:20mL; the mass ratio of the red fluorescent material to the colloidal polymer is 1:10 to 100.

10. The energy down-conversion film prepared by the preparation method according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Europium and manganese codoped and activated blue-green fluorescent powder and preparation method thereof

    CN102127429A

  • Light conversion phosphor powder and preparation method thereof

    CN108517209A

  • Violet light excitated bicomponent three basic colour fluorescent powder and its preparation method

    CN1478855A

Cited By

  • Perovskite quantum dot based on halogen component regulation and control, preparation method and application thereof, perovskite solar cell and photoelectric device