Monocrystalline silicon alkali polishing additive for preparing fused tower footing and use method thereof
By using a single crystal silicon alkaline polishing additive composed of accelerator, defoaming agent, corrosion inhibitor and surfactant in the alkali polishing process, the fusion base is formed, and the environmental pollution of the acid polishing process and the alkali polishing process are solved. The tower base has a single shape and poor flatness, which improves the reflectivity and photoelectric conversion efficiency of the back of the silicon wafer.
Patent Information
- Application Number
- CN202411129438.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, the acid polishing process has environmental pollution problems, while the alkali polishing process has problems such as single shape of the tower base, poor flatness, low reflectivity and small foundation.
A single crystal silicon alkali polishing additive composed of accelerator, defoaming agent, corrosion inhibitor and surfactant is used to form a polishing liquid by heating and stirring in the alkali liquid, and the silicon wafer is polished to form a fusion base. Improve the flatness and reflectivity of the back of the silicon wafer.
It reduces environmental pollution, solves the problems of single morphology and poor flatness of the tower foundation during alkali polishing, improves the reflectivity and photoelectric conversion efficiency of the back of the silicon wafer, and obtains high current.
Smart Images

Figure CN118995225A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a monocrystalline silicon alkali polishing additive for preparing a fused tower base and a use method thereof, belonging to the technical field of monocrystalline silicon battery sheets. Background Art
[0002] In the production process of crystalline silicon solar cells, back polishing has a positive impact on its key performance parameters such as short-circuit current (Isc), open-circuit voltage (Voc), and fill factor (FF), and plays an important role in improving the photovoltaic conversion efficiency of the cell. Polishing the back of the silicon wafer can improve the flatness of the back, reduce light reflection, increase light transmission and absorption, and thus increase Isc; back polishing can improve the back contact performance of the cell and reduce carrier recombination, thereby increasing open circuit voltage and fill factor; in addition, back polishing also improves the contact between the back of the silicon wafer and the aluminum paste, enhances the passivation effect, and reduces back recombination, thereby improving the overall performance and efficiency of the cell.
[0003] At present, the commonly used back polishing methods are mainly acid polishing and alkaline polishing:
[0004] Acid polishing usually uses strong acidic substances such as hydrofluoric acid, nitric acid, and sulfuric acid as polishing agents to corrode silicon wafers. It can effectively remove the oxide layer and impurities on the surface of the silicon wafer and improve the cleanliness of the surface. However, the surface reflectivity of the acid-polished silicon wafer is low. In addition, since acid polishing uses a large amount of acidic substances, the cost of the chemical solution and the waste liquid treatment cost are very high.
[0005] Alkali polishing can remove pits and defects on the silicon surface, generating a smooth surface with lower roughness, which is very important for improving the photoelectric conversion efficiency of solar cells. However, alkali polishing often has the following problems: 1) Incomplete alkali polishing will leave pyramids; 2) The tower base formed by alkali polishing has a single structure, mostly square independent tower bases, poor flatness and low reflectivity; 3) The tower base formed by alkali polishing is small.
[0006] The purpose of the present invention is to provide a single crystal silicon alkali polishing additive for preparing a fused tower base and a method of using the same, so as to replace the acid polishing process, reduce environmental pollution, and solve the problems of single tower base shape, poor flatness, low reflectivity, and small tower base during the alkali polishing process. Summary of the invention
[0007] In order to solve the deficiencies in the prior art, the present invention provides a method for preparing a fused tower base single crystal silicon alkali polishing additive and using the same.
[0008] To solve the above technical problems, the purpose of the present invention is achieved as follows:
[0009] The monocrystalline silicon alkali polishing additive for preparing a fused tower base of the present invention is composed of the following raw materials in percentage: 0.1% to 3.0% accelerator, 0.05% to 1.0% defoamer, 0.1% to 3.0% corrosion inhibitor, 0.05% to 0.5% surfactant, and the balance is deionized water.
[0010] On the basis of the above scheme and as a preferred scheme of the above scheme: the accelerator is one or a combination of two or more of hydrogen peroxide, sodium percarbonate, peracetic acid, persulfate, crown ether. The accelerator can accelerate the reaction rate of alkali and silicon.
[0011] On the basis of the above scheme and as a preferred scheme of the above scheme: the degassing agent is one or a combination of two or more of polyvinyl pyrrolidone, polyvinyl alcohol, glucose and starch. The degassing agent can be adsorbed on the surface of the single crystal silicon wafer, reduce the interfacial tension, accelerate the desorption of hydrogen during the reaction, and is easy to clean without residue.
[0012] On the basis of the above scheme and as a preferred scheme of the above scheme: the corrosion inhibitor is one of benzoic acid, hydrolyzed polymaleic anhydride, sodium polyacrylate, and disodium ethylenediaminetetraacetate, or a combination of two or more thereof. The corrosion inhibitor contains a large number of hydrophilic groups such as hydroxyl and carbonyl groups, which can be adsorbed on the surface of silicon dioxide, greatly reducing the corrosion rate of silicon dioxide by alkali, increasing the reaction rate difference between silicon, silicon dioxide and alkali, so that the PN junction on the front of the battery is not destroyed during the alkali polishing process, and at the same time, the back of the battery also obtains a better polishing effect.
[0013] On the basis of the above scheme and as a preferred scheme of the above scheme: the surfactant is one or a combination of two or more of sodium dodecyl sulfate, alkyl glycoside, sodium dodecylbenzene sulfonate, and dimethyl sulfoxide. The hydrophobic group of the surfactant combines with and covers the dirt in the solution, and the hydrophilic group flows with the water, separating the dirt from the surface of the silicon wafer through emulsification and wetting, having the ability to suspend and disperse solid dirt particles, and having good cleaning ability for the silicon wafer.
[0014] The present invention also relates to a method for using a single crystal silicon alkali polishing additive for preparing a fused tower base, comprising the following steps:
[0015] S1. Preparation of additives: adding 0.1% to 3.0% of accelerator, 0.05% to 1% of defoaming agent, 0.1% to 2.0% of corrosion inhibitor, and 0.05% to 0.5% of surfactant in a mass percentage content into deionized water, and mixing well to prepare additives;
[0016] S2, preparing a polishing liquid: adding the additive prepared in step S1 to the alkali solution, and mixing them evenly to prepare a polishing liquid;
[0017] S3, polishing the back side of the silicon wafer using the polishing liquid prepared in step S2.
[0018] On the basis of the above scheme and as a preferred scheme of the above scheme: the mass ratio of the additive to the alkali solution is 5 to 15:100.
[0019] On the basis of the above scheme and as a preferred scheme of the above scheme: the alkali solution is a NaOH solution or a KOH solution, and the mass concentration of the alkali solution is 45%.
[0020] On the basis of the above scheme and as a preferred scheme of the above scheme: the temperature of the polishing treatment is controlled at 55-75° C., and the time is controlled at 120s-240s.
[0021] The invention has the beneficial effects that the monocrystalline silicon alkali polishing additive for preparing a fused tower base and the use method thereof involved in the invention replaces the acid polishing process by the alkali polishing process with the additive, reduces environmental pollution, and solves the problem of single tower base morphology and poor flatness during the alkali polishing process. The additive of the invention can prepare a fused tower base during the alkali polishing process, improve the flatness and reflectivity of the back of the silicon wafer, and protect the PN junction on the front of the silicon wafer from being damaged. It has better absorption and conversion of light inside the silicon wafer, thereby obtaining high current. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the back surface morphology after polishing in Example 1;
[0023] Figure 2 This is the back surface morphology after polishing in Example 1;
[0024] Figure 3 This is the back surface morphology after polishing in Example 2;
[0025] Figure 4 This is the back surface morphology after polishing in Example 2; DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0027] Example 1
[0028] The formula of the single crystal silicon alkali polishing additive for preparing the fused tower base involved in this embodiment is: composed of the following percentages of raw materials: 1.0% accelerator, 1.0% defoaming agent, 0.1% corrosion inhibitor, 0.5% surfactant, and the balance is deionized water.
[0029] The accelerator is prepared by mixing hydrogen peroxide, sodium percarbonate and peracetic acid in a weight ratio of 1:1:1. The defoaming agent is polyvinyl pyrrolidone. The corrosion inhibitor is prepared by mixing hydrolyzed polymaleic anhydride and sodium polyacrylate in a weight ratio of 1:1. The surfactant is sodium dodecyl sulfate.
[0030] The method of using the single crystal silicon alkali polishing additive for preparing a fused tower base involved in this embodiment is as follows: take a 3L alkali polishing tank, add 2L water, increase the temperature to 62°C, and then add 30g of NaOH, and after the temperature stabilizes, add 16g of the additive involved in this embodiment; after stirring evenly, remove the N-type silicon wafer of BSG, and pre-clean it in a 50°C NaOH and hydrogen peroxide tank for 30s. After the pre-cleaning is completed, put it in a water tank for cleaning for 1min, and then put the silicon wafer into the alkali polishing tank for polishing for 180s. After polishing is completed, put it in the water tank for cleaning for 1min, and the alkali polishing etching process is completed.
[0031] Comparative Example 1
[0032] Take a 3L alkaline polishing tank, add 2L water, raise the temperature to 62°C, then add 30g NaOH, and after the temperature stabilizes, add 16g of the alkaline polishing additive PS35 currently sold on the market; after stirring evenly, take out the N-type silicon wafer of BSG, pre-clean it in a 50°C NaOH and hydrogen peroxide tank for 30s, after the pre-cleaning is completed, put it in a water tank for cleaning for 1min, then put the silicon wafer into the alkaline polishing tank for polishing for 180s, and after polishing, put it in the water tank for cleaning for 1min, and the alkaline polishing etching process is completed.
[0033] Embodiment 2
[0034] The single crystal silicon alkali polishing additive for preparing a fused tower base involved in this embodiment is composed of the following percentages of raw materials: 3.0% accelerator, 0.05% defoaming agent, 3.0% corrosion inhibitor, 0.05% surfactant, and the balance is deionized water.
[0035] The accelerator is a crown ether. The defoaming agent is a compound of polyvinyl pyrrolidone, polyvinyl alcohol and glucose in a weight ratio of 1:1:1. The corrosion inhibitor is disodium ethylenediaminetetraacetic acid. The surfactant is an alkyl glycoside, sodium dodecylbenzene sulfonate and dimethyl sulfoxide in a weight ratio of 1:1:1.
[0036] The method of using the single crystal silicon alkali polishing additive for preparing a fused tower base involved in this embodiment is as follows: take a 3L alkali polishing tank, add 2L water, increase the temperature to 60°C, and then add 30g of NaOH, and after the temperature stabilizes, add 16g of the additive involved in this embodiment; after stirring evenly, remove the N-type silicon wafer of BSG, and pre-clean it in a 50°C NaOH and hydrogen peroxide tank for 30s. After the pre-cleaning is completed, put it in a water tank for cleaning for 1min, and then put the silicon wafer into the alkali polishing tank for polishing for 180s. After polishing is completed, put it in the water tank for cleaning for 1min, and the alkali polishing etching process is completed.
[0037] Comparative Example 2
[0038] Take a 3L alkaline polishing tank, add 2L water, raise the temperature to 60°C, then add 30g NaOH, and after the temperature stabilizes, add 16g of the alkaline polishing additive PS35 currently sold on the market; after stirring evenly, take out the N-type silicon wafer of BSG, pre-clean it in a 50°C NaOH and hydrogen peroxide tank for 30s, after the pre-cleaning is completed, put it in a water tank for cleaning for 1min, then put the silicon wafer into the alkaline polishing tank for polishing for 180s, and after polishing, put it in the water tank for cleaning for 1min, and the alkaline polishing etching process is completed.
[0039] The weight loss and reflectivity data of the alkali polishing process of Example 1 and Example 2 and Comparative Examples 1 and 2 are shown in Table 1. It can be seen from Table 1 that the weight loss of Example 1 is comparable to the alkali polishing additives sold on the market, but the size of the back tower base is larger and the reflectivity is also increased. The high back reflectivity means better absorption and conversion of light inside the silicon wafer, thereby obtaining high current. Figure 1 and Figure 2 It can be seen that the tower base morphology of the silicon wafer polished with the additive of the present invention is fused, and according to the Sq data, it can be concluded that the flatness of the silicon wafer polished with the additive of the present invention is significantly better than that of the silicon wafer polished with the alkali polishing additive PS35 sold on the market. Comparing Example 1 and Example 2, it can be seen that even at low temperature and small weight loss, a relatively flat tower base morphology with a relatively large tower base can still be formed.
[0040] Table 1 Test data after treatment of Examples 1, 2 and Comparative Examples 1, 2
[0041] Group Weight loss (g) Reflectivity(%) Tower base(μm) Sq Example 1 0.22 46.9 9-10 0.28 Comparative Example 1 0.21 46.4 7-8 0.31 Example 2 0.19 47.1 8-9 0.29 Comparative Example 2 0.18 46.3 7-8 0.32
[0042] Example 3
[0043] The single crystal silicon alkali polishing additive for preparing a fused tower base involved in this embodiment is composed of the following percentages of raw materials: 1% accelerator, 0.5% defoaming agent, 1% corrosion inhibitor, 0.2% surfactant, and the balance is deionized water.
[0044] The accelerator is persulfate. The defoaming agent is polyvinyl alcohol, glucose and starch mixed in a weight ratio of 1:1:1. The corrosion inhibitor is hydrolyzed polymaleic anhydride. The surfactant is sodium dodecylbenzene sulfonate and dimethyl sulfoxide mixed in a weight ratio of 1:1.
[0045] Take 350L of alkaline polishing tank, add 335L of water, raise the temperature to 62°C, then add 10L of 45% NaOH, and after the temperature stabilizes, add 2L of the additive involved in this embodiment; after stirring evenly, polish 1600 N-type silicon wafers with BSG removed, pre-clean in a tank of 50°C NaOH and hydrogen peroxide for 40s, then put them in a water tank for cleaning for 100s, and then put the silicon wafers into the alkaline polishing tank for polishing for 3min. After polishing, put them in a water tank for cleaning for 100s, and the alkaline polishing etching process is completed; then enter the subsequent solar cell preparation process to obtain finished solar cells.
[0046] Comparative Example 3
[0047] Take a 350L alkaline polishing tank, add 335L water, raise the temperature to 62°C, then add 10L of 45% NaOH, and after the temperature stabilizes, add 2L of the alkaline polishing additive PS35 currently sold on the market; after uniform circulation, polish 1600 BSG-removed N-type silicon wafers, pre-clean them in a 50°C NaOH and hydrogen peroxide tank for 40s, then put them in a water tank for cleaning for 100s, and then put the silicon wafers into the alkaline polishing tank for polishing for 3min. After polishing, put them in a water tank for cleaning for 100s, and the alkaline polishing etching process is completed; then enter the subsequent solar cell preparation process to obtain finished solar cells.
[0048] Example 4
[0049] The single crystal silicon alkali polishing additive for preparing a fused tower base involved in this embodiment is composed of the following percentages of raw materials: 3.0% accelerator, 0.2% defoaming agent, 0.5% corrosion inhibitor, 0.1% surfactant, and the balance is deionized water.
[0050] The accelerator is a compound of persulfate and crown ether in a weight ratio of 1:2. The defoamer is a compound of polyvinyl pyrrolidone and polyvinyl alcohol in a weight ratio of 1:2. The corrosion inhibitor is sodium polyacrylate. The surfactant is a compound of sodium dodecylbenzene sulfonate and dimethyl sulfoxide in a weight ratio of 1:1.
[0051] Take 350L of alkaline polishing tank, add 335L of water, raise the temperature to 60°C, then add 10L of 45% NaOH, and after the temperature stabilizes, add 2L of the additive involved in this embodiment, stir evenly, polish 1600 N-type silicon wafers with BSG removed, pre-clean in a 50°C NaOH and hydrogen peroxide tank for 40s, then put them in a water tank for cleaning for 100s, then put the silicon wafers into the alkaline polishing tank for polishing for 3min, and after polishing, put them in a water tank for cleaning for 100s, and the alkaline polishing etching process is completed; then enter the subsequent solar cell preparation process to obtain finished solar cells.
[0052] Comparative Example 4
[0053] Take a 350L alkaline polishing tank, add 335L water, raise the temperature to 60℃, then add 10L of 45% NaOH, and after the temperature stabilizes, add 2L of the alkaline polishing additive PS35 currently sold on the market; after uniform circulation, polish 1600 BSG-removed N-type silicon wafers, pre-clean them in a 50℃ NaOH and hydrogen peroxide tank for 40s, then put them in a water tank for cleaning for 100s, then put the silicon wafers into the alkaline polishing tank for polishing for 3min, and after polishing, put them in a water tank for cleaning for 100s, and the alkaline polishing etching process is completed; then enter the subsequent solar cell preparation process to obtain finished solar cells.
[0054] The performance data of the finished battery cells obtained by Example 3 and Example 4 and Comparative Example 3 and Comparative Example 4 are shown in Table 2. It can be seen from Table 2 that the average efficiency of the battery with the additive of the present invention is 26.329%, and the average efficiency of the battery with the additive sold on the market is 26.257%. In comparison, the average efficiency of the battery with the additive of the present invention is increased by 0.071%, which improves the conversion efficiency of the battery to a certain extent. By comparing Example 3 and Example 4, it can be seen that even under low temperature conditions, the conversion efficiency of the battery can still be improved to a certain extent.
[0055] Table 2 Test data of the cells prepared in Examples 3, 4 and Comparative Examples 3, 4
[0056] Group ETA VOC ISC FF Example 3 26.329 0.729 13.950 86.697 Comparative Example 3 26.257 0.728 13.949 86.525 Example 4 26.333 0.725 13.955 86.706 Comparative Example 4 26.260 0.720 13.951 86.530
[0057] The alkaline polishing additive uses sodium hydroxide or potassium hydroxide as a polishing agent. Compared with acid polishing, the chemicals used have less impact on the environment and are easier to neutralize and treat, reducing environmental pollution. The equipment and safety measures required during the treatment process may be less expensive, thereby reducing the overall treatment cost.
[0058] The alkali polishing additive can be used to prepare a back tower base with a fusion-like structure. Compared with the square tower bases prepared by most commercially available alkali polishing additives, it has higher flatness and reflectivity, better absorption and conversion of light inside the silicon wafer, thereby obtaining high current.
[0059] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A single crystal silicon alkali polishing additive for preparing a fused tower base, characterized in that: The invention is composed of the following raw materials in the following percentages: 0.1% to 3.0% of accelerator, 0.05% to 1.0% of defoaming agent, 0.1% to 3.0% of corrosion inhibitor, 0.05% to 0.5% of surfactant, and the balance is deionized water.
2. The single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 1, characterized in that: The accelerator is one or a combination of two or more of hydrogen peroxide, sodium percarbonate, peracetic acid, persulfate, and crown ether.
3. The single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 1, characterized in that: The defoaming agent is one or a combination of two or more of polyvinyl pyrrolidone, polyvinyl alcohol, glucose and starch.
4. The single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 1, characterized in that: The corrosion inhibitor is one of benzoic acid, hydrolyzed polymaleic anhydride, sodium polyacrylate, and disodium ethylenediaminetetraacetate, or a combination of two or more thereof.
5. The single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 1, characterized in that: The surfactant is one of sodium dodecyl sulfate, alkyl glycoside, sodium dodecylbenzene sulfonate, and dimethyl sulfoxide, or a combination of two or more thereof.
6. A method for using a single crystal silicon alkali polishing additive for preparing a fused tower base, characterized in that: The following steps are involved: S1. Preparation of additives: adding 0.1% to 3.0% of accelerator, 0.05% to 1% of defoaming agent, 0.1% to 2.0% of corrosion inhibitor, and 0.05% to 0.5% of surfactant in a mass percentage content into deionized water, and mixing well to prepare additives; S2, preparing a polishing liquid: adding the additive prepared in step S1 to the alkali solution, and mixing them evenly to prepare a polishing liquid; S3, polishing the back side of the silicon wafer using the polishing liquid prepared in step S2.
7. The method for using the single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 6, characterized in that: The mass ratio of the additive to the alkali solution is 5 to 15:
100.
8. The method for using the single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 6, characterized in that: The alkali solution is a NaOH solution or a KOH solution, and the mass concentration of the alkali solution is 45%.
9. The method for using the single crystal silicon alkali polishing additive for preparing a fused tower base according to claim 6, characterized in that: The temperature of the polishing process is controlled at 55-75° C., and the time is controlled at 120s-240s.
Citation Information
Cited By
Silicon wafer back contact cell grooving additive and preparation method and use method thereof
CN120018620A
An additive for grooving back contact cells on crystalline silicon wafers, its preparation method and application method