Automobile flexible shaft zipper lubricating grease and preparation method thereof
Through the combination of lithium stearate soap and composite barium thickener and multi-effect antioxidant, the problems of the short service life of existing greases and insufficient shear resistance under high and low temperature conditions are solved, and lubrication is achieved The grease has significantly improved high temperature resistance, shear resistance and oxidation resistance, and is suitable for automotive soft shaft zipper grease for lifelong use.
Patent Information
- Application Number
- CN202411096652.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing automotive soft shaft zipper grease has a short service life under high and low temperature conditions, has failed to discolor at high temperatures, and has insufficient shear resistance, making it difficult to meet the requirements of lifelong use.
The combination of lithium stearate soap and composite barium thickener was combined with one-step multi-effect antioxidant in situ synthesis to prepare greases with excellent high temperature resistance, shear resistance and oxidation resistance.
It significantly improves the high temperature resistance and shear resistance of grease, enhances the anti-oxidation performance and extreme pressure and wear resistance, extends the service life, and is suitable for applications in harsh working conditions.
Smart Images

Figure BDA0004988122550000031 
Figure BDA0004988122550000041 
Figure BDA0004988122550000042
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lubricating grease, and in particular relates to a lubricating grease for a flexible shaft zipper of an automobile and a preparation method thereof. Background Art
[0002] The automatic shift cables, manual shift cables, parking brake cables, etc. on the car all transmit force and displacement through a combination of steel wire ropes and casings to achieve car acceleration, deceleration or reversing. Their performance is very important for driving safety. In order to achieve efficient transmission of various cable forces and displacements and reduce durable wear, it is necessary to use grease between the car shifter lever and other connectors. Grease needs to be applied to the steel wire rope of the cable product. At present, the grease used in the market can reduce the friction between the car shifter lever and other components, but because it needs to operate under extremely low (-40℃) and extremely high temperature (140℃) conditions during use, the grease is prone to high temperature discoloration and failure, and the service life is short.
[0003] In the prior art, there are various types of greases for wire ropes, mainly soap-based or composite soap-based greases with mineral oil or synthetic hydrocarbon as the base oil. Patent CN202010566391.9 synthesizes a cable grease, which is prepared by adding barium soap thickener and other additives to the synthetic hydrocarbon base oil. The wire ropes coated with the grease in this patent are mainly used in ports. The grease has the advantages of outstanding adhesion, hydrophobicity, rust resistance and wear resistance, but its high and low temperature use effect is not reflected. Patent 202311778604.4 provides a grease for automotive cables and a preparation method thereof. It is a grease specially used for friction pairs such as steel wire ropes and inner-lined plastic pipes of automotive cable products. The grease has the characteristics of high dropping point, low oil separation rate, and good colloid stability. It has good lubricity at high temperature, normal temperature, and low temperature, and has excellent anti-wear performance, but its service life and shear resistance are not reflected.
[0004] Therefore, it is of great significance to develop an automotive flexible shaft cable grease with good high and low temperature performance, no discoloration at high temperature, no softening and loss, and excellent shear resistance and lifelong service life. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and provide an automobile flexible shaft zipper lubricating grease and a preparation method thereof.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] A method for preparing automotive flexible shaft zipper grease comprises the following steps:
[0008] A1. Add 2 / 3 of base oil into the reactor and heat to 50-60℃;
[0009] A2. Add thickener to the reactor, heat and refine to 200-210°C, keep warm for 5 minutes, add the remaining base oil and cool rapidly;
[0010] A3. When the temperature in the reactor drops to 80-100°C, add anti-wear agent, rust inhibitor and multi-effect antioxidant, and adjust the cone penetration. After keeping warm for 2-4 hours, grind 2-3 times to obtain automotive flexible shaft zipper grease.
[0011] Furthermore, the raw materials are calculated in parts by weight as follows: 700-850 parts of base oil, 100-150 parts of thickener, 50-150 parts of anti-wear agent, 1-5 parts of rust inhibitor, and 20-80 parts of multi-effect antioxidant.
[0012] Furthermore, the base oil has a viscosity of 500-1500 mm at 40°C. 2 / s.
[0013] Furthermore, the anti-wear agent is one or both of polytetrafluoroethylene and melamine cyanurate.
[0014] Furthermore, the rust inhibitor is one or both of sulfonate and benzotriazole.
[0015] Furthermore, the thickener is prepared by the following steps:
[0016] B1. Add stearic acid to the reaction kettle, heat to 60-80°C, and stir to dissolve. Mix lithium hydroxide with water, add to the reaction kettle, and keep the temperature at 80-90°C for 0.5-1h.
[0017] B2. Add stearic acid and sebacic acid to the reactor of step B1, heat to 80-90°C, stir to dissolve, mix barium hydroxide octahydrate with water, add to the reactor, control the system temperature to 90-100°C for saponification for 1-2h, and after the saponification is completed, gradually heat to 120-140°C for dehydration to obtain a thickener.
[0018] Furthermore, the raw materials in step B1 are calculated in parts by weight as follows: 40-60 parts of stearic acid, 8-15 parts of lithium hydroxide, and 25-45 parts of water.
[0019] Furthermore, the raw materials in step B2 are calculated in parts by weight as follows: 10-15 parts of stearic acid, 5-10 parts of sebacic acid, 15-20 parts of barium hydroxide octahydrate, and 30-40 parts of water.
[0020] The prepared thickener is a compound of a lithium stearate soap thickener and a complex barium thickener, which has a good thickening effect on the grease and can complement the performance, greatly improving the high temperature resistance and shear resistance of the grease.
[0021] Furthermore, the multi-effect antioxidant is prepared by the following steps:
[0022] S1. Dissolve phenothiazine and potassium tert-butoxide in tetrahydrofuran, stir at 0°C for 30 min, then add iodine to the reaction system, keep warm and stir for 12 h, quench the reaction with deionized water, extract with dichloromethane, wash with deionized water, dry with anhydrous sodium sulfate, and purify by column chromatography (the eluent is a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two is 20:1), remove the eluent by rotary evaporation to obtain intermediate 1; the ratio of phenothiazine, potassium tert-butoxide, tetrahydrofuran, iodine and deionized water is 19.9 g:14.2 g:100 mL:20.1 g:200 mL;
[0023] Phenothiazine reacts with ethyl iodide to obtain intermediate 1; the specific reaction is as follows:
[0024]
[0025] S2. In a 0°C ice-water bath and under nitrogen protection, slowly drip phosphorus oxychloride into N,N-dimethylformamide (DMF) in a three-necked flask equipped with a stirring device. After stirring for 30 minutes, add intermediate 1, control the reaction temperature to 65°C, stir and react for 8 hours. After the reaction is complete, cool to room temperature, pour into ice water, drip sodium hydroxide solution (mass fraction 12%) to adjust the pH value to 5, extract with chloroform 3-4 times, wash with deionized water 3-4 times, dry with anhydrous sodium sulfate, and rotary evaporate to obtain intermediate 2; the ratio of phosphorus oxychloride, N,N-dimethylformamide, intermediate 1, and ice water is 15mL:100mL:22.7g:100mL;
[0026] The specific reaction is as follows:
[0027]
[0028] S3. Under nitrogen protection, in a three-necked flask equipped with a stirring reflux device, the intermediate 2 and 4-aminophenol were mixed and stirred evenly with methanol, and stirred and refluxed at 65°C for 10 hours. After the reaction was completed, the mixture was allowed to stand for 12 hours, and solid was precipitated. The precipitated solid was washed with ice anhydrous methanol for 3-4 times, and vacuum dried at 60°C for 12 hours to obtain intermediate 3; the ratio of intermediate 2, 4-aminophenol and methanol was 22.5g:100mL:10.9g;
[0029] The amino group on 4-aminophenol condenses with the aldehyde group on the intermediate 2 to form an imine group (C=N Schiff base structure) to obtain the intermediate 3; the specific reaction is shown below:
[0030]
[0031] S4, in a three-necked flask equipped with a stirring device, the intermediate 3, phosphorus trichloride, triethylamine (catalyst) and toluene were mixed and stirred uniformly, the reaction temperature was controlled to 70°C, the reaction was kept warm for 6 hours, the reaction was completed, filtered, part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, the volume ratio of the two was 4:3), the eluent was removed by rotary evaporation to obtain intermediate 4; the ratio of the amount of intermediate 3, phosphorus trichloride, triethylamine and toluene was 34.6g:16.1g:15mL:100mL;
[0032] Under the catalysis of triethylamine, intermediate 3 reacts with phosphorus trichloride, and by controlling the molar ratio of the two to be close to 1:1 and a slight excess of phosphorus trichloride, only one chlorine group on the phosphorus trichloride participates in the reaction to obtain intermediate 4; the specific reaction process is as follows:
[0033]
[0034] S5. In a three-necked flask equipped with a stirring device, the intermediate 4, potassium carbonate and N,N-dimethylformamide were mixed, pentaerythritol was added, the temperature was controlled to 80°C, the reaction was stirred for 8 hours, and the reaction was completed. The solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain a multi-effect antioxidant; the ratio of the amount of intermediate 4, potassium carbonate, N,N-dimethylformamide and pentaerythritol was 89.2g:27.6g:150mL:14.5g;
[0035] Intermediate 4 reacts with pentaerythritol, and by controlling the molar ratio of the two to be close to 2:1, a multi-effect antioxidant is obtained. The specific reaction process is as follows:
[0036]
[0037] The prepared multi-effect antioxidant belongs to the phosphite antioxidant. As a kind of auxiliary antioxidant, it can decompose the hydroperoxide generated in the polymer due to oxidative aging and make it inactive, thereby achieving the purpose of terminating or delaying the oxidative degradation of the polymer. The thiophenazine structure contained in the multi-effect antioxidant is a thiocyanate-anthracene type antioxidant, which has a high efficiency antioxidant property for the grease, enhances the antioxidant property of the grease by capturing free radicals, inhibits the increase of viscosity, and plays a synergistic role with the phosphite, greatly enhancing the oxidation stability of the grease; in addition, the sulfur element contained in the multi-effect antioxidant molecule can react with the metal to form a sulfide film, thereby playing an anti-wear role. Moreover, when the working conditions are bad or extreme pressure conditions are entered, an inorganic sulfide protective film can be generated due to the rupture of the CS bond, which can give the grease a strong extreme pressure wear resistance, and can play a synergistic role with the two elements of phosphorus and nitrogen to further enhance the extreme pressure wear resistance of the grease.
[0038] Beneficial effects of the present invention:
[0039] 1. The lubricating grease prepared by the present invention has a thickener which is a compound of a lithium stearate soap thickener and a composite barium thickener, which can complement each other in performance and greatly improve the high temperature resistance and shear resistance of the lubricating grease;
[0040] 2. The present invention adopts a one-step in-situ synthesis process of a grease with a composite soap thickener system. Compared with a simple physical mixing process of two thickeners, the synthesized grease has a more stable structure and better shear resistance.
[0041] 3. The various groups in the prepared multi-effect antioxidant can play a synergistic role, significantly enhancing the antioxidant performance and extreme pressure and anti-wear performance of the grease;
[0042] Therefore, the lubricating grease prepared by the present invention has excellent high temperature resistance and shear resistance, as well as remarkable antioxidant performance and extreme pressure and anti-wear performance, and has important application value in the field of lubricating grease technology. DETAILED DESCRIPTION
[0043] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] Preparation of multi-effect antioxidant:
[0046] S1, 19.9g of phenothiazine and 14.2g of potassium tert-butoxide were dissolved in 100mL of tetrahydrofuran, stirred at 0°C for 30min, then 20.1g of iodoethane was added to the reaction system, the mixture was stirred and reacted for 12h, then the reaction was quenched with 200mL of deionized water, extracted with dichloromethane, washed with deionized water, dried over anhydrous sodium sulfate, and purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two was 20:1), and the eluent was removed by rotary evaporation to obtain intermediate 1;
[0047] S2. In a 0°C ice-water bath and under nitrogen protection, slowly drip 15 mL of phosphorus oxychloride into 100 mL of N,N-dimethylformamide in a three-necked flask equipped with a stirring device. After stirring for 30 min, add 22.7 g of intermediate 1, control the reaction temperature to 65°C, stir and react for 8 h. After the reaction is complete, cool to room temperature, pour into 100 mL of ice water, drip sodium hydroxide solution (mass fraction 12%) to adjust the pH value to 5, extract with chloroform 3 times, wash with deionized water 3 times, dry over anhydrous sodium sulfate, and rotary evaporate to obtain intermediate 2;
[0048] S3. Under nitrogen protection, 22.5 g of intermediate 2, 100 mL of 4-aminophenol and 10.9 g of methanol were mixed and stirred evenly in a three-necked flask equipped with a stirring reflux device, and stirred and refluxed at 65°C for 10 h. After the reaction was completed, the mixture was allowed to stand for 12 h. Solid was precipitated. The precipitated solid was washed 4 times with ice anhydrous methanol and dried in vacuo at 60°C for 12 h to obtain intermediate 3.
[0049] S4, in a three-necked flask equipped with a stirring device, 34.6g of intermediate 3, 16.1g of phosphorus trichloride, 15mL of triethylamine and 100mL of toluene were mixed and stirred evenly, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6h. After the reaction was completed, it was filtered, and part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain intermediate 4;
[0050] S5. In a three-necked flask equipped with a stirring device, 89.2 g of intermediate 4, 27.6 g of potassium carbonate and 150 mL of N,N-dimethylformamide were mixed, 14.5 g of pentaerythritol was added, the temperature was controlled at 80°C, the reaction was stirred for 8 hours, and after the reaction was completed, the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 4:3), the eluent was removed by rotary evaporation to obtain a multi-effect antioxidant.
[0051] Example 2
[0052] Preparation of multi-effect antioxidant:
[0053] S1, 39.8g of phenothiazine and 28.4g of potassium tert-butoxide were dissolved in 200mL of tetrahydrofuran, stirred at 0°C for 30min, then 40.2g of iodoethane was added to the reaction system, the mixture was stirred and reacted for 12h, the reaction was quenched with 400mL of deionized water, and then extracted with dichloromethane, washed with deionized water, dried over anhydrous sodium sulfate, and purified by column chromatography (the eluent was a mixed solvent of petroleum ether / ethyl acetate, the volume ratio of the two was 20:1), and the eluent was removed by rotary evaporation to obtain intermediate 1;
[0054] S2. In a 0°C ice-water bath and under nitrogen protection, slowly drip 30 mL of phosphorus oxychloride into 200 mL of N,N-dimethylformamide in a three-necked flask equipped with a stirring device. After stirring for 30 min, add 45.4 g of intermediate 1, control the reaction temperature to 65°C, stir and react for 8 h. After the reaction is complete, cool to room temperature, pour into 200 mL of ice water, drip sodium hydroxide solution (mass fraction 12%) to adjust the pH value to 5, extract with chloroform 3 times, wash with deionized water 3 times, dry over anhydrous sodium sulfate, and rotary evaporate to obtain intermediate 2;
[0055] S3. Under nitrogen protection, 45 g of intermediate 2, 200 mL of 4-aminophenol and 21.8 g of methanol were mixed and stirred evenly in a three-necked flask equipped with a stirring reflux device, and stirred and refluxed at 65°C for 10 h. After the reaction was completed, the mixture was allowed to stand for 12 h. Solid was precipitated. The precipitated solid was washed 4 times with ice anhydrous methanol and dried in vacuo at 60°C for 12 h to obtain intermediate 3.
[0056] S4, in a three-necked flask equipped with a stirring device, 69.2g of intermediate 3, 32.2g of phosphorus trichloride, 30mL of triethylamine and 200mL of toluene were mixed and stirred uniformly, the reaction temperature was controlled to 70°C, and the reaction was kept warm for 6h. After the reaction was completed, it was filtered, and part of the solvent was removed by rotary evaporation, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate, and the volume ratio of the two was 4:3), and the eluent was removed by rotary evaporation to obtain intermediate 4;
[0057] S5. In a three-necked flask equipped with a stirring device, 178.4 g of intermediate 4, 55.2 g of potassium carbonate and 300 mL of N,N-dimethylformamide were mixed, 29 g of pentaerythritol was added, the temperature was controlled to 80°C, and the reaction was stirred for 8 hours. After the reaction was completed, the solvent was removed by distillation under reduced pressure, and then purified by column chromatography (the eluent was a mixed solvent of benzene / ethyl acetate in a volume ratio of 4:3), and the eluent was removed by rotary evaporation to obtain a multi-effect antioxidant.
[0058] Example 3
[0059] Preparation of thickener:
[0060] B1. Add 40g of stearic acid to the reactor, heat to 60°C, and stir to dissolve. Mix 8g of lithium hydroxide with 25g of water, add to the reactor, and keep the temperature at 80°C for 0.5h.
[0061] B2. Add 10 g of stearic acid and 5 g of sebacic acid to the reactor of step B1, heat to 80°C, stir to dissolve, mix 15 g of barium hydroxide octahydrate with 30 g of water, add to the reactor, control the system temperature to 90°C for saponification for 1 hour, and after the saponification is completed, gradually heat to 120°C for dehydration to obtain a thickener.
[0062] Example 4
[0063] Preparation of thickener:
[0064] B1. Add 60g of stearic acid to the reactor, heat to 80°C, and stir to dissolve. Mix 15g of lithium hydroxide with 45g of water, add to the reactor, and keep the temperature at 90°C for 1h.
[0065] B2. Add 15 g of stearic acid and 10 g of sebacic acid to the reactor of step B1, heat to 90°C, stir to dissolve, mix 20 g of barium hydroxide octahydrate with 40 g of water, add to the reactor, control the system temperature to 100°C for saponification for 2 hours, and after the saponification is completed, gradually heat to 140°C for dehydration to obtain a thickener.
[0066] Example 5
[0067] A1. Add 600g PAO100 base oil into the reactor and heat to 50°C;
[0068] A2. Add 100 g of the thickener prepared in Example 3 to the reactor, heat and refine to 200° C., keep warm for 5 min, add 200 g of base oil and quench;
[0069] A3. When the temperature in the reactor drops to 80°C, add 50g of polytetrafluoroethylene, 1g of sulfonate and 20g of the multi-effect antioxidant prepared in Example 1, and adjust the cone penetration. After keeping warm for 2h, grind twice to obtain automotive flexible shaft zipper grease.
[0070] Example 6
[0071] A1. Add 600g PAO100 base oil into the reactor and heat to 60°C;
[0072] A2. Add 150 g of the thickener prepared in Example 4 to the reactor, heat and refine to 210° C., keep warm for 5 min, add 200 g of base oil and quench;
[0073] A3. When the temperature in the reactor drops to 100° C., add 150 g of melamine cyanurate, 5 g of benzotriazole and 80 g of the multi-effect antioxidant prepared in Example 2, and adjust the cone penetration. After keeping warm for 4 hours, grind 3 times to obtain automotive flexible shaft zipper grease.
[0074] Comparative Example 1
[0075] The thickener is a single lithium soap, and the remaining steps are the same as those in Example 6. The specific preparation process is as follows:
[0076] A1. Add 600g of PAO100 base oil into the reactor and heat to 60°C;
[0077] A2. Add 85.2 g of stearic acid into the reaction kettle and dissolve it under heating and stirring at 80°C;
[0078] A3, dissolve 13.2g lithium hydroxide in 37.5g water, slowly add lithium hydroxide aqueous solution, keep the reaction at 90℃ for 1h;
[0079] A4, gradually raise the temperature to 120℃ for dehydration;
[0080] A5. Heat and refine to 210°C, keep warm for 5 minutes, add the remaining 200g base oil and cool rapidly;
[0081] A6. When the temperature in the reactor drops to 100°C, add 150g of melamine cyanurate, 5g of benzotriazole and 80g of the multi-effect antioxidant prepared in Example 2, and adjust the cone penetration to the appropriate value. Keep warm for 4h and grind 3 times to obtain grease.
[0082] Comparative Example 2
[0083] The thickener is a single complex barium soap, and the remaining steps are the same as those in Example 6. The specific preparation process is as follows:
[0084] A1. Add 600g of PAO100 base oil into a clean reactor and heat to 60°C;
[0085] A2, add 33.0g stearic acid and 18.9g sebacic acid into the reaction kettle and dissolve, and maintain the temperature at 90°C;
[0086] A3. Dissolve 51.3 g of barium hydroxide octahydrate in 150 g of water, add an aqueous solution of barium hydroxide octahydrate, and continue saponification at 90°C for 2 h;
[0087] A4, gradually raise the temperature to 120℃ for dehydration;
[0088] A5. Heat and refine to 210°C, keep warm for 5 minutes, add the remaining 200g base oil and cool rapidly;
[0089] A6. When the temperature in the reactor drops to 100°C, add 150g of melamine cyanurate, 5g of benzotriazole and 80g of the multi-effect antioxidant prepared in Example 2, and adjust the cone penetration. After keeping warm for 4h, grind 3 times to obtain grease.
[0090] Comparative Example 3
[0091] A two-step physical mixing process is adopted, and the specific process is as follows:
[0092] A1. Add 300g of PAO100 base oil into the clean reactor 1 and heat to 60°C;
[0093] A2, add 56.8g of stearic acid into reactor 1 and dissolve, heat and stir at 80℃ to dissolve;
[0094] A3, dissolve 8.82g lithium hydroxide in 25g water, slowly add lithium hydroxide aqueous solution, keep the reaction at 90℃ for 1h;
[0095] A4, gradually raise the temperature to 120℃ for dehydration;
[0096] A5, heat and refine to 210℃, keep warm for 5min, add the remaining 100g base oil and cool rapidly to obtain sample A;
[0097] A6. Add 300g of PAO100 base oil to the clean reactor 2 and heat to 60°C;
[0098] A7, add 11.0g stearic acid and 6.3g sebacic acid into reactor 2 and dissolve, and maintain the temperature at 90°C;
[0099] A8. Dissolve 17.1 g of barium hydroxide octahydrate in 40 g of water, add an aqueous solution of barium hydroxide octahydrate, and continue saponification at 90°C for 2 h.
[0100] A9, gradually raise the temperature to 120℃ for dehydration;
[0101] A10, heat and refine to 210°C, keep warm for 5 minutes, add the remaining 100g base oil and cool rapidly to obtain sample B;
[0102] A10, adding sample A to sample B for physical mixing;
[0103] A12. When the temperature in the reactor drops to 100°C, add 150g of melamine cyanurate, 5g of benzotriazole and 80g of the multi-effect antioxidant prepared in Example 2, and adjust the cone penetration. After keeping warm for 4h, grind 3 times to obtain grease.
[0104] Comparative Example 4
[0105] The multi-effect antioxidant in Example 6 was replaced by a commercially available ammonia antioxidant of equal quality, and the remaining steps were the same as in Example 6 to prepare a lubricating grease.
[0106] The following performance tests were performed on the greases of Examples 5-6 and Comparative Examples 1-4:
[0107] The national standard GB / T 269 "Cone penetration test method for lubricating greases and petroleum greases" is used to test the working cone penetration, extended working cone penetration, shear stability (difference between extended working cone penetration and working cone penetration) and high temperature cone penetration;
[0108] The dropping point is determined using the national standard GB / T 4929 "Determination of the dropping point of lubricating grease";
[0109] The national standard GB / T 7326 "Grease Copper Corrosion Test Method" is used to determine whether the copper corrosion is qualified;
[0110] The national standard GB / T 5018 "Test method for anti-corrosion of lubricating grease" is used to determine whether the anti-corrosion is qualified;
[0111] The wear spot diameter is measured using NB / SH / T 0189 "Determination of anti-wear properties of lubricating oils - four-ball method";
[0112] The wear spot diameter is measured using SH / T 0204 "Determination of anti-wear properties of lubricating grease";
[0113] The oxidation stability is determined by SH / T 0325 "Determination of oxidation stability of lubricating grease";
[0114] The measured results are shown in the following table:
[0115]
[0116] It can be seen from the above table that the grease prepared by the present invention has excellent high temperature resistance and shear resistance, as well as remarkable antioxidant performance and extreme pressure and anti-wear performance, and has important application value in the field of grease technology.
[0117] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0118] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A grease for automotive flexible shaft zipper, characterized in that: The invention comprises the following raw materials in parts by weight: 700-850 parts of base oil, 100-150 parts of thickener, 50-150 parts of anti-wear agent, 1-5 parts of rust inhibitor, and 20-80 parts of multi-effect antioxidant; Wherein, the thickener is prepared by the following steps: B1. Add stearic acid to the reaction kettle, heat to 60-80°C, and stir to dissolve. Mix lithium hydroxide with water, add to the reaction kettle, and keep the temperature at 80-90°C for 0.5-1h. B2. Add stearic acid and sebacic acid to the reactor of step B1, heat to 80-90°C, stir to dissolve, mix barium hydroxide octahydrate with water, add to the reactor, control the system temperature to 90-100°C for saponification for 1-2h, heat to 120-140°C for dehydration, and obtain a thickener.
2. The automotive flexible shaft zipper grease according to claim 1, characterized in that: The multi-effect antioxidant is prepared by the following steps: S1, dissolving phenothiazine and potassium tert-butoxide in tetrahydrofuran, stirring at 0°C for 30 min, adding iodoethane, stirring and reacting for 12 h, quenching the reaction with deionized water, extracting, washing, drying, purifying by column chromatography, and rotary evaporation to obtain intermediate 1; S2. In a 0°C ice-water bath and under nitrogen protection, slowly drip phosphorus oxychloride into N,N-dimethylformamide, stir for 30 minutes, add intermediate 1, and react at 65°C for 8 hours. After the reaction is complete, cool, pour into ice water, adjust the pH value to 5, extract, wash, and dry to obtain intermediate 2; S3. Under nitrogen protection, the intermediate 2 and 4-aminophenol were mixed with methanol and stirred evenly, and refluxed at 65°C for 10 hours. After the reaction was completed, the mixture was allowed to stand for 12 hours. A solid was precipitated, and the precipitated solid was washed and dried to obtain the intermediate 3. S4, mixing intermediate 3, phosphorus trichloride, triethylamine and toluene, stirring evenly, reacting at 70°C for 6 hours, filtering, rotary evaporating, column chromatography purification, and rotary evaporating to obtain intermediate 4; S5. Mix the intermediate 4, potassium carbonate and N,N-dimethylformamide, add pentaerythritol, react at 80°C for 8h, and after the reaction is completed, distill, purify by column chromatography, and rotary evaporate to obtain a multi-effect antioxidant.
3. The automotive flexible shaft zipper grease according to claim 2, characterized in that: In step S1, the ratio of phenothiazine, potassium tert-butoxide, tetrahydrofuran, ethyl iodide and deionized water is 19.9 g: 14.2 g: 100 mL: 20.1 g: 200 mL.
4. The automotive flexible shaft zipper grease according to claim 2, characterized in that: In step S2, the ratio of phosphorus oxychloride, N,N-dimethylformamide, intermediate 1, and ice water is 15 mL: 100 mL: 22.7 g: 100 mL.
5. The automotive flexible shaft zipper grease according to claim 2, characterized in that: In step S3, the ratio of the amount of the intermediate 2,4-aminophenol to methanol is 22.5 g:100 mL:10.9 g.
6. The automotive flexible shaft zipper grease according to claim 2, characterized in that: In step S4, the ratio of the amount of intermediate 3, phosphorus trichloride, triethylamine and toluene is 34.6 g:16.1 g:15 mL:100 mL.
7. The automotive flexible shaft zipper grease according to claim 2, characterized in that: In step S5, the ratio of the amount of intermediate 4, potassium carbonate, N,N-dimethylformamide and pentaerythritol used is 89.2 g:27.6 g:150 mL:14.5 g.
8. The automotive flexible shaft zipper grease according to claim 1, characterized in that: The raw materials in step B1 are calculated in parts by weight as follows: 40-60 parts of stearic acid, 8-15 parts of lithium hydroxide, and 25-45 parts of water.
9. The automotive flexible shaft zipper lubricating grease according to claim 1, characterized in that: The raw materials in step B2 are calculated in parts by weight as follows: 10-15 parts of stearic acid, 5-10 parts of sebacic acid, 15-20 parts of barium hydroxide octahydrate, and 30-40 parts of water.
10. The method for preparing a lubricating grease for automotive flexible shaft zipper according to claim 1, characterized in that: The following steps are involved: A1. Add 2 / 3 of base oil into the reactor and heat to 50-60℃; A2. Add thickener to the reactor, heat and refine to 200-210°C, keep warm for 5 minutes, add the remaining base oil and cool rapidly; A3. When the temperature in the reactor drops to 80-100°C, add anti-wear agent, rust inhibitor and multi-effect antioxidant, adjust the cone penetration, keep warm for 2-4 hours, and grind to obtain automotive flexible shaft zipper grease.