Brass wire and production method and application thereof

By optimizing the composition and production methods of brass wire, the impurities and tissue structure problems of copper needle surface in alkaline batteries are solved, the battery performance and life are improved, the preparation of high-quality brass wire is realized, and the risk of battery leakage is reduced.

CN118996199APending Publication Date: 2024-11-22JINTIAN COPPER GROUP CORP NINGBO
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411141383.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The surface impurities and tissue structure problems of copper needles in alkaline batteries lead to liquid leakage in the battery, affecting the battery performance and life. The existing brass wire cannot meet the needs of high surface quality and mechanical properties.

Method used

By optimizing the composition and production method of brass wire, the Cu content is controlled between 62.0 and 64.0 wt%, and the Fe, Ni and Pb impurities content are below 0.005 wt%, ensuring 94 to 100% of the alpha phase and 0 to 6% of the grain boundary. The β phase has an average grain size of ≤4μm, and high-quality brass wire is prepared by induction continuous annealing and improved tensile mold and coating technology.

Benefits of technology

It improves the mechanical properties and conductivity of brass wires, reduces the contact resistance and hydrogen evolution reaction of the current collector copper needle of the battery, extends the service life of the battery, and reduces the risk of liquid leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996199A_ABST
    Figure CN118996199A_ABST
Patent Text Reader

Abstract

The invention relates to a brass wire rod and a production method thereof. The brass wire rod comprises the following components: 62.0-64.0 wt% of Cu; fe < = 0.005 wt%; ni < = 0.005 wt%; less than or equal to 0.008 wt% of Pb; the balance is Zn and inevitable impurities, and the sum of the impurities does not exceed 0.1 wt%; the brass phase structure comprises 94-100% of a matrix alpha phase and 0-6% of a grain boundary beta phase; the average grain size of the brass is smaller than or equal to 4 micrometers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper and copper alloys, and in particular to a brass wire and a production method and application thereof. Background Art

[0002] Brass composed of copper and zinc is called ordinary brass. Ordinary brass has good electrical conductivity, thermal conductivity and mechanical properties. Because it is easy to process and has good plasticity, ordinary brass is widely used in the manufacture of various parts and components. When the zinc content is less than 35%, zinc can dissolve in copper to form a single phase α, called single-phase brass, which has good plasticity and is suitable for hot and cold press processing. When the zinc content is 36% to 46%, there is an α single phase and a β solid solution based on copper and zinc, called a two-phase brass. The β phase reduces the plasticity of brass and increases its tensile strength. Brass is a copper-zinc binary alloy, and its zinc content varies widely, so its room temperature structure is also very different.

[0003] Alkaline battery is a battery with potassium hydroxide or sodium hydroxide as electrolyte, zinc or aluminum as negative electrode, and manganese dioxide or silver oxide as positive electrode. It is the most common and widely used battery, and is widely used in many fields such as portable electronic devices.

[0004] The current collector is one of the most important parts inside the battery. The current collector of alkaline batteries is a copper needle. The negative zinc paste in alkaline batteries is connected to the negative electrode through the current collector copper needle. The surface state of the copper needle will inevitably affect the battery performance. Impurity elements such as Fe, Ni, Pb in the chemical composition of the copper needle and defects on the surface of the copper needle will increase the contact resistance between the copper needle and the zinc paste, accelerate the corrosion of the primary battery of the negative zinc paste, and the zinc paste will continuously self-discharge to produce hydrogen evolution reaction, which will affect the storage performance of the battery on the one hand, and more importantly, hydrogen will accumulate inside the battery, eventually opening the explosion-proof groove to cause battery leakage. The leaked liquid will corrode the components, copper foil and solder joints on the electrical circuit board, causing the electrical appliance to be scrapped, resulting in losses much higher than the value of the battery itself. The problem of alkaline battery leakage is a technical problem in the industry and has always troubled manufacturers.

[0005] The current collector copper needle requires stable material quality, smooth surface, good verticality, uniform coating, good bonding strength and density. If the copper needle has excessive impurities such as Fe, Ni, Pb, or surface defects that affect the quality of the copper needle surface electroplating layer, it will cause battery leakage and reduce battery life.

[0006] The copper needle is made of ordinary brass. Therefore, in addition to high requirements on the chemical composition and mechanical properties of the brass wire, the production of the current collector copper needle also has extremely high requirements on the surface quality of the wire. If there are defects such as silk flow, peeling, pits, scratches, etc. on the surface of the wire, it will affect the quality of the electroplating layer on the surface of the copper needle. It is worth noting that the internal organizational structure of the copper needle also affects the quality of the coating, which is often overlooked.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The first object of the present invention is to provide a brass wire to address one of the deficiencies of the current technology, so as to meet the demand for high surface quality brass wire for copper needles used in alkaline battery current collectors and reduce leakage of alkaline batteries.

[0009] A second object of the present invention is to provide a method for producing a brass wire.

[0010] The present invention is achieved through the following technical scheme: a brass wire, wherein the components of the brass include: Cu: 62.0-64.0wt%; Fe≤0.005wt%; Ni≤0.005wt%; Pb≤0.008wt%; the remainder is Zn and unavoidable impurities, and the total impurities do not exceed 0.1wt%; the brass phase structure includes 94-100% of matrix α phase and 0-6% of grain boundary β phase; the average grain size of the brass is ≤4μm.

[0011] Through the above technical scheme, the copper content in the brass wire is optimized, and the impurity content is strictly controlled. In the optimized production method, a brass structure containing a matrix α phase and a small amount of grain boundary β phase is obtained, and the brass grains are refined to less than 4μm. The material component quality is stable, the impurity elements are few, and the grains are fine, so that the surface quality of the wire is high and the mechanical properties are good. Finally, the surface electroplating layer of the battery collector copper needle is high in quality, the contact resistance between the copper needle and the zinc paste is reduced, and the primary battery corrosion and hydrogen evolution reaction of the zinc paste are reduced, thereby reducing the possibility of battery leakage and increasing the service life of the alkaline battery.

[0012] Furthermore, the brass wire has a tensile strength of 550-680 MPa, an elongation of 3-12%, and a conductivity of ≥24% IACS. Good mechanical properties and conductivity are the basis for ensuring the application of brass wire as a battery current collector.

[0013] Preferably, the average grain size of the brass is 1 to 4 μm.

[0014] Furthermore, under a 50x microscope, the brass wire has a defect size of less than 10 μm, a defect depth of less than 0.6 μm, and a total number of defects of no more than 2 / cm 2 Strict control of the surface quality of the brass wire ensures the quality of the surface coating of the copper needle as the current collector, reduces the contact resistance between the copper needle and the zinc paste, reduces the primary battery corrosion and hydrogen evolution reaction of the zinc paste, and thus reduces the possibility of battery leakage.

[0015] Furthermore, the brass component also includes Sn: 0.001-0.05wt%; the Sn element is added to replace the Zn element. Adding a trace amount of Sn element to the copper wire can improve the stability of battery performance.

[0016] Furthermore, the brass component also includes In: 0-0.05wt%; the In element is added to replace the Zn element. The hydrogen evolution potential of In is higher than that of Sn, and the battery containing In has stable electrical performance, and the In element and the Sn element in the copper needle work synergistically to further improve the stability of the battery's electrical performance.

[0017] The invention provides a method for producing a brass wire, which specifically comprises the following steps: smelting→upward continuous casting→stretching→annealing→long-drawing continuous annealing→medium-drawing continuous annealing→inspection and packaging, wherein the annealing is step annealing, the annealing temperature of the first stage is 460-520° C., and the holding time is 30-90 min; the annealing temperature of the second stage is 530-590° C., and the holding time is 120-240 min.

[0018] Through the above technical scheme, the raw materials are alloyed through smelting, degassing and slag removal, and the molten copper is transformed into wire through continuous casting and stretching. Gradually stretching and annealing change the shape and size of the material while optimizing the organization and performance of the material, and also improving the surface quality of the wire. Finally, it meets the requirements after passing the inspection.

[0019] Furthermore, the raw materials used for smelting are electrolytic copper, zinc ingots, tin ingots and Cu-In master alloys, where the Fe, Ni and Pb contents of electrolytic copper and zinc ingots must be below 0.003%, and iron tools cannot be used for smelting and stirring. The purity of the raw materials is strictly controlled to reduce the introduction of impurities.

[0020] Preferably, 0.005-0.03wt% of Cu-Zr master alloy is added to each ton of molten copper. Cu-Zr master alloy is added as a modifier to improve the casting structure of the alloy, refine the grains, and improve the plastic processing performance of the ingot.

[0021] Furthermore, the casting temperature of the upward continuous casting is 1030-1060°C, the pulling speed is 0.8-2.0 m / min, and the pulling pitch is 2-8 mm;

[0022] Preferably, the wire is peeled directly after stretching. The peeling process is to prevent defects such as thread flow, bamboo knot pattern, and cracked skin from appearing on the wire surface.

[0023] Preferably, the long-drawing and medium-drawing continuous annealing are both performed by induction continuous annealing;

[0024] Preferably, the stretching speed in the continuous annealing is 1-5 m / s, the annealing voltage is 20-100 V, the annealing coefficient is 5-12, the cooling water temperature is 30-45° C., and the emulsion concentration is 3-8%.

[0025] Preferably, the stretching speed in the middle drawing and annealing is 2-12 m / s, the annealing voltage is 0-130 V, the annealing current is 80-350 A, the cooling water temperature is 30-40 ° C, the emulsion concentration is 7-12%, the last two stretching dies are South African natural diamond dies, the stretching working cone angle is 14-22°, the length of the stretching sizing belt is 0.3-0.7 of the die aperture, and the stretching outlet cone angle is 40-60°;

[0026] More preferably, copper wire jitter absorbers are installed at the ceramic nozzle outlets of the drawing die, induction annealing and cooling section pipelines;

[0027] Preferably, all the tower wheels and wire-passing wheels in contact with the copper wire are sprayed with zirconium oxide coating, and the coating density is ≥6.2g / cm 3 , hardness HRA needs to reach 85-90;

[0028] More preferably, the zirconium oxide coating comprises 90-96wt% zirconium oxide and 4-10wt% Y2O3, wherein the zirconium oxide is composed of 80-90% c-ZrO2 with an area percentage of 2-6%, m-ZrO2 with an area percentage of 8-14%, and t-ZrO2 with an area percentage of 8-14%.

[0029] The brass wire obtained by the present invention is particularly suitable for preparing battery current collector copper needles.

[0030] The beneficial effects of the present invention are as follows: through the design and optimization of brass components and the optimization of production methods, the proportion of α phase and the degree of grain refinement in the brass microstructure are strictly controlled, so that the obtained brass wire has good mechanical properties and processing properties, stable electrical properties and high surface quality. In the production method of brass wire, the problem of electric shock caused by traditional contact annealing is avoided by electromagnetic induction continuous annealing, the wire flow problem is solved by improving the material and parameters of the stretching die, and the problem of scratches caused by the shaking of the copper wire is avoided by utilizing the energy absorption effect of the copper wire jitter absorber (specifically soft material) under pressure, and the chemical composition, phase ratio, density and hardness of the surface coating of the intermediate drawing continuous withdrawal tower wheel and the wire passing wheel are regulated, so as to improve the wear resistance of the coating and reduce the scratch defects of the brass wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0032] Figure 1 This is a metallographic structure photo of the finished product of Example 1 of the present invention;

[0033] Figure 2 This is a metallographic structure photo of the finished product of Comparative Example 1 of the present invention;

[0034] Figure 3 This is a surface photograph of the finished product of Example 1 of the present invention magnified 50 times;

[0035] Figure 4 This is a surface photograph of the finished product of Comparative Example 1 of the present invention magnified 50 times. DETAILED DESCRIPTION

[0036] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. Unless the context otherwise clearly indicates the opposite, the singular form used herein is also intended to include the plural form. It should also be understood that the term "comprising" does not specifically refer to a certain characteristic, field, integer, step, action, element and / or component, but excludes the existence or addition of other characteristics, fields, integers, steps, actions, elements, components and / or groups.

[0037] If a part is described as being "on" another part, it may be directly on the other part or there may be other parts therebetween. When a part is described as being "directly on" another part, there may be no other parts therebetween.

[0038] Although not otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art. Terms with definitions in dictionaries should be interpreted as having the same meaning as those disclosed in the relevant technical literature and this article, and should not be interpreted in an idealized or overly formal sense.

[0039] The high-strength free-cutting copper alloy and the preparation method thereof of the present invention are described below in conjunction with the accompanying drawings. However, the present invention can be implemented in various different ways and is not limited to the embodiments described herein.

[0040] According to a brass wire material of one embodiment of the present invention, the composition of the brass includes: Cu: 62.0-64.0wt%; Fe≤0.005wt%; Ni≤0.005wt%; Pb≤0.008wt%; the balance is Zn, and the total impurities do not exceed 0.1wt%; the brass phase structure includes 94-100% of matrix α phase and 0-6% of grain boundary β phase; the average grain size of the brass is ≤4μm, preferably 1-4μm.

[0041] According to a brass wire material of one embodiment of the present invention, the composition of the brass includes: Cu: 62.0-64.0wt%; Fe≤0.005wt%; Ni≤0.005wt%; Pb≤0.008wt%; Sn: 0.001-0.05wt%; the balance is Zn, and the total impurities do not exceed 0.1wt%; the brass phase structure includes 94-100% α phase and 0-6% grain boundary β phase; the average grain size of the brass is ≤4μm, preferably 1-4μm.

[0042] According to a brass wire material of one embodiment of the present invention, the composition of the brass includes: Cu: 62.0-64.0wt%; Fe≤0.005wt%; Ni≤0.005wt%; Pb≤0.008wt%; Sn: 0.001-0.05wt%; In: 0-0.05wt%; the balance is Zn, and the total impurities do not exceed 0.1wt%; the brass phase structure includes 94-100% α phase and 0-6% grain boundary β phase; the average grain size of the brass is ≤4μm, preferably 1-4μm.

[0043] First, the reason for limiting the brass component will be described.

[0044] The Cu content in brass affects the ratio of α phase and β phase in the brass structure. When the Cu content is lower than 64.0wt%, it can be seen from the Cu-Zn phase diagram that a certain proportion of β phase will appear in the original single-phase brass structure. β phase is a brittle phase. When its proportion is high, it is easy to cause cold forming cracking. The β phase ratio increases with the decrease of the Cu content in brass. When the Cu content is lower than 62.0wt%, the β phase ratio is getting higher and higher, and the brass wire is easy to crack when processing copper needles; when the Cu content exceeds 64wt%, the room temperature structure of brass is a single-phase α phase structure. The higher the Cu content, the better the plasticity of the material, and the easier it is to stick to the mold during cold forming. Therefore, the Cu content in the brass of the present invention ranges from 62.0 to 64.0wt%.

[0045] In the brass of the present invention, the content of Fe and Ni is strictly controlled to be below 0.005wt%. Because the negative active material zinc of the alkaline battery is very sensitive to impurities, when the surface of the zinc paste or the copper needle has trace metals such as Fe and Ni with low surface hydrogen evolution potential, the zinc paste will continuously self-discharge to produce hydrogen evolution reaction, which will affect the storage performance of the alkaline battery on the one hand, and more importantly, hydrogen will accumulate inside the battery, eventually opening the explosion-proof groove to cause battery leakage, and the leaked liquid will corrode the components, copper foil and solder joints on the electrical circuit board, causing the electrical appliance to be scrapped, resulting in a loss much higher than the value of the battery itself.

[0046] The content of the impurity element Pb in the brass of the present invention is limited to less than 0.008wt%, because Pb will reduce the conductivity of the current collector copper needle, reduce the battery capacity, and prolong the battery charging time; in addition, the solubility of Pb in α brass is extremely low, and it is distributed in the form of particles in the crystal and on the grain boundary, which makes the cold deformation performance of brass worse.

[0047] Adding a trace amount of Sn element to the brass of the present invention can improve the stability of the battery's electrical performance, but when the Sn content exceeds 0.05wt%, it has a greater impact on the conductivity of the copper needle. Therefore, the Sn content in the brass of the present invention is in the range of 0.001 to 0.05wt%.

[0048] A trace amount of In element can also be added to the brass of the present invention. In has a higher hydrogen evolution potential than Sn, and the battery containing In has stable electrical performance. In and the Sn element in the copper needle work synergistically to further improve the stability of the battery's electrical performance. However, In is a precious metal element and is expensive, so the amount of In added to the brass of the present invention is controlled to be 0 to 0.05 wt%.

[0049] The balance is Zn element and inevitable impurities. Zn element is a basic component element of brass alloy, and together with Cu element, forms an alloy matrix. The content of impurity elements is strictly limited in order not to affect the effect of the present invention.

[0050] The influence of the brass phase composition is then explained.

[0051] The proportion of α phase in the brass microstructure of the present invention should reach 94-100%, because the α phase has excellent cold deformation performance, and the α single-phase brass wire is easier to cold-forging than the α+β dual-phase brass wire.

[0052] Furthermore, the average grain size of the brass of the present invention is ≤4μm, preferably 1-4μm, because the grain size affects the surface quality of the metal. Due to the different grain orientations in the brass structure, there are slight differences in the degree of deformation of grains with different orientations. Larger grains are prone to bulges and pits, while smaller grains are not prone to such phenomena. In other words, the finer the grains inside the copper wire, the higher the surface finish. However, if the grains are too fine, the yield strength ratio and yield strength of the copper wire will increase, which is not conducive to the cold heading of the copper needle.

[0053] The surface quality of the brass wire obtained should meet the following requirements: take a sample under a 50x microscope, illuminate it vertically with a standard white light source, and observe the surface condition of the wire through the eyepiece. The surface of the wire should be uniform in color, without cracks, pits, abrasions, etc. with a size exceeding 10μm; slight scratches and wire flow defects are allowed, their depth does not exceed 0.6μm, and the total number of defects per unit area does not exceed 2 / cm 2 This is because the surface of the current collector copper needle needs to be electroplated, and the plating depth is generally 0.5 to 1 μm. When the depth of the copper needle surface defect exceeds the plating depth, the plating layer will not be able to completely cover the copper needle surface defect, resulting in leakage during battery use.

[0054] Next, we will explain the characteristics of brass wire.

[0055] The brass wire obtained by the present invention satisfies the following related properties: tensile strength Rm is 550-680MPa, elongation A is 3-12%, and conductivity σ≥24%IACS. If the mechanical properties of the brass wire of the present invention are too high, not only will the deformation resistance in the cold extrusion forming process increase sharply, the mold (especially the slender punch) is prone to instability and fracture, but also the rebound of each process is large, the process stability is poor, and the surface quality of the parts is not good. If the mechanical properties are too low, although the cold extrusion forming process can be ensured to proceed smoothly and the mold life can be extended, the final mechanical property value of the cold extruded part cannot meet the specified requirements. The conductivity of the battery core determines the size of the internal resistance of the battery, which in turn affects the discharge efficiency and overall performance of the battery. The core rod with high conductivity can reduce the resistance, so that the energy loss of the battery during the discharge process is reduced, thereby improving the energy conversion efficiency and service life of the battery.

[0056] Give the production method of brass wire.

[0057] The production method of the brass wire of the present invention mainly includes the following process flow: smelting → upward continuous casting → stretching → annealing → large-scale continuous drawing and annealing → medium-scale continuous drawing and annealing → inspection and packaging. Specifically, the ingredients are prepared and smelted according to the component requirements; then the smelted copper water is flowed into the casting equipment for casting to produce the ingot, and then the ingot is stretched and peeled, and then heated and annealed. The ingot after annealing is continuously stretched and annealed until the brass wire meets the requirements.

[0058] (1) Melting: Induction furnace is used for melting and casting, and the melting temperature is 960~1080℃. Since this product has high requirements for the content of impurities such as Fe, Ni, and Pb, the raw materials are electrolytic copper, zinc ingots and Cu-In master alloys. The Fe, Ni, and Pb content of electrolytic copper and zinc ingots must be below 0.003wt%, and iron tools cannot be used for stirring during the feeding process. For every ton of copper liquid melted, a modifier Cu-Zr master alloy must be added, and the addition amount is 0.005~0.03wt%, in order to improve the casting structure of the alloy, refine the grains, and improve the plastic processing performance of the ingot.

[0059] (2) Upward continuous casting: the billet specification is 8-16 mm, the casting temperature is 1030-1060°C, the pulling speed is 0.8-2.0 m / min, the pulling pitch is 2-8 mm, and the duty cycle is 20-80%. In order to ensure that the mechanical properties of the billet meet the production requirements of the product of the present invention, it is necessary to sample and test the mechanical properties of the billet to meet the following requirements: the tensile strength is 360-420 MPa, and the elongation A100 is ≥40%.

[0060] (3) Stretching: The upper casting billet is stretched and stripped to 6-8.5 mm in diameter. The stripping amount must be no less than 0.2 mm. The stripping cannot be eccentric. The surface of the wire billet after stretching must not have defects such as silk flow, bamboo knot pattern, and cracked skin.

[0061] (4) Annealing: The wire billet after stretching is annealed in a step-by-step manner to improve the uniformity of annealing. The first stage annealing temperature is 460-520°C, the heating time is 60-120 minutes, and the holding time is 30-90 minutes; the second stage annealing temperature is 530-590°C, the heating time is 60-120 minutes, and the holding time is 120-240 minutes.

[0062] (5) Long-drawing and medium-drawing continuous annealing: Continuous drawing and continuous annealing refers to the process of obtaining the required size of the wire blank after a certain number of stretching dies. In order to make the wire convenient for the next processing step, online annealing is performed to eliminate work hardening. The traditional online annealing method is to use a contact brush to transmit a large current for continuous annealing. The short-circuit current heats the copper wire and softens it. This method is suitable for annealing wires with low surface requirements. Its disadvantage is that sparks sometimes occur between the copper wire and the electrode wheel, causing electric shock on the surface of the copper wire. There is relative movement between the electrode wheel and the high-temperature softened copper wire, which is easy to cause scratches. It cannot meet the high surface quality requirements of the battery collector copper needle. Induction continuous annealing uses the principle of electromagnetic induction to heat and anneal the copper wire. When the copper wire passes through the induction coil, due to the high-frequency electric and magnetic fields generated inside the induction coil, an alternating current is generated inside the copper wire, thereby generating heat to achieve annealing. Induction continuous annealing is a non-contact annealing method. The copper wire is annealed evenly and the surface color is consistent, which completely avoids the problems of electric shock and scratches in traditional contact annealing.

[0063] ① Continuous drawing and annealing: The present invention adopts induction continuous annealing. After the previous annealing step, the Φ6-8.5mm wire billet is first stretched to Φ2-4mm by continuous drawing and annealing. The stretching speed is 1-5m / s, the annealing voltage is 20-100V, the annealing current is 1000-3000A, the annealing coefficient is 5-12, the cooling water temperature is 30-45°C, the wire drawing emulsion concentration is 3-8%, the emulsion temperature is controlled at 20-38°C, and the pH value is controlled at 7.0-7.5.

[0064] ② Intermediate drawing and continuous annealing: After the large drawing and continuous annealing, the Ф2-4mm wire billet is further stretched to the specifications of the battery core wire product by intermediate drawing and continuous annealing. The stretching speed in the intermediate drawing and continuous annealing is 2-12m / s, the annealing voltage is 0-130V, the annealing current is 80-350A, the cooling water temperature is 30-40°C, the concentration of the wire drawing emulsion is 5-15%, preferably 7-12wt%, the temperature of the emulsion is controlled at 20-38°C, and the pH value of the emulsion is controlled at 7.5-9.

[0065] If the concentration of the emulsion is too low, the lubrication effect is poor, the friction between the copper wire surface and the mold is large, and the surface finish is poor; if the concentration is too high, it will cause slippage during stretching, affecting the surface quality of the wire. If the temperature of the emulsion is too high, the stability of the emulsion will deteriorate, and if the temperature is too low, the lubrication performance will deteriorate. The pH value of the emulsion is controlled between 7.5 and 9. Within this range, it is difficult for microorganisms to reproduce, otherwise it will promote bacterial growth and the performance of the emulsion will decrease.

[0066] In the process of fine wire production, there are three major problems that plague the industry: first, the hardness and surface finish of the current brass wire drawing die are difficult to meet the requirements of high-surface battery core wires, and there are wire flow defects on the surface of the copper wire; second, the smaller the diameter of the copper wire, the faster the drawing speed, the more serious the jitter phenomenon, and the jitter will cause intermittent friction between the copper wire and the die outlet, causing scratches; third, when the copper wire passes through the continuous pulling and retracting unit, it is inevitable that it will come into contact with the surface of many tower wheels and wire-passing wheels. Long-term friction can easily cause wear marks on the contact surface between the copper wire and the wheel, and the raised parts of the wear marks scratch the surface of the copper wire to cause pits and scratches.

[0067] In this regard, the present invention has made the following improvements: First, the drawing die selection requirements for a group of wires (generally 2 to 12 per group) are as follows: the front drawing die is a polycrystalline die, and the last 2-3 drawing dies are a South African natural diamond die. The working cone angle of the drawing die is controlled at 14 to 22°, the sizing belt length h = 0.3 to 0.7 times the die aperture, and the outlet cone angle is 40 to 60°. Diamond is the hardest material in the world. It is formed by natural crystallization and is a single crystal without particles. The molecular arrangement structure is more reasonable and the wear resistance is excellent. The surface finish Ra of the die hole sizing belt should reach 0.005 to 0.015 μm. South African diamond is more superior to other origins in hardness and toughness. The polycrystalline material has uniform crystallinity and high surface finish. It is a wear-resistant synthetic material with the lowest friction. These characteristics enable the polycrystalline wire drawing die to ensure the surface finish and accuracy of the wire during the long-term wire drawing process. The working area of ​​the drawing die is the metal stretching plastic deformation area. The sizing zone of the drawing die is to make the wire get the final size. If the sizing zone is too long, the friction will increase during drawing and the surface finish will deteriorate. In order to improve the surface quality, a short sizing zone should be selected. The wire exit area of ​​the drawing die is the last part of the copper wire leaving the die hole. The setting of the working cone angle and the outlet cone angle can avoid damage to the copper wire at the outlet of the sizing and scratches when the wire is reversed during shutdown.

[0068] The second is to improve the problem of copper wire jitter: when drawing thin wires at high speed, equipment jitter, the copper wire stretching axis and the center line of the die hole are not completely in a straight line, the drawing die wears, the tension on the wire storage wheel is unstable, the wire drawing lubrication is poor, the main motor gear box wears, etc. will cause the high-speed moving wire to jitter, and the jitter phenomenon becomes more serious as the drawing speed increases. However, reducing the drawing speed will inevitably lead to a decrease in production efficiency. In this regard, the present invention designs and installs a copper wire jitter absorber at the outlet of the ceramic nozzle of the wire drawing die, the induction annealing section, and the cooling section pipeline. The principle is to use soft absorption materials to absorb the energy generated by the copper wire jitter under a certain pressure, thereby avoiding the jitter of the copper wire. The soft absorption material here is mainly composed of natural fibers with a density of 0.1 to 0.45 g / cm 3 If the density is too high, it is easy to scratch the surface of the copper wire. If the density is too low, the energy absorption is weak. The applied pressure is 0.5-2kgf / cm 2 If the pressure is too small, the copper wire will shake. If the pressure is too large, the friction resistance between the copper wire and the absorbent material will increase, and the friction marks on the surface of the copper wire will increase.

[0069] The second is to improve the problem of easy wear of the tower wheel and the wire wheel: the surface of all the tower wheels and wire wheels in contact with the copper wire in the medium-drawn continuous reel is sprayed with a zirconium oxide coating, and the chemical composition of the zirconium oxide coating is: the main component ZrO2 with a content of 90-96wt%, and the rare earth stabilizer Y2O3 with a content of 4-10wt%; the main component phase composition is m-ZrO2, t-ZrO2 and c-ZrO2 three-phase composition, of which the area of ​​c-ZrO2 accounts for 80-90%, the area of ​​m-ZrO2 accounts for 2-6%, and the area of ​​t-ZrO2 accounts for 8-14%. The density of the zirconium oxide coating is ρ≥6.2g / cm 3 , hardness HRA needs to reach 85~90. It is well known that the hardness of zirconium oxide is 5 times that of diamond. The hardness represents the ability of the material to resist scratches. The performance of zirconium oxide mainly depends on the phase composition and distribution ratio. Zirconia has three phase structures: monoclinic phase (m-ZrO2), tetragonal phase (t-ZrO2) and cubic phase (c-ZrO2), wherein the metastable tetragonal phase can be transformed into a stable monoclinic phase under stress induction, and a large amount of fracture energy is absorbed due to the volume effect produced by the phase change, slowing down or preventing the propagation of cracks, and enhancing the toughness of the zirconium oxide coating; cubic phase zirconium oxide has high density and high hardness, and the higher the proportion of this phase, the higher the hardness of the coating, and the better the wear resistance, but in order to improve the hardness and brittleness of the coating, the addition of a certain proportion of tetragonal phase and monoclinic phase can effectively avoid the coating from cracking and falling off due to high hardness and brittleness. Therefore, the zirconium oxide coating used in the present invention is composed of three phases, which can effectively solve the problem of easy wear of the tower wheel and the wire wheel.

[0070] (6) Inspection and packaging: Test the mechanical properties of the wire and observe the distribution and size of surface defects under a 50x microscope. Qualified wires can be put into storage.

[0071] Thus, the brass wire obtained has a tensile strength of 550-680MPa, an elongation of 3-12%, a conductivity of ≥24% IACS, and a defect size of <10μm, a defect depth of <0.6μm, and a total number of defects of no more than 2 / cm under a 50x microscope. 2 The contact resistance between the current collector copper needle and the zinc paste made of the wire is small, the primary battery corrosion and hydrogen evolution reaction of the zinc paste are greatly weakened, and the battery leakage situation is greatly improved.

[0072] The present invention provides 3 embodiments and 1 comparative example, and the alloy compositions are shown in Table 17.

[0073] Example 1

[0074] A production method of a brass wire with a specification of Φ1.29 mm is as follows:

[0075] (1) Smelting: Electrolytic copper, zinc ingot, tin ingot and Cu-In master alloy are added into a smelting furnace according to the proportion and smelted in vacuum at a smelting temperature of 960-1080°C. The measured contents of Fe, Ni and Pb impurities in electrolytic copper are 0.0011wt%, 0.0013wt% and 0.0010wt% respectively; the measured contents of Fe, Ni and Pb impurities in zinc ingot are 0.0013wt%, 0.0010wt% and 0.0014wt% respectively. 0.012wt% of zirconium-copper alloy (Zr content: 50wt%) is added to each ton of molten copper.

[0076] (2) Upward continuous casting: billet specification Φ10mm, casting temperature 1040-1050℃, traction speed 1.5m / min, traction pitch 4mm, duty cycle 40%. The measured mechanical properties of the billet are: tensile strength 382MPa, elongation A100 46.5%.

[0077] (3) Stretching: The upper cast billet is stretched and stripped to Φ7.8 mm, and the stripping amount is 0.24 mm.

[0078] (4) Annealing: The first stage annealing temperature is 500°C, the heating time is 90 min, and the holding time is 60 min; the second stage annealing temperature is 550°C, the heating time is 30 min, and the holding time is 180 min.

[0079] (5) Continuous drawing and annealing: The Φ7.8 mm wire billet after annealing is stretched to Φ3 mm through continuous drawing and annealing. The process parameters are as follows:

[0080] Table 1 Process parameters of large-scale continuous drawing and annealing in Example 1

[0081]

[0082] (6) Intermediate drawing and annealing: After the large drawing and annealing, the Φ3 mm wire billet is stretched to the finished product Φ1.29 mm through intermediate drawing and annealing. The intermediate drawing and annealing process parameters are as follows:

[0083] Table 2 Continuous drawing and annealing process parameters in Example 1

[0084]

[0085] The parameters of the mold used are as follows:

[0086] Table 3 Die parameters for continuous drawing in Example 1

[0087]

[0088] The technical parameters of the surface coating of the intermediate pulley and the wire pulley are as follows:

[0089] Table 4 Technical parameters of the surface coating of the pulley and the wire wheel in Example 1

[0090]

[0091]

[0092] (7)Inspect the packaging.

[0093] Example 2

[0094] A production method of a brass wire with a specification of Φ1.2mm is as follows:

[0095] (1) Smelting: Electrolytic copper, zinc ingots and Cu-In master alloy are added into a smelting furnace according to the proportions for vacuum smelting at a smelting temperature of 990-1040°C. The measured contents of Fe, Ni and Pb impurities in the electrolytic copper are 0.0012wt%, 0.0013wt% and 0.0011wt% respectively; the measured contents of Fe, Ni and Pb impurities in the zinc ingot are 0.0016wt%, 0.0014wt% and 0.0012wt% respectively. 0.009wt% of zirconium-copper alloy (Zr content: 50wt%) is added for every ton of molten copper.

[0096] (2) Upward continuous casting: billet specification Φ9.8mm, casting temperature 1045-1055℃, traction speed 1.6m / min, traction pitch 3.5mm, duty cycle 40%. The measured mechanical properties of the billet are: tensile strength 391MPa, elongation A100 44%.

[0097] (3) Stretching: The upper cast billet is stretched and stripped to Φ7.6 mm, and the stripping amount is 0.22 mm.

[0098] (4) Annealing: The first stage annealing temperature is 490°C, the heating time is 90 min, and the holding time is 90 min; the second stage annealing temperature is 540°C, the heating time is 45 min, and the holding time is 210 min.

[0099] (5) Continuous drawing and annealing: The Φ7.6 mm wire billet after annealing is stretched to Φ2.9 mm through continuous drawing and annealing. The process parameters are as follows:

[0100] Table 5 Process parameters of large-scale continuous drawing and annealing in Example 2

[0101]

[0102] (6) Intermediate drawing and annealing: After the large drawing and annealing, the Φ3 mm wire billet is stretched to the finished product Φ1.29 mm through intermediate drawing and annealing. The intermediate drawing and annealing process parameters are as follows:

[0103] Table 6 Continuous drawing and annealing process parameters in Example 2

[0104]

[0105]

[0106] The parameters of the mold used are as follows:

[0107] Table 7 Die parameters for continuous drawing in Example 2

[0108]

[0109] The technical parameters of the surface coating of the intermediate pulley and the wire pulley are as follows:

[0110] Table 8 Technical parameters of the surface coating of the pulley and the wire wheel in Example 2

[0111]

[0112] (7)Inspect the packaging.

[0113] Example 3

[0114] A production method of a brass wire with a specification of Φ1.9 mm is as follows:

[0115] (1) Smelting: Electrolytic copper, zinc ingots and tin ingots were added into a smelting furnace according to the proportions for vacuum smelting at a smelting temperature of 1000-1060°C. The measured contents of Fe, Ni and Pb impurities in electrolytic copper were 0.0014wt%, 0.0012wt% and 0.0013wt% respectively; the measured contents of Fe, Ni and Pb impurities in zinc ingots were 0.0013wt%, 0.0015wt% and 0.0012wt% respectively. 0.022wt% of zirconium-copper alloy (Zr content: 50wt%) was added for every ton of molten copper.

[0116] (2) Upward continuous casting: billet specification Φ12mm, casting temperature 1050-1060℃, traction speed 1.3m / min, traction pitch 3mm, duty cycle 45%. The measured mechanical properties of the billet are: tensile strength 405MPa, elongation A100 46.3%.

[0117] (3) Stretching: The upper cast billet is stretched and stripped to Φ8.2 mm, and the stripping amount is 0.28 mm.

[0118] (4) Annealing: The first stage annealing temperature is 520°C, the heating time is 60 min, and the holding time is 60 min; the second stage annealing temperature is 570°C, the heating time is 60 min, and the holding time is 150 min.

[0119] (5) Continuous drawing and annealing: The Φ8.2 mm wire billet after annealing is stretched to Φ3.2 mm through continuous drawing and annealing. The process parameters are as follows:

[0120] Table 9 Process parameters of large-scale continuous drawing and annealing in Example 3

[0121]

[0122] (6) Intermediate drawing and annealing: After the large drawing and annealing, the Φ2-4 mm wire blank is stretched to the finished product Φ1-2 mm by intermediate drawing and annealing. The intermediate drawing and annealing process parameters are as follows:

[0123] Table 10 Continuous drawing and annealing process parameters in Example 3

[0124]

[0125] The parameters of the mold used are as follows:

[0126] Table 11 Die parameters for continuous drawing in Example 3

[0127]

[0128] The technical parameters of the surface coating of the intermediate pulley and the wire pulley are as follows:

[0129] Table 12 Technical parameters of the surface coating of the pulley and the wire wheel in Example 3

[0130]

[0131] (7)Inspect the packaging.

[0132] Comparative Example 1

[0133] A production method of a brass wire with a specification of Φ1.29 mm is as follows:

[0134] (1) Smelting: Electrolytic copper and zinc ingots are added into a smelting furnace according to the proportion and smelted in vacuum at a smelting temperature of 960-1080°C. The measured contents of Fe, Ni and Pb impurities in the electrolytic copper are 0.0014wt%, 0.0012wt% and 0.0013wt% respectively; the measured contents of Fe, Ni and Pb impurities in the zinc ingot are 0.0013wt%, 0.0015wt% and 0.0012wt% respectively. 0.022wt% of zirconium-copper alloy (Zr content: 50wt%) is added for every ton of molten copper.

[0135] (2) Upward continuous casting: billet specification Φ10mm, casting temperature 1030-1060℃, traction speed 2.0m / min, traction pitch 4.5mm, duty cycle 30%. The measured mechanical properties of the billet are: tensile strength 356MPa, elongation A100 38%.

[0136] (3) Stretching: The upper cast billet is stretched and stripped to Φ7.8 mm, and the stripping amount is 0.16 mm.

[0137] (4) Annealing: The annealing temperature is 520°C, the heating time is 60 min, and the holding time is 180 min.

[0138] (5) Continuous drawing and annealing: The Φ7.8 mm wire billet after annealing is stretched to Φ3 mm through continuous drawing and annealing. The process parameters are as follows:

[0139] Table 13 Comparative Example 1 Large Continuous Drawing Process Parameters

[0140]

[0141] (6) Intermediate drawing and annealing: After the large drawing and annealing, the Φ3 mm wire billet is stretched to the finished product Φ1.29 mm through intermediate drawing and annealing. The intermediate drawing and annealing process parameters are as follows:

[0142] Table 14 Continuous drawing and annealing process parameters in comparative example 1

[0143]

[0144]

[0145] The parameters of the mold used are as follows:

[0146] Table 15 Die parameters selected for continuous drawing in comparative example 1

[0147]

[0148] The technical parameters of the surface coating of the intermediate pulley and the wire pulley are as follows:

[0149] Table 16 Technical parameters of the surface coating of the pulley and the wire wheel in comparative example 1

[0150]

[0151] (7)Inspect the packaging.

[0152] The following tests were performed on Examples 1-3 and Comparative Example 1. The test results are detailed in Tables 18 and 19. Table 17 below is a comparison table of the chemical compositions of the Examples of the present invention and the Comparative Example.

[0153] The microscopic phase composition, phase area ratio and grain size of the product in the present invention are measured by metallographic analysis software under an optical microscope; the specific results are shown in the attached Figure 1 , Figure 2 As shown;

[0154] The tensile strength and elongation of the product in the present invention are tested in accordance with GB / T228.1-2021 "Metallic Materials Tensile Test Part 1: Room Temperature Test Method";

[0155] The surface roughness of the product in the present invention is measured according to GB / T1031-2016 (product geometry specification (GPS) surface structure profile method), and the surface roughness is evaluated by the center line system (profile method). The specific detection method is: the diamond stylus of the roughness measuring instrument slowly slides along the radial direction of the wire surface, and the Ra value of a measuring stroke is directly obtained from the indicating instrument, and the average value is obtained by measuring three times;

[0156] The surface defects of the product in the present invention are measured by using image analysis software under an optical microscope, as shown in the attached figure. Figure 3 , Figure 4 shown.

[0157] Table 17 Chemical composition of Examples 1-3 and Comparative Example 1 of the present invention

[0158]

[0159] Table 18 Microstructure and mechanical properties of Examples 1-3 of the present invention and Comparative Example 1

[0160]

[0161] Table 3 Surface test results of Examples 1-3 and Comparative Example 1 of the present invention

[0162]

[0163] Figure 1 This is a microstructure photograph of Example 1. The gray-white color in the figure is the matrix α phase, and the gray-black dots are the grain boundary β phase. It can be seen from the figure that the matrix α phase grains are small and evenly distributed, with an average grain size of only 1.8μm and an area share of 95.6%. There is also a very small amount of β phase in the figure. Figure 2 The microstructure of comparative example 1 is shown in the figure. The grayish white is the matrix α phase, the α phase grains are large and unevenly distributed, the average grain size reaches 12μm, and the area accounts for 92.5%. The grayish black is the β phase, the β phase grain size is large and the area accounts for 92.5%. Figure 1 A lot more. Figure 3 This is an optical microscope photograph of the wire of Example 1. In the picture, the surface of the wire is smooth and uniform in color, without defects such as cracks, pits, and scratches. There are only individual point defects, and the roughness is only 0.010μm. Figure 4 This is an optical microscope photograph of the wire obtained in Comparative Example 1. In the picture, the surface of the wire is not smooth and has many scratch defects. The surface roughness reaches 0.060μm.

[0164] Comparative Example 1 adopts a conventional production process, does not add additional elements such as Sn and In, and does not add a modifier Cu-Zr intermediate alloy; no step annealing is used after the first stretching, which results in uneven micro-grain sizes and uneven distribution, indirectly causing the elongation, conductivity and surface quality of the wire of Comparative Example 1 to be inferior to those of Examples 1-3.

[0165] Meanwhile, the conventional mold, emulsion parameters, and conventional surface coatings for the step pulley and the wire passing pulley are used in the middle drawing and annealing process of Comparative Example 1, which results in defects such as cracks, pits, and scratches. The above factors lead to the surface quality of the finished product of Comparative Example 1 being inferior to that of Examples 1-3.

[0166] The present invention can be implemented in various ways and is not limited to the above-mentioned embodiments and / or examples. A person skilled in the art can understand that the present invention can be implemented in other specific ways without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments and / or examples are exemplary and are not intended to limit the present invention.

Claims

1. A brass wire, characterized in that: The components of the brass include: Cu: 62.0-64.0wt%; Fe≤0.005wt%; Ni≤0.005wt%; Pb≤0.008wt%; the balance is Zn and inevitable impurities, and the total impurities do not exceed 0.1wt%; the brass phase structure includes 94-100% of matrix α phase and 0-6% of grain boundary β phase; the average grain size of the brass is ≤4μm.

2. A brass wire according to claim 1, characterized in that: The tensile strength of the brass wire is 550-680 MPa; Preferably, the elongation of the brass wire is 3 to 12%; Preferably, the electrical conductivity of the brass wire is ≥24% IACS; Preferably, the average grain size of the brass is 1 to 4 μm.

3. A brass wire according to claim 1 or 2, characterized in that: The brass wire has a defect size of less than 10 μm, a defect depth of less than 0.6 μm, and a total number of defects of no more than 2 / cm under a 50x microscope. 2 .

4. A brass wire according to claim 3, characterized in that: The brass component also includes Sn: 0.001-0.05wt%; the Sn element is added to replace the Zn element.

5. The brass wire according to claim 3, characterized in that: The brass component also includes In: 0-0.05wt%; the In element is added to replace the Zn element.

6. The brass wire according to claim 4, characterized in that: The brass component also includes In: 0-0.05wt%; the In element is added to replace the Zn element.

7. A method for producing a brass wire according to any one of claims 1 to 6, characterized in that: The process includes the following steps: smelting → upward continuous casting → stretching → annealing → large drawing and continuous annealing → medium drawing and continuous annealing → inspection and packaging; The annealing is a step annealing, wherein the annealing temperature of the first stage is 460-520° C., and the holding time is 30-90 minutes; the annealing temperature of the second stage is 530-590° C., and the holding time is 120-240 minutes.

8. The method for producing a brass wire according to claim 7, characterized in that: The raw materials used for smelting are electrolytic copper, zinc ingots, tin ingots and Cu-In master alloys, among which the Fe, Ni and Pb contents of electrolytic copper, zinc ingots and tin ingots must be below 0.003%, and iron tools cannot be used for smelting and stirring; Preferably, 0.005-0.03 wt % of Cu-Zr master alloy is added per ton of molten copper. Preferably, the smelting temperature is 960-1080°C.

9. A method for producing a brass wire according to claim 7 or 8, characterized in that: The casting temperature of the upward continuous casting is 1030-1060°C, the pulling speed is 0.8-2.0 m / min, and the pulling pitch is 2-8 mm; preferably, the skinning process is directly performed after stretching; Preferably, the long-drawing and medium-drawing continuous annealing are both performed by induction continuous annealing; Preferably, the stretching speed in the continuous drawing and annealing is 1-5 m / s, the annealing voltage is 20-100 V, the annealing current is 1000-3000 A, the annealing coefficient is 5-12, the cooling water temperature is 30-45° C., the emulsion concentration is 3-8%, and the emulsion pH value is 7.0-7.5; Preferably, the stretching speed in the middle drawing and annealing is 2-12 m / s, the annealing voltage is 0-130 V, the annealing current is 80-350 A, the cooling water temperature is 30-40° C., the emulsion concentration is 7-12%, the emulsion pH value is 7.5-9, the last two to three stretching dies are South African natural diamond dies, the stretching working cone angle is 14-22°, the length of the stretching sizing belt is 0.3-0.7 of the die aperture, and the stretching outlet cone angle is 40-60°; More preferably, copper wire vibration absorbers are installed at the outlets of the drawing die, induction annealing and cooling section pipeline ceramic nozzles; preferably, all the tower wheels and wire wheels in contact with the copper wire are sprayed with zirconium oxide coatings, and the coating density is ≥6.2g / cm 3 , hardness HRA needs to reach 85-90; More preferably, the zirconium oxide coating comprises 90-96wt% zirconium oxide and 4-10wt% Y2O3, wherein the zirconium oxide is composed of 80-90% c-ZrO2 with an area percentage of 2-6%, m-ZrO2 with an area percentage of 8-14%, and t-ZrO2 with an area percentage of 8-14%.

10. Use of the brass wire according to any one of claims 1 to 6 in a battery current collector.

Citation Information

Cited By

  • Wire surface defect detection method and system based on image recognition model

    CN120510103A

  • Pseudo-ginseng brass for bullets and preparation method thereof

    CN120606065A