Method for preparing adjustable localized surface plasma by using nano array
By preparing nanoarrays in gallium oxide-based devices, the local field is enhanced, and the problem of low performance of gallium oxide-based devices is solved, the combination of high light current and low dark current is achieved, and the detection rate and performance of Ga2O3 film is improved.
Patent Information
- Application Number
- CN202410887815.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-22
AI Technical Summary
The detection rate and other performance of existing gallium oxide-based devices is low, mainly because while increasing the photocurrent, the dark current will also increase, resulting in no significant increase in the light-dark current ratio, which limits the application of Ga2O3 films.
Using nanoarrays to prepare adjustable local surface plasma methods, metal nanoarrays are prepared by laser molecular beam epitaxial, enhancing the local field, increasing the photocurrent without increasing the dark current. The specific steps include cleaning the substrate, preparing semiconductor films and preparing Metal nanoarrays.
The photocurrent of Ga2O3 film is significantly improved, the detection rate and performance are improved, and the nanoarray is formed under low temperature conditions, maintaining the low dark current of the material, enhancing the light capture capability and carrier generation.
Smart Images

Figure CN118996342A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor optoelectronic technology, and in particular relates to a method for preparing adjustable localized surface plasma using a nanoarray. Background Art
[0002] β-Ga 2 O 3 As a wide bandgap semiconductor material (bandgap width is 4.9eV), it has broad application prospects in many fields such as solar-blind ultraviolet detectors, deep ultraviolet transparent conductive films, gas sensors and thin-film transistors, and has become a research hotspot in the field of wide bandgap semiconductor materials. 2 O 3 There are still many problems with the performance of the film, which greatly limits its application in the fields of light emission, detection and electronic devices. How to improve the performance of the gallium oxide film itself is a key issue in improving the performance of gallium oxide-based devices.
[0003] In order to make Ga 2 O 3 Thin films can be used more widely. One of the best solutions is not to increase the Ga 2 O 3 The dark current of the film is also improved 2 O 3 At present, there are many studies on improving the performance of gallium oxide-based devices, but there are still many problems; the reason why it is difficult to effectively prepare high-performance Ga using laser molecular beam epitaxy is that 2 O 3 The main reason is that when the photocurrent of gallium oxide-based devices is increased, the dark current of gallium oxide-based devices will also increase, so that the light-to-dark current ratio of the device is not greatly improved. This greatly limits the 2 O 3 Thin film detection rate and other properties. Summary of the invention
[0004] The present invention designs a method for preparing adjustable localized surface plasma using a nanoarray, which solves the technical problem that the existing gallium oxide-based devices have low performance such as detection rate.
[0005] In order to solve the above-mentioned technical problems, the present invention adopts the following solutions: A method for preparing adjustable localized surface plasma using nanoarrays includes the following steps: step 1, cleaning the substrate; step 2, preparing a semiconductor film; step 3, preparing a metal nanoarray.
[0006] Preferably, the preparation of the metal nanoarray in step 3 is carried out by laser molecular beam epitaxy, which specifically includes the following steps: step 31, mounting the metal target on the target holder of the laser molecular beam epitaxy system, and then covering the clean porous anodized aluminum template on the semiconductor film prepared in step 2 to form an assembly; step 32, fixing the assembly to the sample holder of the growth chamber, and then evacuating, heating, and introducing sputtering gas into the growth chamber; step 33, finally using a pulsed laser to focus on the surface of the target material to deposit the assembly, and after the deposition is completed, removing the porous anodized aluminum template to obtain the metal nanoarray.
[0007] Preferably, the heating temperature in step 32 is 20°C-800°C; or / and, the growth chamber is evacuated to 1*10 - 6 Pa, and the vacuum degree is maintained at 1*10 -3 Pa-30Pa; or / and, the sputtering gas in step 32 is oxygen or a mixture of oxygen and argon; or / and, the pressure in the growth chamber after the sputtering gas is introduced in step 32 is 5*10 -2 Pa.
[0008] Preferably, the thickness of the metal nanoarray in step 33 is 1-10 nm; or / and, the deposition time in step 33 is 95 seconds; or / and, the power of the pulse laser used in step 33 is 300 mW.
[0009] Preferably, the semiconductor film is prepared in step 2 by pulsed laser deposition, comprising the following steps: Step 21, fix the cleaned substrate in step 1 to the sample stage of the growth chamber, install the semiconductor target on the target holder, evacuate the vacuum, heat the substrate, and introduce sputtering gas; Step 22: When a laser pulse is focused on the target surface, the target material is instantly evaporated to form a plasma plume containing the target material elements; the plasma plume then rapidly expands in a direction perpendicular to the target surface and is deposited on the substrate surface obtained in step 1 to form a semiconductor film.
[0010] Preferably, the heating temperature in step 21 is 20° C.-800° C.; or / and, In step 21, the growth chamber is evacuated to 1*10 -6 Pa, and the vacuum degree is maintained at 1*10 -3 Pa-30Pa; or / and, the sputtering gas in step 21 is oxygen or a mixture of oxygen and argon; or / and, the pressure of the growth chamber after the sputtering gas is introduced in step 21 is 5*10 -2 Pa.
[0011] Preferably, the deposition time in step 22 is 20 min-360 min; or / and, the pulse laser power in step 22 is 300 mW.
[0012] Preferably, the specific steps of cleaning the substrate in step 1 are: putting the substrate into a beaker, ultrasonically cleaning with acetone, alcohol, and deionized water for more than 5 minutes to remove organic impurities and residual ions on the substrate, and then drying with nitrogen or inert gas for later use; Preferably, the substrate is made of single crystal sapphire, single crystal silicon, single crystal gallium oxide, silicon carbide or quartz glass.
[0013] Preferably, the method for preparing the semiconductor film in step 2 can be replaced by: magnetron sputtering deposition, pulsed laser deposition, molecular beam epitaxy, plasma enhanced chemical vapor deposition, organometallic chemical vapor deposition and the like; Alternatively, the method for preparing the metal nanoarray in step 3 can be replaced by thermal evaporation, electron beam evaporation, magnetron sputtering deposition, pulsed laser deposition, molecular beam epitaxy, plasma enhanced chemical vapor deposition or organometallic chemical vapor deposition.
[0014] A metal nanoarray, characterized in that: the semiconductor photocurrent is increased by more than 10 times when prepared by the above method; the semiconductor is Ga 2 O 3 , zinc oxide, tin dioxide, hafnium oxide, cuprous oxide, aluminum nitride, gallium nitride, boron nitride or indium nitride.
[0015] The method of preparing adjustable localized surface plasmon using nanoarrays has the following beneficial effects: (1) The present invention generates an enhanced local field by introducing a metal nanoarray, amplifying the electromagnetic field near the metal nanoparticles, and can absorb more photons at the same absorption intensity. While not increasing the dark current of the material, it increases the photocurrent of the material, which can significantly improve the material's detection rate and other performance.
[0016] (2) The target particles sputtered by the present invention have higher energy and better adhesion to the substrate, and can form nanoarrays at lower temperatures or even at room temperature. The deposition of nanoarrays at low temperatures can be achieved on some special substrate materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 is the extinction spectrum of aluminum nanoparticles; Figure 2 Ga modified with aluminum nanoparticle arrays at different particle spacings 2 O 3 Local light field distribution diagram of the film; Figure 3This is a scanning electron microscope image of the metal nanoarray prepared by the present invention; Figure 4 is a small-scale scanning electron microscope (SEM) image of the nanoarray of the present invention; Figure 5 This is a large-scale scanning electron microscope (SEM) image of the nanoarray of the present invention. DETAILED DESCRIPTION
[0018] Combine the following Figures 1 to 5 , the present invention is further described: like Figure 1 As shown, Al nanoparticles show a very significant localized surface plasmon resonance (LSPR) peak for light around a wavelength of about 250 nm. This finding indicates that Al nanoparticles have very strong LSPR characteristics for light in this specific band, which is of great significance for the design and optimization of optoelectronic devices based on metal nanoparticles. This property of Al nanoparticles can be used to enhance the light absorption efficiency of photodetectors and improve the sensitivity and response speed of devices. In addition, the intensity and position of the LSPR effect can be controlled by changing the shape, size and arrangement of metal nanoparticles, which provides flexibility for designing nanostructures with specific optical properties. By precisely controlling the LSPR effect of Al nanoparticles, precise control of ultraviolet light detection performance can be achieved to meet the needs of specific applications.
[0019] like Figure 2 As shown, the light field distribution of four different structures at a wavelength of 250 nm. The array with a spacing of 150 nm can allow more light to be transmitted into the gallium oxide film. The distribution of this light field intensity is crucial for understanding how aluminum nanoparticles affect the optical properties of gallium oxide films.
[0020] like Figure 3 As shown, the dot-like protrusions are aluminum nanoarrays. These nanoparticles are highly regularly arranged and consist of a series of ordered nanodots, demonstrating the uniformity and periodicity of the nanoarray. When spherical metal nanoparticles are irradiated with light, the oscillating electric field causes the electrons to oscillate coherently. When the electron cloud is displaced relative to the nucleus, the Coulomb attraction between them generates a restoring force, causing the electron cloud to oscillate collectively relative to the metal lattice. Nanoparticles (NPs) have a very large specific surface area and a strong local field enhancement effect, which can amplify the electromagnetic field near the nanoparticles and absorb more photons under the same conditions.
[0021] like Figure 4 and Figure 5As shown in the figure, aluminum nanoarrays can improve their light capture capabilities through their high specific surface area and local field enhancement effect. This enhanced light capture capability not only increases the generation of photogenerated carriers, but may also affect the performance of the detector by changing the kinetic behavior of carriers. For example, aluminum nanoarrays can act as carrier traps, extending their lifetimes and thus improving the signal strength of the detector. At the same time, this trap effect may also affect the carrier recombination process, thereby regulating the response time and recovery time of the detector.
[0022] The photothermal hotspots generated by the plasma resonance (LSPR) effect of the aluminum nanoarrays on the surface of the metal nanostructures provide areas of high energy density for carriers. These photothermal hotspots can act as traps for carriers and significantly affect the response characteristics of the detector. By adjusting the size, shape and spacing of the aluminum nanoarrays, we can precisely control the distribution and intensity of the photothermal hotspots, thereby optimizing the performance of the detector.
[0023] Embodiment 1: This embodiment is to prepare Ga with high photoelectric performance 2 O 3 The method for producing a thin film is specifically carried out according to the following steps: Step 1: Clean the substrate. Place the sapphire substrate in a beaker and ultrasonically clean it for 5 minutes using acetone, alcohol, and deionized water in sequence, and then blow dry it with nitrogen.
[0024] Step 2: Preparation of Ga using laser molecular beam epitaxy 2 O 3 film.
[0025] Ga 2 O 3 The target material is mounted on the target holder of the laser molecular beam epitaxy system, and then the substrate cleaned in step 1 is fixed to the sample holder of the growth chamber and evacuated to 1*10 -6 Pa, heat the substrate to 400°C, introduce oxygen, and adjust the gate valve to keep the pressure of the vacuum chamber at 5*10 -2 Pa.
[0026] Turn on the pulse laser, deposit for 3600 seconds, remove the substrate, and obtain Ga 2 O 3 film.
[0027] Step 3: Prepare aluminum nanoarrays using laser molecular beam epitaxy. The specific steps are as follows: ① Install the metal aluminum target on the target holder of the laser molecular beam epitaxy system, and then cover the clean porous anodized aluminum template with the Ga prepared in step 2. 2 O 3The assembly is formed on the film; the assembly is fixed to the sample holder of the growth chamber and vacuumed to 1*10 -6 Pa, heat the assembly to 400°C, then introduce oxygen into the growth chamber; adjust the gate valve to keep the pressure of the vacuum chamber at 5*10 -2 Pa remains unchanged.
[0028] The pulse laser was turned on and the deposition was performed for 95 seconds. After the deposition was completed, the porous anodized aluminum template was removed to obtain a metal nanoarray.
[0029] Embodiment 2: The difference between this embodiment and the first embodiment is that the substrate heating temperature in step 2 is 300° C. The other aspects are the same as the first embodiment.
[0030] Embodiment 3: The difference between this embodiment and embodiment 1-2 is that the substrate heating temperature in step 2 is 200° C. The rest is the same as embodiment 1.
[0031] Embodiment 4: This embodiment is different from Embodiments 1-3 in that the temperature of the heated substrate in step 2 is 100° C. The rest is the same as Embodiment 1.
[0032] Embodiment 5: This embodiment is different from Embodiments 1-4 in that the temperature of the heated substrate in step 2 is room temperature. The rest is the same as Embodiment 1.
[0033] Example 6: This example is different from examples 1-5 in that the heating temperature in step 3 is 800° C. The rest is the same as example 1.
[0034] Example 7: This example is different from Examples 1-6 in that the heating temperature in step 3 is 700° C. The rest is the same as Example 1.
[0035] Embodiment 8: This embodiment differs from Embodiments 1-7 in that the heating temperature in step 3 is 600° C. The rest is the same as Embodiment 1.
[0036] Example 9: This example is different from Examples 1-8 in that the heating temperature in step 3 is 500° C. The rest is the same as Example 1.
[0037] Example 10: This example is different from Example 1-9 in that the heating temperature in step 3 is 400° C. The rest is the same as Example 1.
[0038] Examples 3-10 all involve changing the temperature, and this temperature change has a change in the bandgap width: the higher the heating temperature, the larger the bandgap width, and the two are in a proportional relationship.
[0039] The present invention is described above by way of example in conjunction with the accompanying drawings. It is obvious that the implementation of the present invention is not limited to the above-mentioned method. As long as various improvements are made using the method concept and technical solution of the present invention, or the concept and technical solution of the present invention are directly applied to other occasions without improvement, they are all within the protection scope of the present invention.
Claims
1. A method for preparing adjustable localized surface plasma using a nanoarray, comprising the following steps: step 1, cleaning the substrate; step 2, preparing a semiconductor film; step 3, preparing a metal nanoarray.
2. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 1, characterized in that: In step 3, the metal nanoarray is prepared by laser molecular beam epitaxy, which specifically includes the following steps: Step 31, mounting the metal target on the target holder of the laser molecular beam epitaxy system, and then covering the clean porous anodized aluminum template on the semiconductor film prepared in step 2 to form a composite body; Step 32, fixing the assembly to the sample holder of the growth chamber, and then evacuating the growth chamber, heating it, and introducing sputtering gas; Step 33: Finally, a pulsed laser is used to focus on the target surface to deposit the assembly. After the deposition is completed, the porous anodized aluminum template is removed to obtain a metal nanoarray.
3. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 2, characterized in that: In step 32, the heating temperature is 20°C-800°C; or / and, In step 32, the growth chamber is evacuated to 1*10 -6 Pa, and the vacuum degree is maintained at 1*10 -3 Pa-30Pa; or / and, The sputtering gas in step 32 is oxygen or a mixture of oxygen and argon; or / and, After the sputtering gas is introduced in step 32, the pressure in the growth chamber is 5*10 -2 Pa.
4. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 3, characterized in that: The thickness of the metal nanoarray in step 33 is 1-10 nm; or / and, The deposition time in step 33 is 95 seconds; or / and, The power of the pulse laser used in step 33 is 300 mW.
5. The method for preparing adjustable localized surface plasmon using a nanoarray according to any one of claims 1 to 4, characterized in that: The semiconductor film prepared in step 2 is prepared by pulsed laser deposition, comprising the following steps: Step 21, fix the cleaned substrate in step 1 to the sample stage of the growth chamber, install the semiconductor target on the target holder, evacuate the vacuum, heat the substrate, and introduce sputtering gas; Step 22: When a laser pulse is focused on the target surface, the target material is instantly evaporated to form a plasma plume containing the target material elements; the plasma plume then rapidly expands in a direction perpendicular to the target surface and is deposited on the substrate surface obtained in step 1 to form a semiconductor film.
6. The method for preparing a high-quality semiconductor single crystal thin film using an array buffer layer according to claim 5, characterized in that: The heating temperature in step 21 is 20°C-800°C; or / and, In step 21, the growth chamber is evacuated to 1*10 -6 Pa, and the vacuum degree is maintained at 1*10 -3 Pa-30Pa; or / and, The sputtering gas in step 21 is oxygen or a mixture of oxygen and argon; or / and, After the sputtering gas is introduced in step 21, the pressure in the growth chamber is 5*10 -2 Pa.
7. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 6, characterized in that: The deposition time in step 22 is 20 min-360 min; or / and, In step 22, the pulse laser power is 300 mW.
8. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 5 or 6, characterized in that: The specific steps of cleaning the substrate in step 1 are: putting the substrate into a beaker, ultrasonically cleaning it with acetone, alcohol, and deionized water for more than 5 minutes to remove organic impurities and residual ions on the substrate, and then blowing it dry with nitrogen or inert gas for standby use; the material of the substrate is single crystal sapphire, single crystal silicon, single crystal gallium oxide, silicon carbide or quartz glass.
9. The method for preparing adjustable localized surface plasmon using nanoarray according to claim 2 or 5, characterized in that: The method for preparing the semiconductor film in step 2 can be replaced by: magnetron sputtering deposition, pulsed laser deposition, molecular beam epitaxy, plasma enhanced chemical vapor deposition, organometallic chemical vapor deposition and the like; Alternatively, the method for preparing the metal nanoarray in step 3 can be replaced by thermal evaporation, electron beam evaporation, magnetron sputtering deposition, pulsed laser deposition, molecular beam epitaxy, plasma enhanced chemical vapor deposition or organometallic chemical vapor deposition.
10. A metal nanoarray, characterized in that: The semiconductor photocurrent is increased by more than 10 times by using the method described in any one of claims 1 to 9; the semiconductor is Ga2O3, zinc oxide, tin dioxide, hafnium oxide, cuprous oxide, aluminum nitride, gallium nitride, boron nitride or indium nitride.