Method and device for chemical displacement gold plating on metal substrate with assistance of laser
By using nanosecond laser-assisted chemical displacement gold plating on stainless steel to remove the passivation film and form a gold film transition layer, the problems of easy coating peeling and complex processes are solved, achieving a highly efficient and environmentally friendly gold plating process.
Patent Information
- Application Number
- CN202411022792.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technologies for gold plating on stainless steel often result in the plating layer easily peeling off, and the process is complex, costly, and requires the use of photoresist, leading to environmental pollution.
Nanosecond laser irradiation is used to irradiate the interface between the workpiece to be gold plated and the ammonium sulfite plating solution. The thermal effect of the laser is used to remove the passivation film and cause it to micro-remelt. The remelted surface undergoes a displacement reaction with Au+ in the plating solution, depositing a gold film and forming a transition layer to improve the adhesion.
It achieves maskless localized gold plating, simplifies the process, improves production efficiency, enhances coating adhesion, and avoids the use of photoresist and environmental pollution.
Smart Images

Figure CN118996409A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of composite processing, and in particular to a method and a device for chemical replacement gold plating on a metal substrate using laser assistance. Background Art
[0002] Gold has excellent electrical and thermal conductivity, corrosion resistance and welding properties. The gold plating is delicate and bright, easy to polish, and has both aesthetics and practicality. It is widely used in semiconductors, machinery manufacturing, instrumentation and decorative lighting.
[0003] In particular, gold is the best coating material for connectors and plugs due to its extremely low contact resistivity and excellent corrosion resistance. Copper, stainless steel and other materials are usually used as the substrate, and then gold is plated to ensure low contact resistance, corrosion resistance and aesthetics. Compared with copper, stainless steel has poorer conductivity but higher strength, and is more suitable for devices with low current, frequent plugging and unplugging, and high connector strength requirements, such as charger plugs, control switches, etc.
[0004] Directly plating gold on stainless steel makes the coating fall off easily. The current process is to first pre-plating Ni on stainless steel as a transition layer, and then plating gold on Ni to ensure the bonding strength of the coating. Usually a mask is used to obtain a localized coating, which requires the use of a photoresist, which not only has poor compatibility with the plating solution, but also pollutes the environment. Whether pre-plating Ni or using a photoresist, the process is more complicated and the cost is increased. Therefore, it is urgent to develop a reliable and simple method for plating stainless steel with gold. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention provides a method and device for chemical replacement gold plating on a metal substrate using laser assistance. The interface between the workpiece to be plated with gold and the ammonium sulfite plating solution is irradiated by nanosecond laser. The thermal effect of the laser can effectively remove the passivation film on the surface of the workpiece to be plated with gold and slightly remelt it. The active metal elements on the remelted surface react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, and a gold film is deposited in the laser irradiated area, while the non-irradiated area is protected by a dense oxide film and does not undergo a replacement reaction, thereby ultimately achieving maskless localized gold plating. In the present invention, the Au replaced during laser irradiation will penetrate into the remelting layer, and the remelting layer acts as a transition layer between the substrate and the gold film, effectively improving the bonding strength of the coating. Therefore, a pre-plated transition layer is no longer required, thereby simplifying the processing technology and improving production efficiency.
[0006] The present invention achieves the above technical objectives through the following technical means.
[0007] A method for chemical replacement gold plating on a metal substrate using laser assistance, using laser underwater irradiation to remove the passivation film on the surface of the workpiece to be plated, and to locally remelt the workpiece to be plated, and the metal elements on the remelted surface react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, thereby depositing a gold layer on the surface of the workpiece to be plated.
[0008] The above scheme specifically includes the following steps:
[0009] Step 1: Build a laser-assisted chemical replacement gold plating processing system on the workpiece to be gold-plated;
[0010] Step 2: Use nanosecond laser to irradiate the interface between the workpiece to be plated and the plating solution. Due to the thermal effect of the laser, the irradiated area is surface activated, specifically removing the surface passivation film and causing the workpiece to be plated to be locally remelted;
[0011] Step 3: After the local remelting, the gold-plated workpiece is heated in a water bath in the original plating solution, or the local remelting workpiece obtained in step 2 is placed in a new plating solution of the same type and heated in a water bath. The metal elements on the surface after activation react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, a gold layer is deposited, and the unactivated area does not react under the barrier of the passivation layer of the workpiece to be gold-plated;
[0012] Step 4: Clean the gold-plated workpiece with deionized water and dry it quickly.
[0013] In the above scheme, the water bath heating temperature is 60-70°C.
[0014] In the above scheme, when the workpiece to be gold-plated is moved after local remelting, the activated surface needs to be isolated from oxygen.
[0015] In the above scheme, the water bath heating time is determined by the required coating thickness, and the maximum thickness of 0.2 μm is reached in 10 minutes.
[0016] In the above scheme, an ammonium sulfite system plating solution is used, wherein HAuCl4 is Au + The source needs to be replenished regularly, with ammonium sulfite as the complexing agent and potassium citrate as the pH stabilizer; or the ammonium sulfite plating solution can be replaced, and the electrode potential of the Au+ complex in the replacement plating solution is higher than the electrode potential of the element of the workpiece to be gold-plated, so that the replacement reaction can occur.
[0017] In the above scheme, the laser scans vertically, the sample is placed horizontally, the laser scanning line spacing is 0.01-0.05mm, the scanning speed is 100-500mm / s, the single pulse energy is 1.5-2.5μJ, the spot pulse frequency is 3000-4000kHz, and the pulse width is 100-300ns.
[0018] In the above scheme, the gold displaced during laser irradiation is remelted together with the workpiece to be gold-plated to form a transition layer between the gold film and the substrate.
[0019] In the above scheme, the workpiece to be gold-plated does not need pretreatment; the workpiece to be gold-plated must be a metal substrate, and the metal substrate can undergo a replacement reaction with the plating solution, and at the same time, there is a dense oxide film on the surface of the metal substrate to ensure the localized processing of the laser.
[0020] A laser-assisted chemical replacement gold plating device on a metal substrate comprises a laser activation system, a motion control system and a chemical deposition system; the laser activation system comprises a computer, a laser, a reflector, a focusing lens, a laser beam, an ammonium sulfite plating solution, a workpiece to be gold-plated and an electrolytic bath; the laser beam emitted by the computer controls the laser to change the optical path through the reflector, and is focused by the focusing lens to irradiate the interface between the ammonium sulfite plating solution and the workpiece to be gold-plated; the motion control system comprises a computer, a motion controller and an xyz three-coordinate mobile platform, the computer controls the motion controller, the motion controller controls the xyz three-coordinate mobile platform, and the xyz three-coordinate mobile platform is provided with an electrolytic bath; the chemical deposition system comprises an ammonium sulfite plating solution, a workpiece to be gold-plated, an electrolytic bath, a water bath medium and a water bath pot; the ammonium sulfite plating solution is placed in the electrolytic bath, the workpiece to be gold-plated is horizontally placed in the ammonium sulfite plating solution, and the electrolytic bath is placed in the water bath pot and heated by the water bath medium.
[0021] Beneficial effects:
[0022] 1. In the method of the present invention, nanosecond laser is used to irradiate the interface between the workpiece to be gold-plated and the ammonium sulfite plating solution. The thermal effect of the laser can effectively remove the passivation film on the surface of the workpiece to be gold-plated and slightly remelt it. The active metal elements on the remelted surface undergo a substitution reaction with Au+ in the plating solution to deposit a gold film. No external current is required and it can be used in electrically sensitive areas.
[0023] 2. In the method of the present invention, laser irradiation is a process of surface activation. The activated surface can replace the gold film, and the non-activated area is protected by the passivation film on the surface of the workpiece, and no replacement reaction occurs. Therefore, maskless localized gold plating can be achieved without being restricted by the compatibility of the photoresist and the plating solution. At the same time, the process is simplified and the environmental pollution caused by the photoresist is reduced.
[0024] 3. In the method of the present invention, part of Au will be mixed with the workpiece to be gold-plated during laser remelting, forming a transition layer between the gold film and the substrate. The presence of the transition layer can effectively improve the adhesion of the gold film, eliminating the process of pre-plating the transition layer.
[0025] 4. In the present invention, the gold displaced during laser irradiation is slightly remelted together with the substrate to form a gold-substrate mixed layer between the gold film and the substrate. The mixed layer plays a role of transition and buffer, effectively improving the adhesion strength of the gold film.
[0026] 5. Since the laser has the function of underwater cleaning, the workpiece to be gold-plated does not require pretreatment.
[0027] 6. Compared with traditional electrodeposition, the method of the present invention does not require photoresist and pre-plated transition layer, has no external current, can be used in electrically sensitive areas, simplifies the existing gold plating process, and provides a new method and idea for the preparation of localized gold plating.
[0028] 7. The method of the present invention utilizes nanosecond laser to irradiate the interface between the workpiece and the gold plating solution. Due to the thermal effect of the laser, the irradiated area is surface activated. The specific process is to remove the surface oxide film and slightly remelt it. The active metal elements in the activated surface react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs and a gold layer is deposited. The unactivated area does not react due to the barrier of the passivation layer, thus achieving maskless localized gold plating. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A schematic diagram of a processing system for laser surface activation steps of laser-assisted chemical replacement gold plating on a metal substrate;
[0030] Figure 2 A schematic diagram of a processing system for chemical displacement gold plating steps of chemical displacement gold plating on a metal substrate using laser assistance;
[0031] Figure 3 The surface morphology of a 3×3 mm localized gold coating prepared by laser-assisted chemical replacement gold plating on stainless steel in Example 2; wherein (a) is a surface morphology of a laser surface activated coating, (b) is a surface morphology of a chemical replacement coating, ① is a laser surface activated area, ③ is a chemical replacement gold plating area, ② and ④ are 316L stainless steel substrates;
[0032] Figure 4 This is a surface morphology of a 3×3 mm localized gold coating prepared by laser-assisted chemical replacement gold plating on Ni in Example 4; wherein ① is the chemical replacement gold plating area, and ② is the Ni substrate;
[0033] Figure 5 This is a surface morphology of Example 5 in which a 3×3 mm localized gold coating was prepared by laser-assisted chemical replacement gold plating on Al; wherein ① is the chemical replacement gold plating area, and ② is the Al substrate.
[0034] Reference numerals:
[0035] 1-computer; 2-laser; 3-reflector; 4-focusing lens; 5-laser beam; 6-ammonium sulfite plating solution; 7-workpiece to be plated with gold; 8-electrolytic cell; 9-motion controller; 10-xyz three-coordinate moving platform; 11-water bath medium; 12-water bath pot. DETAILED DESCRIPTION
[0036] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0037] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "axial", "radial", "vertical", "horizontal", "inner", "outer" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0038] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0039] A method for chemical replacement gold plating on a metal substrate using laser assistance, suitable for a surface protected by a dense oxide film, and the main elements of which can react with Au(SO3)2 in an ammonium sulfite plating solution 3- Materials that undergo substitution reactions, such as Al, Ni, stainless steel, etc.
[0040] Ammonium sulfite plating solution can replace Au in the plating solution + The electrode potential of the complex is higher than that of the element of the workpiece to be plated, so that the replacement reaction can occur.
[0041] The water bath heating temperature is 60-70°C, and the heating time is determined by the required thickness, reaching a maximum thickness of 0.2μm in 10 minutes. The water bath temperature can be greater than 70°C, which can achieve a faster deposition speed, but it requires the risk of solution failure.
[0042] A method for chemical replacement gold plating on a metal substrate using laser assistance, using laser underwater irradiation to remove the passivation film on the surface of the workpiece to be plated, and to locally remelt the workpiece to be plated, and the metal elements on the remelted surface react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, thereby depositing a gold layer on the surface of the workpiece to be plated.
[0043] The above scheme specifically includes the following steps:
[0044] Step 1: Build a laser-assisted chemical replacement gold plating processing system on the workpiece to be gold-plated;
[0045] Step 2: Use nanosecond laser to irradiate the interface between the workpiece to be plated and the plating solution. Due to the thermal effect of the laser, the irradiated area is surface activated, specifically removing the surface passivation film and causing the workpiece to be plated to be locally remelted;
[0046] Step 3: After the local remelting, the gold-plated workpiece is heated in a water bath in the original plating solution, or the local remelting workpiece obtained in step 2 is placed in a new plating solution of the same type and heated in a water bath. The metal elements on the surface after activation react with Au(SO3)2 in the plating solution. 3 - A replacement reaction occurs, a gold layer is deposited, and the unactivated area does not react under the barrier of the passivation layer of the workpiece to be gold-plated;
[0047] Step 4: Clean the gold-plated workpiece with deionized water and dry it quickly.
[0048] The water bath heating temperature is 60-70°C.
[0049] When the workpiece to be plated is moved after local remelting, the activated surface needs to be isolated from oxygen.
[0050] The water bath heating time depends on the required coating thickness, and the maximum thickness of 0.2μm is reached in 10 minutes.
[0051] Use ammonium sulfite system plating solution, where HAuCl4 is Au + Source, needs to be replenished regularly, ammonium sulfite is the complexing agent, potassium citrate is the pH stabilizer; or replace the ammonium sulfite plating solution, replace the Au in the plating solution + The electrode potential of the complex is higher than that of the element of the workpiece to be plated, so that the replacement reaction can occur.
[0052] The laser scans vertically, the sample is placed horizontally, the laser scanning line spacing is 0.01-0.05mm, the scanning speed is 100-500mm / s, the single pulse energy is 1.5-2.5μJ, the spot pulse frequency is 3000-4000kHz, and the pulse width is 100-300ns.
[0053] The gold displaced during laser irradiation is remelted together with the workpiece to be gold-plated, forming a transition layer between the gold film and the substrate.
[0054] The workpiece to be gold-plated does not require pretreatment; the workpiece to be gold-plated must be a metal substrate, and the metal substrate can undergo a replacement reaction with the plating solution, and at the same time, a dense oxide film is present on the surface of the metal substrate to ensure the localized processing of the laser.
[0055] A device for chemical replacement gold plating on a metal substrate using laser assistance, comprising a laser activation system, a motion control system and a chemical deposition system; the laser activation system comprises a computer 1, a laser 2, a reflector 3, a focusing lens 4, a laser beam 5, an ammonium sulfite plating solution 6, a workpiece to be gold plated 7, and an electrolytic cell 8; the computer 1 controls the laser beam emitted by the laser 2 to change the optical path through the reflector 3, and to be focused by the focusing lens 4 and then irradiate to the interface between the ammonium sulfite plating solution 6 and the workpiece to be gold plated 7; the motion control system comprises a computer 1, a motion controller 9 , an xyz three-coordinate mobile platform 10, the computer 1 controls a motion controller 9, the motion controller 9 controls the xyz three-coordinate mobile platform 10, an electrolytic cell 8 is placed on the xyz three-coordinate mobile platform 10; the chemical deposition system comprises an ammonium sulfite plating solution 6, a workpiece to be gold-plated 7, an electrolytic cell 8, a water bath medium 11, and a water bath pot 12; the ammonium sulfite plating solution 6 is placed in the electrolytic cell 8, the workpiece to be gold-plated 7 is horizontally placed in the ammonium sulfite plating solution 6, the electrolytic cell 8 is placed in the water bath pot 12, and is heated by the water bath medium 11.
[0056] Comparative Example 1
[0057] A method for chemical replacement gold plating on 316L stainless steel using laser assistance, the specific implementation steps are as follows:
[0058] Laser-assisted surface activation: A 316L stainless steel sheet of 10×10×0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 0.5 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0059] Chemical replacement gold plating: The stainless steel sheet after laser-assisted surface activation is transferred to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the stainless steel sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0060] A trace amount of gold appeared in the laser irradiated area, and no gold was deposited in the unirradiated area.
[0061] Comparative Example 2
[0062] A method for chemical replacement gold plating on 316L stainless steel using laser assistance, the specific implementation steps are as follows:
[0063] Laser-assisted surface activation: A 316L stainless steel sheet of 10×10×0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically, with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 1 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns;
[0064] Chemical replacement gold plating: The stainless steel sheet after laser-assisted surface activation is transferred to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the stainless steel sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0065] A small amount of gold appeared in the laser irradiated area, and no gold was deposited in the unirradiated area.
[0066] Example 1
[0067] A method for chemical replacement gold plating on 316L stainless steel using laser assistance, the specific implementation steps are as follows:
[0068] Laser-assisted surface activation: A 316L stainless steel sheet of 10×10×0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 1.5 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0069] Chemical replacement gold plating: The stainless steel sheet after laser-assisted surface activation is transferred to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the stainless steel sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0070] A bright, continuous gold film appears in the laser irradiated area, with a small amount of defects on the surface of the gold film, and no gold is deposited in the non-irradiated area.
[0071] Example 2
[0072] A method for chemical replacement gold plating on 316L stainless steel using laser assistance, the specific implementation steps are as follows:
[0073] Laser-assisted surface activation: A 316L stainless steel sheet of 10 × 10 × 0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 2 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0074] Chemical replacement gold plating: The stainless steel sheet after laser-assisted surface activation is transferred to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the stainless steel sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0075] A bright, continuous, and dense gold film appeared in the laser irradiated area, and no gold was deposited in the unirradiated area.
[0076] Example 3
[0077] A method for chemical replacement gold plating on 316L stainless steel using laser assistance, the specific implementation steps are as follows:
[0078] Laser-assisted surface activation: A 316L stainless steel sheet of 10 × 10 × 0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 2.5 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0079] Chemical replacement gold plating: The stainless steel sheet after laser-assisted surface activation is transferred to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the stainless steel sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0080] A bright, continuous gold film appears in the laser irradiated area. There are etching marks on the surface of the gold film. The boundary of the gold film is blurred and the localization is poor. There is no gold deposition in the non-irradiated area.
[0081] Example 4
[0082] A method for chemical replacement gold plating on Ni using laser assistance, the specific implementation steps are as follows:
[0083] Laser-assisted surface activation: A Ni sheet of 10 × 10 × 0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 2 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0084] Chemical replacement gold plating: transfer the Ni sheet after laser-assisted surface activation to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the Ni sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0085] A bright, continuous, and dense gold film appeared in the laser irradiated area, and no gold was deposited in the unirradiated area.
[0086] Example 5
[0087] A method for chemical replacement gold plating on Al using laser assistance, the specific implementation steps are as follows:
[0088] Laser-assisted surface activation: an Al sheet of 10 × 10 × 0.2 mm was placed horizontally in an ammonium sulfite plating solution, and the laser was irradiated vertically with a scanning line spacing of 10 μm, a scanning speed of 300 mm / s, a single pulse energy of 2 μJ, a pulse frequency of 4000 kHz, and a pulse width of 150 ns.
[0089] Chemical replacement gold plating: Transfer the Al sheet after laser-assisted surface activation to a new ammonium sulfite plating solution, which has been preheated in a water bath. During the transfer, the Al sheet is kept horizontal, and the water film on the surface is used to isolate oxygen and transfer quickly. Then heat in a 70°C water bath for 5 minutes.
[0090] A bright, continuous, and dense gold film appeared in the laser irradiated area, and no gold was deposited in the unirradiated area.
[0091] Table 1 shows the coating formation after the single pulse energy, pulse frequency and pulse width values act on the stainless steel substrate
[0092]
[0093]
[0094] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0095] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A method for chemical replacement gold plating on a metal substrate using laser assistance, characterized in that: Laser irradiation is used to remove the passivation film on the surface of the workpiece to be plated, and the workpiece to be plated is locally remelted. The metal elements on the remelted surface react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, thereby depositing a gold layer on the surface of the workpiece to be plated.
2. The method for laser-assisted chemical replacement gold plating on a metal substrate according to claim 1, characterized in that: The specific steps include: Step 1: Build a laser-assisted chemical replacement gold plating processing system on the workpiece to be gold-plated; Step 2: Use nanosecond laser to irradiate the interface between the workpiece to be plated and the plating solution. Due to the thermal effect of the laser, the irradiated area is surface activated, specifically removing the surface passivation film and causing the workpiece to be plated to be locally remelted; Step 3: After the local remelting, the gold-plated workpiece is heated in a water bath in the original plating solution, or the local remelting workpiece obtained in step 2 is placed in a new plating solution of the same type and heated in a water bath. The metal elements on the surface after activation react with Au(SO3)2 in the plating solution. 3- A replacement reaction occurs, a gold layer is deposited, and the unactivated area does not react under the barrier of the passivation layer of the workpiece to be gold-plated; Step 4: Clean the gold-plated workpiece with deionized water and dry it quickly.
3. The method for laser-assisted chemical replacement gold plating on a metal substrate according to claim 2, characterized in that: The water bath heating temperature is 60-70°C.
4. The method for laser-assisted chemical replacement gold plating on a metal substrate according to claim 2, characterized in that: When the workpiece to be plated is moved after local remelting, the activated surface needs to be isolated from oxygen.
5. The method for laser-assisted chemical replacement gold plating on a metal substrate according to claim 2, characterized in that: The water bath heating time depends on the required coating thickness, and the maximum thickness of 0.2μm is reached in 10 minutes.
6. The method for laser-assisted chemical replacement gold plating on a metal substrate according to any one of claims 1 to 5, characterized in that: Use ammonium sulfite system plating solution, where HAuCl4 is Au + Source, needs to be replenished regularly, ammonium sulfite is the complexing agent, potassium citrate is the pH stabilizer; or replace the ammonium sulfite plating solution, replace the Au in the plating solution + The electrode potential of the complex is higher than that of the element of the workpiece to be plated, so that the replacement reaction can occur.
7. The method for laser-assisted chemical replacement gold plating on a metal substrate according to any one of claims 1 to 5, characterized in that: The laser scans vertically, the sample is placed horizontally, the laser scanning line spacing is 0.01-0.05mm, the scanning speed is 100-500mm / s, the single pulse energy is 1.5-2.5μJ, the spot pulse frequency is 3000-4000kHz, and the pulse width is 100-300ns.
8. The method for laser-assisted chemical replacement gold plating on a metal substrate according to any one of claims 1 to 5, characterized in that: The gold displaced during laser irradiation is remelted together with the workpiece to be gold-plated, forming a transition layer between the gold film and the substrate.
9. The method for laser-assisted chemical replacement gold plating on a metal substrate according to any one of claims 1 to 5, characterized in that: The workpiece to be gold-plated does not require pretreatment; the workpiece to be gold-plated must be a metal substrate, and the metal substrate can undergo a replacement reaction with the plating solution, and at the same time, a dense oxide film is present on the surface of the metal substrate to ensure the localized processing of the laser.
10. A device for the method of laser-assisted chemical replacement gold plating on a metal substrate according to any one of claims 1 to 5, characterized in that: It comprises a laser activation system, a motion control system and a chemical deposition system; the laser activation system comprises a computer, a laser, a reflector, a focusing lens, a laser beam, an ammonium sulfite plating solution, a workpiece to be gold-plated and an electrolytic cell; the laser beam emitted by the computer controls the laser to change the optical path through the reflector, and is focused by the focusing lens and then irradiated to the interface between the ammonium sulfite plating solution and the workpiece to be gold-plated; the motion control system comprises a computer, a motion controller and an xyz three-coordinate moving platform, the computer controls the motion controller, the motion controller controls the xyz three-coordinate moving platform, and the electrolytic cell is placed on the xyz three-coordinate moving platform; the chemical deposition system comprises an ammonium sulfite plating solution, a workpiece to be gold-plated, an electrolytic cell, a water bath medium and a water bath pot; the ammonium sulfite plating solution is placed in the electrolytic cell, the workpiece to be gold-plated is horizontally placed in the ammonium sulfite plating solution, the electrolytic cell is placed in the water bath pot and heated by the water bath medium.