Method for preparing M-RuO2 nanoparticles through vapor deposition
Through the optimization of conditions by vapor deposition method, M-RuO2 nanoparticles without surfactant were prepared, which solved the low amplification ability and pollution problems of the preparation of RuO2 nanocatalysts in the prior art, and achieved efficient and economical catalyst production and excellent acidity OER reaction performance.
Patent Information
- Application Number
- CN202410932098.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art When preparing RuO2 nanocatalysts, the liquid phase method has low amplification capability and requires the use of organic surfactants, resulting in contamination and high production costs, making it difficult to be suitable for large-scale production and economicalization.
By using the vapor deposition method, M-RuO2 nanoparticles without surfactants were prepared by optimizing reduction and oxidation conditions and deposition kinetic parameters, and 48 metal elements doped with Ru, achieving simple and efficient alloy particle synthesis.
It has achieved a large-scale mass-produced M-RuO2 nanoalloy particles with no surfactant and low cost, which significantly improves catalytic activity and stability, and is suitable for acidic electrocatalytic water decomposition reactions.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing M-RuO2 nanoparticles by a vapor deposition method, belonging to the technical field of nano material preparation. Background Art
[0002] To date, RuO2 is one of the most advanced electrocatalysts for acidic OER, but ruthenium monometallic oxides will generate soluble RuO4 during the acidic OER reaction. The incorporation of other elements to form alloys can effectively adjust the intrinsic electronic structure of the catalyst and optimize the adsorption energy of the reaction intermediates, thereby enhancing the electrocatalytic performance of RuO2.
[0003] At present, the synthesis of nanocatalysts mainly adopts liquid phase method, which has low scale-up ability and is not suitable for large-scale production of ruthenium-based nanocatalysts. In addition, most synthesis methods require the use of organic surfactants to control the particle size, but this will undoubtedly contaminate the catalyst surface, so careful cleaning is required before use to make the nanoalloy particles catalytically active. The complex synthesis and contaminant removal process increases the production cost, making these technologies economically unfeasible.
[0004] In recent years, chemical vapor deposition (CVD) has been widely regarded as an advanced technology for growing nanomaterials. It can use gas or steam to prepare morphology-controlled metal nanomaterials at lower temperatures and over larger areas, showing great development potential in the field of electrocatalytic oxygen evolution reaction. Summary of the invention
[0005] The present invention aims to provide a method for preparing M-RuO2 nanoparticles by vapor deposition, and synthesizes a series of M-RuO2 nanoparticles without surfactant by optimizing reduction and oxidation conditions and deposition kinetic parameters.
[0006] The implementation process of the present invention is as follows: A method for preparing M-RuO2 nanoparticles by vapor deposition comprises the following steps: (1) dissolving ruthenium acetylacetonate and acetylacetonate of metal M in a molar ratio of Ru:M=12:1 to 6:4 in a polar organic solvent, and removing the organic solvent to obtain a mixed precursor, wherein M is selected from Li, Mg, Ca, Ba, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Ag, Cd, Hf, Ta, W, Re, Rh, Pd, Ir, Pt, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Al, Ga, In, Sn, Pb, Bi; (2) In a reducing gas H2 / Ar, the mixed precursor is vapor deposited at 300-500°C to obtain M-Ru nanoparticles; (3) The M-Ru nanoparticles are partially oxidized at a temperature of 100 to 500 °C to obtain M-RuO2 nanoparticles.
[0007] In the above step (1), the polar organic solvent is selected from acetone, methanol, ethanol, ether, ethyl acetate, chloroform or glacial acetic acid.
[0008] The M-RuO2 nanoparticles prepared by the above method are used in acidic electrocatalytic water decomposition.
[0009] Beneficial effects of the present invention: The present invention can obtain M-RuO2 nano alloy particles through simple deposition loading and calcination. It is a scalable, surfactant-free, low-cost solid chemical synthesis method. 48 metal elements are selected to be doped with Ru respectively to successfully prepare M-RuO2 nano particles, indicating that the method has universal applicability. No surfactant is required in the synthesis process, and large-scale mass production can be achieved. The present invention provides a simple and efficient new method for preparing M-RuO2 nano alloy particles, and shows excellent activity and stability in the field of catalytic acidic OER reactions. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 is a TEM image of Zn-RuO2 nanoparticles in Example 1; Figure 2 Is the OER performance test diagram of Zn-RuO2 nanoparticles in Example 1 (CV and chronoamperometric test); Figure 3 Is the OER performance test diagram of Pt-RuO2 nanoparticles in Example 2 (CV and chronoamperometric test); Figure 4 Is the OER performance test diagram of Sm-RuO2 nanoparticles in Example 3 (CV and chronoamperometric test); Figure 5 Example 4 is the OER performance test diagram of Sn-RuO2 nanoparticles (CV and chronoamperometric test); Figure 6 Is the OER performance test diagram of V-RuO2 nanoparticles in Example 5 (CV and chronoamperometric test); Figure 7 It is a summary of the electrochemical test results of M-RuO2 nanoparticles (mass activity and stability slope). DETAILED DESCRIPTION
[0011] The technical solution of the present invention is further described below with reference to specific embodiments, but the protection scope of the present invention is not limited thereto.
[0012] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be purchased commercially. Example 1
[0013] Weigh 50 mg Ru(acac)3 and 14.18 mg Zn(acac)2 and dissolve them in 2 ml acetone. Ultrasonicate for 20 min to completely dissolve the precursor. Place the mixed solution in a vacuum oven at 50 ºC to evaporate the acetone for later use. Place the dried powder in a quartz boat and calcine it in a tube furnace with a reducing gas H2 / Ar at a temperature of 400 ºC and a heating rate of 10 ºC·min -1 , the gas flow rate was 20 sccm, and the holding time was 1 h.
[0014] The reduced Zn-Ru nanoparticles were partially oxidized. 20 mg of Zn-Ru powder was weighed and placed in a quartz boat. O2 was introduced into a tube furnace for calcination at a temperature of 300 ºC and a heating rate of 1 ºC·min -1 , gas flow rate is 20sccm, and the holding time is 1 h to obtain Zn-RuO2 nanoparticles. Figure 1 TEM image of Zn-RuO2 nanoparticles. Figure 2 LSV and chronoamperometric curves of Zn-RuO2 nanoparticles.
[0015] The ICP results of Zn-RuO2 were: Ru: 31.58 ppb, Zn: 119.17 ppb Example 2
[0016] Weigh 50 mg Ru(acac)3 and 21.16 mg Pt(acac)2 and dissolve them in 2 ml ethanol. Ultrasonicate for 20 min to completely dissolve the precursor. Place the mixed solution in a vacuum oven at 50 ºC to evaporate the acetone for later use. Place the dried powder in a quartz boat and calcine it in a tube furnace with a reducing gas H2 / Ar at a temperature of 400 ºC and a heating rate of 10 ºC·min -1 , the gas flow rate was 20 sccm, and the holding time was 1 h.
[0017] The reduced Pt-Ru nanoparticles were partially oxidized. 20 mg of Pt-Ru powder was weighed and placed in a quartz boat. O2 was introduced into a tube furnace for calcination at a temperature of 300 °C and a heating rate of 1 °C·min -1 , gas flow rate is 20sccm, and the holding time is 1 h to obtain Pt-RuO2 nanoparticles. Figure 3 LSV curve of Pt-RuO2 nanoparticles.
[0018] The ICP results of Pt-RuO2 were: Ru: 12.76 ppb, Pt: 80.42 ppb. Example 3
[0019] Weigh 50 mg of Ru(acac)3 and 24.08 mg of Sm(acac)3 and dissolve them in 1 ml of ether. Ultrasonicate for 20 min to completely dissolve the precursor. Place the mixed solution in a vacuum oven at 50 ºC to evaporate the acetone for later use. Place the dried powder in a quartz boat and calcine it in a tube furnace with a reducing gas H2 / Ar at a temperature of 400 ºC and a heating rate of 10 ºC·min -1 , the gas flow rate was 20 sccm, and the holding time was 1 h.
[0020] The reduced Sm-Ru nanoparticles were partially oxidized. 20 mg of Sm-Ru powder was weighed and placed in a quartz boat. O2 was introduced into a tube furnace for calcination at a temperature of 350 ºC and a heating rate of 1 ºC·min -1 , gas flow rate is 20sccm, and the holding time is 1 h to obtain Sm-RuO2 nanoparticles. Figure 4 LSV curve of Sm-RuO2 nanoparticles.
[0021] The ICP results of Sm-RuO2 were: Ru: 5.17 ppb, Sm: 107.3 ppb. Example 4
[0022] Weigh 50 mg Ru(acac)3 and 9.94 mg Sn(acac)2 and dissolve them in 1 ml acetone. Ultrasonicate for 20 min to completely dissolve the precursor. Place the mixed solution in a vacuum oven at 50 ºC to evaporate the acetone for later use. Place the dried powder in a quartz boat and calcine it in a tube furnace with reducing gas H2 / Ar at 400 ºC and a heating rate of 10 ºC·min. -1 , the gas flow rate was 20 sccm, and the holding time was 1 h.
[0023] The reduced Sn-Ru nanoparticles were partially oxidized. 20 mg of Sn-Ru powder was weighed and placed in a quartz boat. O2 was introduced into a tube furnace for calcination at a temperature of 300 ºC and a heating rate of 1 ºC·min. -1 , gas flow rate is 20sccm, and holding time is 1 h to obtain In-RuO2 nanoparticles. Figure 5 LSV curve of Sn-RuO2 nanoparticles.
[0024] The ICP results of Sn-RuO2 were: Ru: 4.83 ppb, Sn: 626.155 ppb. Example 5
[0025] Weigh 50 mg Ru(acac)3 and 4.85 mg V(acac)3 and dissolve them in 1 ml chloroform. Ultrasonicate for 20 min to completely dissolve the precursor. Place the mixed solution in a vacuum oven at 50 ºC to evaporate the acetone for later use. Place the dried powder in a quartz boat and calcine it in a tube furnace with reducing gas H2 / Ar at 400 ºC and a heating rate of 10 ºC·min -1 , the gas flow rate was 20 sccm, and the holding time was 1 h.
[0026] The reduced V-Ru nanoparticles were partially oxidized. 20 mg of V-Ru powder was weighed and placed in a quartz boat. O2 was introduced into a tube furnace for calcination at a temperature of 300 °C and a heating rate of 1 °C·min. -1 , gas flow rate is 20sccm, and the holding time is 1 h to obtain V-RuO2 nanoparticles. Figure 6 LSV curve of V-RuO2 nanoparticles.
[0027] The ICP results of V-RuO2 were: Ru: 12.94 ppb, V: 1.36 ppb.
[0028] Figure 7 The radar chart shows the summary of electrochemical test results of M-RuO2 nanoparticles. The radar chart shows that the mass activity of Sn-RuO2, Hf-RuO2 and W-RuO2 samples exceeds 3.5 A‧mg -1 The mass activity of Cu-RuO2, Zr-RuO2, Mo-RuO2, Bi-RuO2, Ce-RuO2, Nd-RuO2, Tb-RuO2, and Ho-RuO2 samples reached 3 A‧mg -1At the same time, the stability of RuO2 is significantly improved after doping with elements such as Mg / Al / Mn / Co / Ni / Cd / In / Sn / Re / Pb / Sm / Gd / Dy / Tm / Yb / Lu (a slope lower than 1 is considered to be more stable than RuO2, and the lower the slope, the better the stability).
Claims
1. Preparation of M-RuO by Vapor Deposition 2 Nanoparticle method, Features The following steps are involved: (1) dissolving ruthenium acetylacetonate and acetylacetonate of metal M in a molar ratio of Ru:M=12:1 to 6:4 in a polar organic solvent, and removing the organic solvent to obtain a mixed precursor, wherein M is selected from Li, Mg, Ca, Ba, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Zr, Nb, Mo, Ag, Cd, Hf, Ta, W, Re, Rh, Pd, Ir, Pt, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Al, Ga, In, Sn, Pb, Bi; (2) In the reducing gas H 2 / Ar, vapor depositing the mixed precursor at 300-500 ºC to obtain M-Ru nanoparticles; (3) Partially oxidize the M-Ru nanoparticles at a temperature of 100-500 °C to obtain M-RuO 2 Nanoparticles.
2. M-RuO according to claim 1 2 Nanoparticle method, Features: The polar organic solvent is selected from acetone, methanol, ethanol, ether, ethyl acetate, chloroform or glacial acetic acid.
3. The method of claim 1 is used to prepare M-RuO 2 Nanoparticles.
4. M-RuO according to claim 3 2 Application of nanoparticles in acidic electrocatalytic water splitting.
Citation Information
Cited By
Preparation method and application of Gd-doped rutile ruthenium dioxide nanosheet
CN119663364A