Electrolytic corrosion liquid as well as preparation method and application thereof

By using electrolytic corrosion liquid prepared by phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol, the problems of harmful components and limited application scope in the existing electrolytic corrosion liquid are solved, and safe and efficient residual stress detection is achieved.

CN118996593APending Publication Date: 2024-11-22DONGFENG MOTOR GRP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948133.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing electrolytic corrosion liquid contains the high carcinogen hexavalent chromium and the strong oxidant chromium anhydride, which poses personal safety risks. Most electrolytic corrosion liquids are only suitable for specific fields and cannot meet the residual stress detection needs at different depths.

Method used

The composition of an electrolytic corrosion solution is provided, including phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol. It is prepared by a specific concentration ratio to form an electrolytic corrosion solution without harmful components, ensuring high conductivity and pH close to neutrality, avoiding Local corrosion and gas bubbling are suitable for residual stress detection at different depths.

Benefits of technology

The electrolytic corrosion liquid is non-toxic and odorless, safe to use, has high conductivity, avoids local corrosion and gas bubbling, ensures that the surface of the electrolytic corrosion pit is flat and bright, and is suitable for the residual stress detection of most metals, reducing the safety of testers risk.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996593A_ABST
    Figure CN118996593A_ABST
Patent Text Reader

Abstract

The invention relates to electrolytic corrosion liquid as well as a preparation method and application thereof, and belongs to the technical field of electrolytic corrosion. The electrolytic corrosion liquid is composed of phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerin and the like and does not contain components harmful to the human body, in the components, phosphoric acid belongs to medium-strong acid, is nontoxic and odorless and does not generate strong corrosion reaction on most metals, and after sodium hydroxide is added for neutralization, the pH value of the prepared electrolytic corrosion liquid is close to neutral; the paint is not easy to volatilize at room temperature, and can protect the safety of testers. During electrolytic corrosion, the solution contains a large amount of PO4 < 3->, SO4 < 2->, Na < + > and Cu < 2 + >, so that the conductivity of the electrolytic corrosion solution is ensured. Moreover, due to the addition of glycerol, local preferential corrosion of tip protrusions on the surfaces of the parts is avoided, the surfaces of electrolytic corrosion pits obtained through electrolytic corrosion are smoother and brighter, meanwhile, the effect of removing and avoiding hydrogen in electrolyte is achieved, and the situation that the corrosion effect is affected by bubbling during electrolytic corrosion is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrolytic corrosion technology, and in particular to an electrolytic corrosion solution and a preparation method and application thereof. Background Art

[0002] Electrolytic corrosion technology is widely used in the fields of metal surface treatment, metallographic grain boundary corrosion observation, etc. Different electrolytic corrosion solutions are used for different application scenarios and materials. For example, in the surface treatment of metal parts, in addition to the chemical properties such as conductivity, the performance of the electrolytic corrosion solution also pays attention to properties such as viscosity; for metallographic grain boundary observation, its electrolytic corrosion performance is a point of particular concern.

[0003] Taking gears as an example, the residual stress on the surface of its parts has a great influence on the performance. At the same time, the technical requirements for residual stress at different depths of gears are also different. When testing the residual stress at different depths of gears, electrolytic corrosion technology can be used to prepare residual stress test samples at different depths of gears. The electrolytic corrosion liquid has a great influence on the effect of electrolytic corrosion. Most of the existing electrolytic corrosion liquids are only applicable to a specific technical field, and most of them contain highly carcinogenic substances such as hexavalent chromium and strong oxidants such as chromic anhydride, which pose a high personal safety risk to users. Summary of the invention

[0004] The present application provides an electrolytic corrosion solution and a preparation method and application thereof, so as to improve the problem that the current electrolytic corrosion solution contains harmful components.

[0005] In a first aspect, the present application provides an electrolytic corrosion solution, the components of which include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and a solvent.

[0006] As an optional implementation manner, the mass concentration of the phosphoric acid is 83% to 90%.

[0007] As an optional embodiment, each 100 mL of the electrolytic corrosion solution includes 10 mL to 12 mL of the phosphoric acid; and / or

[0008] Each 100 mL of the electrolytic corrosion solution includes 22 g to 26 g of sodium hydroxide; and / or

[0009] Each 100 mL of the electrolytic corrosion solution includes 15 g to 20 g of copper sulfate pentahydrate; and / or

[0010] Every 100 mL of the electrolytic corrosion solution includes 6 g to 9 g of glycerol.

[0011] As an optional embodiment, each 100 mL of the electrolytic corrosion solution includes 10.5 mL to 11.5 mL of the phosphoric acid; and / or

[0012] Each 100 mL of the electrolytic corrosion solution includes 23 g to 25 g of sodium hydroxide; and / or

[0013] Each 100 mL of the electrolytic corrosion solution includes 16 g to 19 g of copper sulfate pentahydrate; and / or

[0014] Every 100 mL of the electrolytic corrosion solution includes 7 g to 8 g of glycerol.

[0015] As an optional embodiment, each 100 mL of the electrolytic corrosion solution includes 10.8 mL to 11.2 mL of the phosphoric acid; and / or

[0016] Each 100 mL of the electrolytic corrosion solution includes 23.5 g to 24.5 g of sodium hydroxide; and / or

[0017] Each 100 mL of the electrolytic corrosion solution includes 17 g to 18 g of copper sulfate pentahydrate; and / or

[0018] Every 100 mL of the electrolytic corrosion solution includes 7.3 g to 7.7 g of glycerol.

[0019] As an optional embodiment, the solvent includes water.

[0020] In a second aspect, the present application provides a method for preparing an electrolytic corrosion solution, the method comprising:

[0021] Phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol are mixed in a solvent to obtain an electrolytic etching solution.

[0022] As an optional embodiment, the step of mixing phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol in a solvent to obtain an electrolytic corrosion solution comprises:

[0023] mixing phosphoric acid with a portion of the solvent to obtain a first solution;

[0024] dissolving sodium hydroxide in the first solution to obtain a second solution;

[0025] dissolving copper sulfate pentahydrate in the second solution to obtain a third solution;

[0026] Mixing the third solution and glycerol to obtain a fourth solution;

[0027] The fourth solution is diluted with the remaining solvent to obtain an electrolytic corrosion solution.

[0028] In a third aspect, the present application provides a method for detecting residual stress of a component, the method comprising:

[0029] The electrolytic corrosion liquid is used to electrolytically corrode the component to obtain a plurality of corrosion pits of different depths;

[0030] The residual stress test is performed on the plurality of corrosion pits.

[0031] As an optional embodiment, the component has a protrusion; and / or

[0032] The member comprises a gear; and / or

[0033] The component is composed of medium and low alloy steel; and / or

[0034] The mass content of alloy elements in the composition of the component is ≤10%.

[0035] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0036] The electrolytic corrosion solution provided in the embodiment of the present application is composed of phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol, etc., and does not contain any ingredients harmful to the human body. Among these ingredients, phosphoric acid itself is a medium-strong acid, non-toxic, odorless, and does not produce strong corrosion reactions on most metals. After being neutralized by adding sodium hydroxide, the pH of the prepared electrolytic corrosion solution is close to neutral, and it is not easy to volatilize at room temperature, which can protect the safety of test personnel. When electrolytic corrosion is carried out, the solution contains a large amount of PO4 3- 、SO4 2- 、Na + , Cu 2+ , ensuring the conductivity of the electrolytic corrosion solution. In addition, the addition of glycerol avoids the local preferential corrosion of the tip protrusions on the surface of the parts, making the surface of the electrolytic corrosion pits obtained by electrolytic corrosion smoother and brighter. It also has the function of removing and avoiding hydrogen in the electrolyte, avoiding bubbling during electrolytic corrosion that affects the corrosion effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0039] Figure 1 A flowchart of the method provided in the embodiment of the present application. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0041] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0042] An embodiment of the present application provides an electrolytic corrosion solution, the components of which include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and a solvent.

[0043] The electrolytic corrosion solution is composed of phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol, etc., and does not contain any ingredients that are harmful to the human body. Among these ingredients, phosphoric acid itself is a medium-strong acid, non-toxic, odorless, and does not produce strong corrosion reactions on most metals. After being neutralized by adding sodium hydroxide, the pH of the prepared electrolytic corrosion solution is close to neutral, and it is not easy to volatilize at room temperature, which can protect the safety of the test personnel. When electrolytic corrosion is carried out, the solution contains a large amount of PO4 3- 、SO4 2- 、Na + , Cu 2+ , ensuring the conductivity of the electrolytic corrosion solution. In addition, the addition of glycerol avoids the local preferential corrosion of the tip protrusions on the surface of the parts, making the surface of the electrolytic corrosion pits obtained by electrolytic corrosion smoother and brighter. It also has the function of removing and avoiding hydrogen in the electrolyte, avoiding bubbling during electrolytic corrosion that affects the corrosion effect.

[0044] In some embodiments, the mass concentration of the phosphoric acid is 83% to 90%. Exemplarily, the mass concentration of the phosphoric acid can be 83%, 84%, 85%, 86%, 87%, 88%, 89% or 90%, etc., and can also be any value within the range of 83% to 90%.

[0045] In some embodiments, every 100 mL of the electrolytic corrosion solution includes 10 mL to 12 mL of the phosphoric acid; every 100 mL of the electrolytic corrosion solution includes 22 g to 26 g of sodium hydroxide; every 100 mL of the electrolytic corrosion solution includes 15 g to 20 g of copper sulfate pentahydrate; and every 100 mL of the electrolytic corrosion solution includes 6 g to 9 g of glycerol.

[0046] Furthermore, every 100 mL of the electrolytic corrosion solution includes 10.5 mL to 11.5 mL of the phosphoric acid; every 100 mL of the electrolytic corrosion solution includes 23 g to 25 g of sodium hydroxide; every 100 mL of the electrolytic corrosion solution includes 16 g to 19 g of copper sulfate pentahydrate; and every 100 mL of the electrolytic corrosion solution includes 7 g to 8 g of glycerol.

[0047] Furthermore, every 100 mL of the electrolytic corrosion solution includes 10.8 mL to 11.2 mL of the phosphoric acid; every 100 mL of the electrolytic corrosion solution includes 23.5 g to 24.5 g of sodium hydroxide; every 100 mL of the electrolytic corrosion solution includes 17 g to 18 g of copper sulfate pentahydrate; and every 100 mL of the electrolytic corrosion solution includes 7.3 g to 7.7 g of glycerol.

[0048] Exemplarily, the amount of phosphoric acid in each 100 mL of electrolytic corrosion solution can be 10 mL, 10.2 mL, 10.4 mL, 10.6 mL, 10.8 mL, 11 mL, 11.2 mL, 11.4 mL, 11.6 mL, 11.8 mL or 12 mL, etc., and it can also be any value in the range of 10 mL to 12 mL. The amount of sodium hydroxide in each 100 mL of electrolytic corrosion solution can be 22 g, 22.2 g, 22.4 g, 22.6 g, 22.8 g, 23 g, 23.2 g, 23.4 g, 23.6 g, 23.8 g, 24 g, 24.2 g, 24.4 g, 24.6 g, 24.8 g, 25 g, 25.2 g, 25.4 g, 25.6 g, 25.8 g or 26 g, etc., and it can also be any value in the range of 22 g to 26 g. The amount of copper sulfate pentahydrate in each 100 mL of the electrolytic corrosion solution can be 15 g, 15.5 g, 16 g, 16.5 g, 17 g, 17.5 g, 18 g, 18.5 g, 19 g, 19.5 g or 20 g, etc., and can also be any value in the range of 15 g to 20 g. The amount of glycerol in each 100 mL of the electrolytic corrosion solution can be 6 g, 6.5 g, 7 g, 7.5 g, 8 g, 8.5 g or 9 g, etc., and can also be any value in the range of 6 g to 9 g.

[0049] In some embodiments, the solvent comprises water.

[0050] Figure 1 A flow chart of the method provided in the embodiment of the present application is as follows: Figure 1 As shown, based on a general inventive concept, an embodiment of the present application also provides a method for preparing an electrolytic corrosion solution, the method comprising: mixing phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol in a solvent to obtain an electrolytic corrosion solution.

[0051] The method is used to prepare the above-mentioned electrolytic corrosion solution. The specific content of the electrolytic corrosion solution can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.

[0052] In some embodiments, the step of mixing phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol in a solvent to obtain an electrolytic corrosion solution comprises:

[0053] S1. mixing phosphoric acid with a portion of the solvent to obtain a first solution;

[0054] S2. dissolving sodium hydroxide in the first solution to obtain a second solution;

[0055] S3. dissolving copper sulfate pentahydrate in the second solution to obtain a third solution;

[0056] S4. mixing the third solution and glycerol to obtain a fourth solution;

[0057] S5. Using the remaining solvent to dilute the fourth solution to obtain an electrolytic corrosion solution.

[0058] Specifically, in this embodiment, taking the preparation of 100mL of electrolytic corrosion solution as an example, the preparation process is as follows: take 10-12ml of phosphoric acid and place it in a beaker, add deionized water, dilute to 50ml, then take 22-26g of NaOH and add it to the beaker, set the speed of 100r / min and stir for 1min to accelerate dissolution, then take 15-20g of copper sulfate pentahydrate and add it to the beaker, stir at a speed of 100r / min for 1min to accelerate dissolution; then take 6-9g of glycerol and add it to the beaker, mix evenly; finally, add deionized water, dilute the solution to 100ml, stir at a speed of 100r / min for 1min, mix the solution evenly, and obtain an electrolytic corrosion solution.

[0059] Based on a general inventive concept, an embodiment of the present application also provides a method for detecting residual stress of a component, the method comprising: electrolytically corroding the component using the electrolytic corrosion solution provided above to obtain multiple corrosion pits of different depths; and performing residual stress detection on the multiple corrosion pits.

[0060] The method is implemented based on the above-mentioned electrolytic corrosion solution. The specific content of the electrolytic corrosion solution can refer to the above-mentioned embodiment. Since the method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.

[0061] Specifically, in this embodiment, the specific process of electrolytic corrosion of the component by the electrolytic corrosion liquid can be: as in the above steps, prepare the electrolytic corrosion liquid, and seal and store the prepared neutral electrolytic corrosion liquid. Use cotton balls to dip into 3% hydrochloric acid aqueous solution and anhydrous ethanol to wipe the component detection surface in turn, remove the oil stains on the surface of the component, and use a hair dryer to blow dry the surface of the sample. Cut the protective paper into a size of 10*10mm, and use a puncher to open a hole with a diameter of 2mm in the middle of the protective paper. One side of the protective paper is adhesive, and the other side is a smooth surface without adhesiveness. The protective paper with a hole is pasted on the residual stress detection position of the component. The surface of the component leaking from the 2mm hole is the location of electrolytic corrosion and the location of residual stress detection. The diameter of the protective paper hole depends on the residual stress detection depth requirement and the residual stress equipment capacity requirement. The greater the residual stress detection depth, the appropriate increase in the hole diameter ensures that the X-ray hits the corrosion surface with the required detection depth during the residual stress detection. With different hole diameters, the electrolytic corrosion contact area changes accordingly, and the electrolytic process parameters can be confirmed in turn by the control variable method. Press the plasticine into a flat cylinder, then cut out a through hole in the middle. The diameter of the through hole is larger than the opening diameter of the protective paper 2mm, and smaller than the side length of the cut protective paper. Press the shaped plasticine on the protective paper. Inject the electrolytic corrosion liquid into the plasticine through hole and contact the surface of the component leaking from the center of the protective paper. The diameter of the plasticine through hole ensures that the electrolytic corrosion liquid can completely contact the surface of the component leaking from the opening of the protective paper after being injected into the through hole, and at the same time ensure that the electrolytic corrosion liquid does not contact the surface of the component outside the protective paper. Connect the anode of the electrolyzer to the component, and the cathode to the electrolytic corrosion liquid in the plasticine through hole. After the electrolyzer is powered on, an electrochemical reaction is formed. The electrolysis process parameters are as follows: DC voltage 24V, electrolysis current 5A, electrolytic corrosion depth 20μm when the electrolysis time is 5S, electrolytic corrosion depth 40μm when the electrolysis time is 10s, and electrolytic corrosion depth 60μm when the electrolysis time is 15s. The electrolytic corrosion depth can adjust the rate of electrolytic corrosion by adjusting the current and voltage of the electrolytic instrument. Combined with the electrolytic corrosion time setting, the preparation of corrosion pits with a given corrosion depth can be achieved. For example, when the DC voltage is 24V, the electrolytic current is 1A, and the electrolytic time is 3S, the electrolytic corrosion depth is 5μm.

[0062] In the electrochemical reaction, the component acts as an anode, and Fe loses electrons to become Fe 2+ , due to Cu 2+ The reducing property is stronger and it is easier to obtain electrons. The Cu 2+The cathode obtains electrons and becomes Cu, achieving electrolytic corrosion on the surface of the component while no gas is generated at the cathode, avoiding gas bubbling during electrolytic corrosion. There is no high concentration of strong acid in the electrolyte, and no strong corrosion reaction will occur with the metal itself, avoiding smoke during the electrolysis process. There is no high concentration of strong acid in the electrolytic corrosion solution, ensuring that there will be no strong chemical corrosion of the parts. At the same time, through the concentration ratio of each component in the electrolytic corrosion solution, there will be no excessive reaction during electrochemical corrosion, making the electrolysis rate controllable.

[0063] In some embodiments, the component has a protrusion, further, the protrusion has a pointed edge, and further, the component can be a gear.

[0064] In some embodiments, the component is made of medium-low alloy steel. Specifically, the mass content of alloy elements in the component is ≤10%.

[0065] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0066] Example 1

[0067] The invention discloses an electrolytic etching solution, wherein the components of the electrolytic etching solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and deionized water.

[0068] The mass concentration of phosphoric acid is 87%.

[0069] Each 100 mL of the electrolytic corrosion solution includes 9 mL of the phosphoric acid;

[0070] Each 100 mL of electrolytic corrosion solution includes 20 g of sodium hydroxide;

[0071] Each 100 mL of electrolytic corrosion solution includes 14 g of copper sulfate pentahydrate;

[0072] Each 100 mL of the electrolytic corrosion solution includes 5 g of glycerol.

[0073] Example 2

[0074] The invention discloses an electrolytic etching solution, wherein the components of the electrolytic etching solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and deionized water.

[0075] The mass concentration of phosphoric acid is 87%.

[0076] Every 100 mL of the electrolytic corrosion solution includes 10 mL of the phosphoric acid;

[0077] Each 100 mL of electrolytic corrosion solution includes 22 g of sodium hydroxide;

[0078] Each 100 mL of electrolytic corrosion solution includes 15 g of copper sulfate pentahydrate;

[0079] Each 100 mL of the electrolytic corrosion solution includes 6 g of glycerol.

[0080] Example 3

[0081] The invention discloses an electrolytic etching solution, wherein the components of the electrolytic etching solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and deionized water.

[0082] The mass concentration of phosphoric acid is 87%.

[0083] Each 100 mL of the electrolytic corrosion solution includes 11 mL of the phosphoric acid;

[0084] Each 100 mL of electrolytic corrosion solution includes 24 g of sodium hydroxide;

[0085] Each 100 mL of electrolytic corrosion solution includes 17 g of copper sulfate pentahydrate;

[0086] Each 100 mL of the electrolytic corrosion solution includes 8 g of glycerol.

[0087] Example 4

[0088] The invention discloses an electrolytic etching solution, wherein the components of the electrolytic etching solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and deionized water.

[0089] The mass concentration of phosphoric acid is 87%.

[0090] Each 100 mL of the electrolytic corrosion solution includes 12 mL of the phosphoric acid;

[0091] Each 100 mL of electrolytic corrosion solution includes 26 g of sodium hydroxide;

[0092] Each 100 mL of electrolytic corrosion solution includes 20 g of copper sulfate pentahydrate;

[0093] Each 100 mL of the electrolytic corrosion solution includes 9 g of glycerol.

[0094] Example 5

[0095] The invention discloses an electrolytic etching solution, wherein the components of the electrolytic etching solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and deionized water.

[0096] The mass concentration of phosphoric acid is 87%.

[0097] Each 100 mL of the electrolytic corrosion solution includes 13 mL of the phosphoric acid;

[0098] Each 100 mL of electrolytic corrosion solution includes 27 g of sodium hydroxide;

[0099] Each 100 mL of electrolytic corrosion solution includes 22 g of copper sulfate pentahydrate;

[0100] Each 100 mL of the electrolytic corrosion solution includes 10 g of glycerol.

[0101] Comparative Example 1

[0102] The invention discloses an electrolytic etching solution, the components of which include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and deionized water.

[0103] The mass concentration of phosphoric acid is 87%.

[0104] Each 100 mL of the electrolytic corrosion solution includes 11 mL of the phosphoric acid;

[0105] Each 100 mL of electrolytic corrosion solution includes 24 g of sodium hydroxide;

[0106] Each 100 mL of the electrolytic etching solution includes 17 g of copper sulfate pentahydrate.

[0107] Comparative Example 2

[0108] The invention discloses an electrolytic etching solution, the components of which include ethanol, deionized water and perchloric acid.

[0109] Wherein, the ethanol is anhydrous ethanol, and the mass concentration of perchloric acid is 60%.

[0110] Each 100ml of electrolytic corrosion solution includes 80ml of anhydrous ethanol;

[0111] Each 100ml of electrolytic corrosion solution includes 14ml of deionized water;

[0112] Every 100 ml of the electrolytic etching solution includes 6 ml of the perchloric acid.

[0113] The electrolytic corrosion liquid provided in each embodiment and comparative example is used to electrolytically corrode the component, and the component is a gear (the gear material grade is: 20CrMnTi). The specific process of electrolytic corrosion is as follows: wipe the component detection surface with a cotton ball dipped in 3% hydrochloric acid aqueous solution and anhydrous ethanol in turn to remove the oil stains on the surface of the component, and blow dry the surface of the sample with a hair dryer. Cut the protective paper into a size of 10*10mm, and use a puncher to open a hole with a diameter of 2mm in the middle of the protective paper. One side of the protective paper is adhesive, and the other side is a smooth surface without adhesiveness. The protective paper with a hole is pasted on the residual stress detection position of the component. The surface of the component exposed by the 2mm hole is the location of electrolytic corrosion and the location of residual stress detection. The diameter of the protective paper hole depends on the residual stress detection depth requirement and the residual stress equipment capacity requirement. The greater the residual stress detection depth, the appropriate increase in the hole diameter ensures that the X-ray hits the corrosion surface with the required detection depth during residual stress detection. With different hole diameters, the electrolytic corrosion contact area changes accordingly, and the electrolytic process parameters can be confirmed in turn by the control variable method. Press the plasticine into a flat cylinder, then cut out a through hole in the middle. The diameter of the through hole is larger than the opening diameter of the protective paper 2mm, and smaller than the side length of the cut protective paper. Press the shaped plasticine on the protective paper. Inject the electrolytic corrosion liquid into the plasticine through hole and contact the surface of the component leaking from the center of the protective paper. The diameter of the plasticine through hole ensures that the electrolytic corrosion liquid can completely contact the surface of the component leaking from the opening of the protective paper after being injected into the through hole, and at the same time ensure that the electrolytic corrosion liquid does not contact the surface of the component outside the protective paper. Connect the anode of the electrolyzer to the component, and the cathode to the electrolytic corrosion liquid in the plasticine through hole. After the electrolyzer is powered on, an electrochemical reaction is formed. The electrolysis process parameters are as follows: DC voltage 24V, electrolysis current 5A, electrolytic corrosion depth 20μm when the electrolysis time is 5S, electrolytic corrosion depth 40μm when the electrolysis time is 10s, and electrolytic corrosion depth 60μm when the electrolysis time is 15s. The situation of the electrolytic corrosion pit is shown in the following table.

[0114]

[0115] It can be seen from the above table that the electrolytic corrosion solution provided in the embodiment of the present application can perform good electrolytic corrosion on the component, which is beneficial to the subsequent detection of residual stress of the component.

[0116] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0117] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b and c can be single or multiple.

[0118] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. An electrolytic corrosion solution, characterized in that: The components of the electrolytic corrosion solution include phosphoric acid, sodium hydroxide, copper sulfate pentahydrate, glycerol and solvent.

2. The electrolytic corrosion solution according to claim 1, characterized in that: The mass concentration of the phosphoric acid is 83% to 90%.

3. The electrolytic corrosion solution according to claim 1 or 2, characterized in that: Each 100 mL of the electrolytic corrosion solution includes 10 mL to 12 mL of the phosphoric acid; and / or Each 100 mL of the electrolytic corrosion solution includes 22 g to 26 g of sodium hydroxide; and / or Each 100 mL of the electrolytic corrosion solution includes 15 g to 20 g of copper sulfate pentahydrate; and / or Every 100 mL of the electrolytic corrosion solution includes 6 g to 9 g of glycerol.

4. The electrolytic corrosion solution according to claim 1 or 2, characterized in that: Each 100 mL of the electrolytic corrosion solution includes 10.5 mL to 11.5 mL of the phosphoric acid; and / or Each 100 mL of the electrolytic corrosion solution includes 23 g to 25 g of sodium hydroxide; and / or Each 100 mL of the electrolytic corrosion solution includes 16 g to 19 g of copper sulfate pentahydrate; and / or Every 100 mL of the electrolytic corrosion solution includes 7 g to 8 g of glycerol.

5. The electrolytic corrosion solution according to claim 1 or 2, characterized in that: Each 100 mL of the electrolytic corrosion solution includes 10.8 mL to 11.2 mL of the phosphoric acid; and / or Each 100 mL of the electrolytic corrosion solution includes 23.5 g to 24.5 g of sodium hydroxide; and / or Each 100 mL of the electrolytic corrosion solution includes 17 g to 18 g of copper sulfate pentahydrate; and / or Every 100 mL of the electrolytic corrosion solution includes 7.3 g to 7.7 g of glycerol.

6. The electrolytic corrosion solution according to claim 1 or 2, characterized in that: The solvent includes water.

7. A method for preparing an electrolytic corrosion solution, characterized in that: The method comprises: Phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol are mixed in a solvent to obtain an electrolytic etching solution.

8. The method for preparing the electrolytic corrosive solution according to claim 7, characterized in that: The step of mixing phosphoric acid, sodium hydroxide, copper sulfate pentahydrate and glycerol in a solvent to obtain an electrolytic corrosion solution comprises: mixing phosphoric acid with a portion of the solvent to obtain a first solution; dissolving sodium hydroxide in the first solution to obtain a second solution; dissolving copper sulfate pentahydrate in the second solution to obtain a third solution; Mixing the third solution and glycerol to obtain a fourth solution; The fourth solution is diluted with the remaining solvent to obtain an electrolytic corrosion solution.

9. A method for detecting residual stress of a component, characterized in that: The method comprises: Electrolytically corroding a component using the electrolytic corrosive solution described in any one of claims 1 to 6 to obtain a plurality of corrosion pits of different depths; The residual stress test is performed on the plurality of corrosion pits.

10. The method for detecting residual stress of a component according to claim 9, characterized in that: The member has a protrusion; and / or The member comprises a gear; and / or The component is composed of medium and low alloy steel; and / or The mass content of alloy elements in the composition of the component is ≤10%.