Oil-water separation material as well as preparation method and application thereof
By forming a bilayer structure of polydopamine/copper nanoclusters and sodium octadecyl dithiocarbamate modifier on a stainless steel mesh, the problems of complex preparation and environmental pollution of superhydrophobic metal mesh are solved, achieving efficient and environmentally friendly oil-water separation.
Patent Information
- Application Number
- CN202411356553.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-27
AI Technical Summary
Existing superhydrophobic metal meshes have stringent preparation conditions, complex processes, and high costs, and also suffer from problems such as unsatisfactory mechanical strength, chemical incompatibility, and environmental pollution.
Using stainless steel mesh as the substrate, an oil-water separation material is formed by using a double-layer polydopamine/copper nanocluster intermediate layer and sodium octadecyl dithiocarbamate as a superhydrophobic modifier. The polydopamine deposition layer is formed on the surface of the stainless steel mesh by the self-polymerization of dopamine hydrochloride, and copper nanoparticles are formed by reducing Cu2+ with NaBH4. The surface energy is then modified with a hydrophobic agent.
It achieves an oil-water separation efficiency of over 96%, the material preparation is simple and environmentally friendly, and it can be reused more than 40 times while maintaining excellent hydrophobicity and high-efficiency separation performance.
Smart Images

Figure CN119038684A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oily wastewater treatment, and specifically relates to an oil-water separation material and a preparation method and application thereof. Background Art
[0002] Frequent oil spills and the continuous discharge of oily wastewater pose a great threat to the ecological environment, marine ecosystems and human health. Therefore, efficient oil-water separation methods are crucial to solving such environmental problems.
[0003] There are many traditional methods for separating oil-water mixtures, which can be divided into three categories according to the separation principle: physical separation, chemical treatment, and biodegradation. The main physical separation methods are: centrifugation, gravity, adsorption, and membrane separation. The chemical treatment methods are mainly divided into: chemical demulsification and oxidation-reduction. The biodegradation method introduces microorganisms into oily wastewater and uses the metabolism of microorganisms to degrade oil pollutants in wastewater and purify water resources. Traditional methods have various disadvantages, including low separation efficiency, long time consumption, and secondary pollution. These traditional methods have certain limitations in practical applications. Therefore, it is extremely important to develop cheap, simple, and easy-to-operate oil-water separation technology to achieve rapid and effective separation of oil and water.
[0004] In recent years, superhydrophobic metal meshes for filtering oil-water mixtures have been widely reported. In particular, superhydrophobic stainless steel meshes have become one of the most promising candidates for treating marine oil spills and industrial oily wastewater due to their low cost and satisfactory durability. However, the current superhydrophobic metal meshes have the following technical problems: (1) The preparation conditions of superhydrophobic metal meshes are harsh, the process is complex and the cost is high. In particular, expensive precision equipment such as high-temperature furnaces, vacuum equipment and coating spray guns are required, and the investment and maintenance costs are high; (2) In the process of preparing superhydrophobic metal meshes, improper surface treatment or coating such as acid etching may cause embrittlement or peeling of the metal surface, thereby weakening its mechanical strength. (3) The use of thiol modifiers causes environmental pollution; (4) The chemical incompatibility between the metal mesh and the superhydrophobic coating may lead to weak interaction, thereby affecting the adhesion of the coating, which in turn makes the stability and recyclability of most superhydrophobic stainless steel meshes unsatisfactory.
[0005] Therefore, it is urgent to develop a method for preparing a super-hydrophobic metal wire mesh for oily wastewater treatment that has little effect on the mechanical properties of the metal itself, has mild reaction conditions, and has safe and simple process operations. Summary of the invention
[0006] In view of the above technical problems, the present invention provides an oil-water separation material and a preparation method and application thereof. The oil-water separation material provided by the present invention has a stainless steel mesh as a substrate, a double-layer polydopamine / copper nanocluster as an intermediate layer, and sodium octadecyl dithiocarbamate as a superhydrophobic modifier, and the oil-water separation efficiency exceeds 96%.
[0007] The present invention is achieved through the following technical solutions: A method for preparing an oil-water separation material comprises the following steps: (1) Pre-treat the stainless steel mesh; (2) placing the stainless steel mesh in a weakly alkaline dopamine hydrochloride solution, stirring for a period of time at a suitable temperature, washing and drying to obtain a stainless steel mesh with polydopamine deposited on the surface; (3) The stainless steel mesh with polydopamine deposited on the surface obtained in step (2) is immersed in CuCl 2 After stirring the solution at room temperature for a certain period of time, NaBH 4 The aqueous solution is stirred for a certain period of time, and then washed and dried to a constant weight to obtain a stainless steel mesh with a polydopamine / copper nanocluster coating deposited on the surface; (4) Repeat steps (2) to (3) to obtain a stainless steel mesh with a double-layer polydopamine / copper nanocluster coating deposited on the surface; (5) The stainless steel mesh obtained in step (4) is placed in a sodium octadecyl dithiocarbamate solution for modification. After modification for a period of time, the stainless steel mesh is taken out and naturally dried to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, that is, the oil-water separation material is obtained.
[0008] Furthermore, step (1) is specifically as follows: selecting a stainless steel mesh with a mesh size of 600-1000 mesh, ultrasonically treating the stainless steel mesh with ethanol, acetone and deionized water in sequence, and drying at room temperature after the ultrasonic treatment. In this step, the surface pollutants and oil film can be effectively removed by ultrasonic treatment.
[0009] Furthermore, in step (2), the weakly alkaline dopamine hydrochloride solution is prepared by dissolving dopamine hydrochloride in a Tris-HCl buffer solution, and the pH of the prepared weakly alkaline dopamine hydrochloride solution is 7-8.8; and the concentration of the weakly alkaline dopamine hydrochloride solution is 2 g·L −1 .
[0010] Under alkaline conditions, dopamine hydrochloride can spontaneously undergo polymerization reaction, and can firmly adhere to the surface of the stainless steel mesh without special treatment of the stainless steel mesh to form a firm polydopamine deposition layer. The surface of the polydopamine deposition layer can be grafted with metal ions and low surface energy substances, thereby giving the metal material surface superhydrophobic properties. Therefore, the pH of the dopamine hydrochloride solution needs to be limited to 7-8.8 in the present invention.
[0011] Furthermore, in step (2), the stirring temperature is 20-60 °C and the stirring time is 4-24 h. Controlling the stirring conditions in this step can make the polydopamine coating deposit more uniformly and achieve an appropriate thickness. In the present invention, the control of temperature and stirring time can optimize the uniformity and thickness of the polydopamine coating and ensure that the coating is uniformly deposited on the surface of the stainless steel mesh. Appropriate stirring conditions can also promote polymerization reactions and improve the adhesion and structural stability of the coating. Higher temperatures can accelerate polymerization reactions and increase deposition rates, but may result in uneven coatings or excessive thickness; lower temperatures help form more uniform coatings, but the deposition rate is slower. Therefore, finding the optimal temperature range and stirring time is crucial to obtaining an ideal polydopamine coating.
[0012] Furthermore, in step (3), CuCl 2 The concentration of the solution is 0.02~0.1mol / L; NaBH 4 The concentration of the aqueous solution is 0.04~0.08mol / L; In CuCl 2 The solution was stirred for 0.5 h and NaBH 4 The aqueous solution was stirred for 2 h. 4 The aqueous solution can 2+ Completely reduced to copper nanoparticles.
[0013] Furthermore, in step (5), the sodium octadecyl dithiocarbamate solution is prepared by: Dissolve 0.001-0.01 mol of octadecylamine and 0.001-0.01 mol of sodium hydroxide in 85 mL of ether, stir and dissolve to obtain a suspension, add 0.04-0.4 mol of carbon disulfide to the suspension to obtain a mixed solution; vigorously stir the mixed solution (400-500 rpm) at room temperature for 0.5-2 h; collect the obtained white solid product, and dry it to obtain sodium octadecyl dithiocarbamate; The prepared sodium octadecyl dithiocarbamate is dispersed in ethanol to prepare a sodium octadecyl dithiocarbamate solution.
[0014] Furthermore, in step (5), the concentration of the sodium octadecyl dithiocarbamate solution is 0.15-0.45 g·L −1 , and the modification time is 2 to 6 h. Under the concentration and modification time defined in the present invention, sodium octadecyl dithiocarbamate can be uniformly attached to the surface of the material to form a stable and lasting hydrophobic layer, thereby improving the water resistance and anti-pollution ability, and at the same time, realizes economical and effective modification at a lower concentration, and has the advantages of lower toxicity and environmental protection.
[0015] An oil-water separation material uses a stainless steel mesh as a substrate, a double-layer polydopamine / copper nanocluster as an intermediate layer, and sodium octadecyl dithiocarbamate as a super-hydrophobic modifier.
[0016] Furthermore, the oil-water separation efficiency of the oil-water separation material exceeds 96%, and the static contact angle of the oil-water separation material to water is greater than 151°.
[0017] An application of an oil-water separation material, wherein the oil-water separation material is used for separating oily wastewater and recovering leaked crude oil.
[0018] Technical principle of the present invention: The present invention utilizes the self-polymerization of dopamine hydrochloride to form a polydopamine deposition layer on the surface of the stainless steel mesh. In addition, the polydopamine deposition layer can be used as a secondary modification platform to adsorb Cu in the solution. 2+ , and as a nucleation surface, using NaBH 4 Aqueous solution can completely reduce the copper ions in the solution to copper nanoparticles, thereby constructing micro-nano structures (copper nanoclusters). In addition, polydopamine has super strong adhesion, which can combine with the stainless steel mesh and adhere the copper nanoparticles to the surface to form the desired roughness; then the hydrophobic agent is used for low surface energy modification.
[0019] Beneficial technical effects of the present invention: The preparation method of the oil-water separation material provided by the present invention is simple, the raw material source is wide, and it is environmentally friendly; the oil-water separation efficiency exceeds 96%, and the oil-water separation process can be repeated for more than 40 times while still maintaining excellent hydrophobicity (contact angle>151°) and high efficiency (above 96.2%).
[0020] The preparation of the oil-water separation material provided by the present invention does not require special equipment and can be easily implemented in large-scale production.
[0021] The oil-water separation material provided by the present invention adopts sodium octadecyl dithiocarbamate as a super-hydrophobic modifier; compared with thiol modifiers, sodium octadecyl dithiocarbamate exists in a solid form and is not easy to volatilize, so less harmful gases are released during the application process; and it is relatively stable in the environment, usually shows low bioaccumulation and toxicity, and is relatively environmentally friendly.
[0022] The oil-water separation material provided by the present invention can be used to separate various oil-water mixtures under natural gravity environment, and has important application potential in treating oily wastewater and offshore oil spills. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 SEM image of the original stainless steel mesh.
[0024] Figure 2 This is a scanning electron microscope image of the oil-water separation material prepared in the example of the present invention.
[0025] Figure 3 This is a water contact angle measurement diagram of the oil-water separation material prepared in an embodiment of the present invention.
[0026] Figure 4 Graph showing the oil-water separation efficiency of the oil-water separation material prepared in an embodiment of the present invention.
[0027] Figure 5 This is a water contact angle measurement diagram of the oil-water separation material prepared in Example 2 of the present invention.
[0028] Figure 6 This is a water contact angle measurement diagram of the oil-water separation material prepared in Example 3 of the present invention.
[0029] Figure 7 This is a water contact angle measurement diagram of the oil-water separation material prepared in Example 4 of the present invention.
[0030] Figure 8 This is a water contact angle measurement diagram of the oil-water separation material prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] On the contrary, the present invention covers any substitution, modification, equivalent method and scheme made on the essence and scope of the present invention as defined by the claims. Further, in order to make the public have a better understanding of the present invention, some specific details are described in detail in the detailed description of the present invention below. Those skilled in the art can fully understand the present invention without the description of these details.
[0033] In the following examples, room temperature refers to 25±5°C.
[0034] Embodiment 1: This embodiment provides a method for preparing an oil-water separation material, comprising the following steps: (1) Select a stainless steel mesh with a mesh size of 800 mesh, and ultrasonically clean it with ethanol, acetone and deionized water for 15 minutes in sequence to remove surface contaminants. Then, dry it naturally at room temperature. In this embodiment, the ultrasonic power is 200W; the ultrasonic frequency is 40KHZ.
[0035] (2) Dissolve dopamine hydrochloride in a buffer solution prepared with Tris-HCl at pH 7 to obtain a concentration of 2 g·L −1 of dopamine hydrochloride solution; The cleaned stainless steel mesh in step (1) was placed in the prepared dopamine hydrochloride solution and stirred at 25°C for 20 h. Subsequently, the obtained sample was rinsed with water and finally dried at 85°C to obtain a stainless steel mesh with polydopamine deposited thereon.
[0036] (3) The stainless steel mesh deposited with polydopamine in step (2) was immersed in a 0.08 M CuCl 2 The solution was stirred at 25 °C for 0.5 h (300 rpm). Then, NaBH 4 Aqueous solution, NaBH 4 The final concentration was 0.05 M, and stirring was performed for 2 h to completely reduce the copper ions bound to the polydopamine coating. Finally, the modified stainless steel mesh was taken out, cleaned, and dried to a constant weight to obtain a stainless steel mesh with polydopamine / copper nanoclusters deposited thereon.
[0037] (4) Repeat steps (2) to (3) on the stainless steel mesh of polydopamine / copper nanoclusters obtained in step (3) to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters deposited on the surface.
[0038] (5) Place the double-layer polydopamine / copper nanoclusters obtained in step (4) on a stainless steel mesh with a concentration of 0.3 g·L -1 The mesh was further modified at 25°C (or within the range of 25°C ± 5°C) for 4 h. Then, it was taken out and dried naturally to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyldithiocarbamate coating deposited on the surface, i.e., an oil-water separation material.
[0039] Figure 1 This is a scanning electron microscope image of the original stainless steel mesh. Figure 2 The oil-water separation material prepared in this example (the material modified by sodium octadecyl dithiocarbamate) Figure 1 The SEM image of the original stainless steel mesh is shown, and the observation results show that the surface is very smooth. After superhydrophobic modification (see Figure 2), the surface of the stainless steel mesh is completely covered with small particles, which are randomly distributed to form irregular aggregates. Figure 3 This is a water contact angle measurement diagram of the oil-water separation material prepared in this example.
[0040] Embodiment 2: This embodiment provides a method for preparing an oil-water separation material, comprising the following steps: (1) Select a stainless steel mesh with a mesh size of 600 mesh, and ultrasonically clean it with ethanol, acetone, and deionized water for 15 minutes in sequence to remove surface contaminants. Then, dry it naturally at room temperature.
[0041] (2) Dissolve dopamine hydrochloride in a buffer solution prepared with Tris-HCl at pH = 8.5 to obtain a concentration of 1 g·L −1 of dopamine hydrochloride solution; The cleaned stainless steel mesh in step (1) is placed in the prepared dopamine hydrochloride solution and stirred at 20°C for 24 hours. Subsequently, the obtained sample is rinsed with water and finally dried at 85°C to obtain a stainless steel mesh with polydopamine deposited thereon; (3) The stainless steel mesh deposited with polydopamine in step (2) was immersed in a 0.05 M CuCl 2 The solution was stirred at 25 °C for 1.0 h (300 rpm). Then, NaBH 4 Aqueous solution, NaBH 4 The final concentration was 0.04 M, and stirring was performed for 3 h to completely reduce the copper ions bound to the polydopamine coating. Finally, the modified stainless steel mesh was taken out, cleaned, and dried to a constant weight to obtain a stainless steel mesh with a polydopamine / copper nanocluster coating deposited thereon; (4) Repeat steps (2) to (3) on the stainless steel mesh obtained in step (3) to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters deposited on the surface.
[0042] (5) Place the stainless steel mesh obtained in step (4) into a solution with a concentration of 0.15 g·L -1 The mesh was modified in a sodium octadecyl dithiocarbamate solution for 6 h. Then, it was taken out and dried naturally to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, that is, the oil-water separation material was prepared. Figure 5 This is a water contact angle measurement diagram of the oil-water separation material prepared in this example.
[0043] Embodiment 3: This embodiment provides a method for preparing an oil-water separation material, comprising the following steps: (1) Select a stainless steel mesh with a mesh size of 1000 mesh, and ultrasonically clean it with ethanol, acetone and deionized water for 15 minutes in sequence to remove surface contaminants. Then, dry it naturally at room temperature.
[0044] (2) Dissolve dopamine hydrochloride in a buffer solution prepared with Tris-HCl at pH = 8.8 to obtain a concentration of 4 g·L −1 of dopamine hydrochloride solution; The cleaned stainless steel mesh in step (1) is placed in the prepared dopamine hydrochloride solution and stirred at 40°C for 15 h. Subsequently, the obtained sample is rinsed with water and finally dried at 85°C to obtain a stainless steel mesh with polydopamine deposited thereon; (3) The stainless steel mesh deposited with polydopamine in step (2) was immersed in a 0.1 M CuCl 2 The solution was stirred at 25 °C for 0.5 h (300 rpm). Then, NaBH 4 Aqueous solution, NaBH 4 The final concentration was 0.08 M, and stirring for 1 h could completely reduce the copper ions bound to the polydopamine coating. Finally, the modified stainless steel mesh was taken out, cleaned, and dried to a constant weight to obtain a stainless steel mesh with a polydopamine / copper nanocluster coating deposited thereon.
[0045] (4) Repeat steps (2) to (3) on the stainless steel mesh obtained in step (3) to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters deposited on the surface.
[0046] (5) Place the stainless steel mesh obtained in step (4) into a solution with a concentration of 0.45 g·L -1 The mesh was placed in a sodium octadecyl dithiocarbamate solution for 2 hours. Then, the mesh was taken out and dried naturally to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, thus preparing an oil-water separation material. Figure 6 This is a water contact angle measurement diagram of the oil-water separation material prepared in this example.
[0047] Embodiment 4: This embodiment provides a method for preparing an oil-water separation material, comprising the following steps: (1) Select a stainless steel mesh with a mesh size of 800 mesh, and ultrasonically clean it with ethanol, acetone, and deionized water for 15 minutes in sequence to remove surface contaminants. Then, dry it naturally at room temperature.
[0048] (2) Dissolve dopamine hydrochloride in a buffer solution prepared with Tris-HCl at pH 7.5 to obtain a concentration of 3 g·L −1 of dopamine hydrochloride solution.
[0049] The cleaned stainless steel mesh in step (1) was placed in the prepared dopamine hydrochloride solution and stirred at 60°C for 4 h. Subsequently, the obtained sample was rinsed with water and finally dried at 85°C to obtain a stainless steel mesh with polydopamine deposited thereon; (3) The stainless steel mesh deposited with polydopamine in step (2) was immersed in a 0.02 M CuCl 2 The solution was stirred at 25 °C for 1.5 h (300 rpm). Then, NaBH 4 Aqueous solution, NaBH 4 The final concentration was 0.06 M, and stirring was performed for 2 h to completely reduce the copper ions bound to the polydopamine coating. Finally, the modified stainless steel mesh was taken out, cleaned, and dried to a constant weight to obtain a stainless steel mesh with a polydopamine / copper nanocluster coating deposited thereon.
[0050] (4) Repeat steps (2) to (3) on the stainless steel mesh obtained in step (3) to obtain a stainless steel mesh on which a double layer of polydopamine / copper nanoclusters is deposited.
[0051] (5) Place the stainless steel mesh obtained in step (4) into a solution with a concentration of 0.2 g·L -1 The mesh was modified in a sodium octadecyl dithiocarbamate solution for 5 h. Then, it was taken out and dried naturally to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, that is, the oil-water separation material was prepared; Figure 7 This is a water contact angle measurement diagram of the oil-water separation material prepared in this example.
[0052] Embodiment 5: This embodiment provides a method for preparing an oil-water separation material, comprising the following steps: (1) Select a stainless steel mesh with a mesh size of 800 mesh, and ultrasonically clean it with ethanol, acetone, and deionized water for 15 minutes in sequence to remove surface contaminants. Then, dry it naturally at room temperature.
[0053] (2) Dissolve dopamine hydrochloride in a buffer solution prepared with Tris-HCl at pH = 8.5 to obtain a concentration of 2 g·L −1 of dopamine hydrochloride solution; The cleaned stainless steel mesh in step (1) was placed in the prepared dopamine hydrochloride solution and stirred at 25°C for 24 hours. Subsequently, the obtained sample was rinsed with water and finally dried at 85°C to obtain a stainless steel mesh with polydopamine deposited thereon.
[0054] (3) The stainless steel mesh deposited with polydopamine in step (2) was immersed in a 0.08 M CuCl 2The solution was stirred at 25 °C for 0.5 h (300 rpm). Then, NaBH 4 Aqueous solution, NaBH 4 The final concentration was 0.05 M, and the copper ions bound to the polydopamine coating were completely reduced by stirring for 2 h. Finally, the modified stainless steel mesh was taken out, cleaned, and dried to a constant weight to obtain a stainless steel mesh with polydopamine / copper nanoclusters deposited thereon.
[0055] (4) Repeat steps (2) to (3) on the stainless steel mesh obtained in step (3) to obtain a stainless steel mesh with a double-layer polydopamine / copper nanocluster coating deposited on the surface.
[0056] (5) Place the stainless steel mesh obtained in step (4) into a solution with a concentration of 0.4 g·L -1 The mesh was modified in a sodium octadecyl dithiocarbamate solution for 4 h. Then, it was taken out and dried naturally to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, that is, the oil-water separation material was prepared. Figure 8 This is a water contact angle measurement diagram of the oil-water separation material prepared in this example.
[0057] The oil-water separation materials prepared in Examples 1-5 were subjected to oil-water separation tests, and the test results showed that the separation efficiency of the oil-water separation materials prepared in each example reached more than 90%; and the oil-water separation process could be repeated 40 times while still maintaining excellent hydrophobicity (contact angle > 151°) and high efficiency (more than 96.2%).
[0058] like Figure 4 As shown in Figure 2, in order to evaluate the filtration capacity of the superhydrophobic stainless steel mesh, filtration experiments of different oil-water mixtures were conducted. The separation efficiency of deionized water mixed with three test oils (kerosene, chloroform, and hexane) at a volume ratio of 3:1 exceeded 97.6%.
[0059] The oil-water separation material prepared by the present invention is a metal mesh super-hydrophobic material modified with modified octadecylamine, which has a simple preparation process, low production cost, good mechanical stability, resistance to organic solvents, salt solutions and acid-base solutions, and the obtained modified stainless steel mesh exhibits excellent super-hydrophobicity (contact angle>151°) and high separation efficiency (>96.2%). Among them, organic solvent resistance is related to the hydrophobicity and chemical stability of the material, ensuring that it is not dissolved or degraded during the oil-water separation process; salt solution resistance helps to maintain the separation effect in seawater or salt water environment; acid-base solution resistance reflects the chemical stability of the material under extreme pH conditions, ensuring that it is still effective in various industrial applications.
[0060] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention is still covered by the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing an oil-water separation material, It is characterized in that The following steps are involved: (1) Pre-treat the stainless steel mesh; (2) placing the pretreated stainless steel mesh in a weakly alkaline dopamine hydrochloride solution, stirring at a suitable temperature, washing, and drying to obtain a stainless steel mesh with polydopamine deposited on the surface; (3) The stainless steel mesh with polydopamine deposited on the surface obtained in step (2) is immersed in CuCl 2 After stirring at room temperature, NaBH 4 The aqueous solution is stirred, washed, and dried to a constant weight to obtain a stainless steel mesh with polydopamine / copper nanoclusters deposited on the surface; (4) Repeat steps (2) to (3) to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters deposited on the surface; (5) The stainless steel mesh obtained in step (4) is placed in a sodium octadecyl dithiocarbamate solution for modification, and after modification, it is taken out and naturally dried to obtain a stainless steel mesh with a double layer of polydopamine / copper nanoclusters and sodium octadecyl dithiocarbamate coating deposited on the surface, that is, the oil-water separation material is obtained.
2. A method for preparing an oil-water separation material according to claim 1, It is characterized in that Step (1) specifically comprises: selecting a stainless steel mesh with a mesh size of 600-1000 meshes, ultrasonically treating the stainless steel mesh with ethanol, acetone and deionized water in sequence, and drying the mesh at room temperature after the ultrasonic treatment.
3. A method for preparing an oil-water separation material according to claim 1, It is characterized in that In step (2), the weakly alkaline dopamine hydrochloride solution is prepared by dissolving dopamine hydrochloride in a Tris-HCl buffer solution; The pH of the prepared weakly alkaline dopamine hydrochloride solution is 7-8.8; and the concentration of the weakly alkaline dopamine hydrochloride solution is 1-4 g·L −1 .
4. A method for preparing an oil-water separation material according to claim 1, It is characterized in that In step (2), the stirring temperature is 20-60 °C and the stirring time is 4-24 h.
5. A method for preparing an oil-water separation material according to claim 1, It is characterized in that In step (3), the CuCl 2 The concentration of the solution is 0.02~0.1 mol / L; the NaBH 4 The concentration of the aqueous solution is 0.04~0.08 mol / L; In CuCl 2 The stirring time in the solution was 0.5~1.5 h. 4 The stirring time in aqueous solution is 1~3 h.
6. A method for preparing an oil-water separation material according to claim 1, It is characterized in that In step (5), the sodium octadecyl dithiocarbamate solution is prepared by: Dissolve 0.001-0.01 mol of octadecylamine and 0.001-0.01 mol of sodium hydroxide in 85 mL of ether, stir to dissolve to obtain a suspension, add 0.02-0.2 mol of carbon disulfide to the suspension to obtain a mixed solution; vigorously stir the mixed solution at a speed of 400-500 rpm for 0.5-2 h at room temperature; collect the obtained white solid product, dry it, and obtain sodium octadecyl dithiocarbamate; The prepared sodium octadecyl dithiocarbamate is dispersed in ethanol to prepare a sodium octadecyl dithiocarbamate solution.
7. A method for preparing an oil-water separation material according to claim 1, It is characterized in that In step (5), the concentration of the sodium octadecyl dithiocarbamate solution is 0.15-0.45 g·L −1 The modification time is 2~6 h.
8. An oil-water separation material, prepared by the method according to any one of claims 1 to 7, It is characterized in that The oil-water separation material uses a stainless steel mesh as a substrate, a double-layer polydopamine / copper nanocluster as an intermediate layer, and sodium octadecyl dithiocarbamate as a super-hydrophobic modifier.
9. The oil-water separation material according to claim 8, It is characterized in that The oil-water separation efficiency of the oil-water separation material exceeds 96%. After the oil-water separation test, the static contact angle to water is greater than 151°.
10. Use of the oil-water separation material according to any one of claims 8 to 9, It is characterized in that The oil-water separation material is used for separation of oily wastewater and recovery of leaked crude oil.
Citation Information
Patent Citations
Hydrophobic film structure, preparation method thereof and mildewproof wood
CN110450250A
Preparation method of super-hydrophobic oleophylic material
CN110755888A
Method for preparing wear-resistant super-hydrophobic coating by electro-deposition method
CN111996561A
Super-hydrophilic Ti-Cu / polydopamine composite coating and preparation method thereof
CN114225124A
Photocatalytic oil-water separation material and preparation method thereof
US20220184590A1