Electrospun fibrous membrane as well as preparation method and application thereof
Through the core-shell structure and porous structure of the electrospun fiber membrane, combined with radiation refrigeration polymer and impact-resistant polymer, the problem of insufficient reliability and sensing performance of flexible electronic fabrics in harsh environments is solved, and high-performance impact-resistant , sensing and waterproof performance.
Patent Information
- Application Number
- CN202411228962.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, when preparing flexible electronic fabrics, it is difficult to take into account both impact resistance, sensing sensitivity, radiation refrigeration performance and waterproof performance, resulting in insufficient reliability and sensing performance of electronic fabrics in harsh environments.
The core-shell structure and porous structure of electrospinning fiber membrane are used to prepare shell and core-layer spinning liquid through coaxial spinning technology, and the radiation refrigeration polymer and impact-resistant polymer are used to form high pressure sensitivity and impact-resistant Performance of electrospun fiber membrane.
It achieves a balance of high pressure sensitivity, impact resistance, radiation refrigeration performance and waterproof performance. The fiber membrane still maintains good performance after repeated bending and washing, and is suitable for multifunctional electronic fabrics and wearable devices.
Smart Images

Figure CN118996724A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional fiber membranes, and in particular relates to an electrospun fiber membrane and a preparation method and application thereof. Background Art
[0002] As a new generation of flexible electronic technology, smart electronic fabrics have great application prospects in the fields of mobile medical care, health monitoring, human-computer interaction, etc. The development of fiber electronic fabrics will bring people smarter, more convenient and safer solutions, help promote smart wearable technology to a new height, and bring a smarter, healthier and more comfortable experience to future life. In demanding application scenarios such as modern sportswear, space suits and fire suits, there are high requirements for smart textiles for personal protection, health monitoring, body comfort and wearing durability. However, non-woven integration, such a smart clothing system, has always been a long-sought but challenging goal. Since the fibers obtained by traditional spinning methods cannot meet the requirements of non-woven integration, they are difficult to be compatible in terms of wearable comfort, high sensor sensitivity, structural stability and impact resistance, which greatly limits the development of electronic fabrics. Therefore, the development of non-woven fiber films with excellent multi-sensing performance, wearing comfort and structural stability has become the focus of development in this field.
[0003] Flexible polymer materials are materials with good flexibility and have great prospects for the preparation of wearable electronic fabrics. While flexibility brings better sensing sensitivity, it also reduces the impact resistance, fatigue resistance and robustness of electronic fabrics. For example, Huang Yongan et al. reported a flexible sensor network and its preparation method and application in CN118424352A. The flexible sensor network includes a flexible substrate and a flexible support skeleton, which is reinforced with a flexible support skeleton. Due to the limited strength of the flexible substrate, it is easily damaged in harsh environments. The reinforcement of the metal skeleton is conducive to ensuring the reliability of the flexible sensor network under more complex working conditions and improving the stretchability of the flexible sensor network, but greatly reduces the sensitivity of the sensor. Therefore, it is urgent to develop a flexible electronic fabric that can take into account impact resistance, sensing sensitivity, radiation cooling performance, and waterproof performance at the same time. Summary of the invention
[0004] The present invention provides an electrospun fiber membrane and a preparation method and application thereof, which solves the problem that the flexible electronic fabric prepared in the prior art has improved its impact resistance but cannot take into account the sensing sensitivity, radiation cooling performance and waterproof performance.
[0005] The first object of the present application is to provide an electrospun fiber membrane, the raw material composition of which is:
[0006] A shell spinning solution, wherein the main components of the shell spinning solution are a radiation cooling polymer and an ionic liquid;
[0007] A core layer spinning solution, wherein the core layer spinning solution is mainly composed of an impact-resistant high molecular polymer with shear thickening properties;
[0008] The shell layer spinning solution and the core layer spinning solution are coaxially spun to prepare an electrospun fiber membrane.
[0009] The electrospun fiber membrane prepared in the present application has a core-shell structure and a porous structure, and its function is: when the electrospun fiber membrane is subjected to stress and compression deformation, the air in the pores between the fibers is first compressed, and then the low modulus shell polymer of the core-shell structure fiber and the low modulus core layer impact-resistant polymer at low shear rate are strained, and continue to absorb part of the stress. When the stress increases to a certain extent, the modulus of the impact-resistant polymer in the core layer continues to increase, absorbing the main large stress. This compression process increases the capacitance change during the force-bearing process, thereby increasing the pressure sensing sensitivity. Moreover, this process increases the absorbable impact force and enhances the impact resistance. The role of the porous structure and the core-shell structure, the air in the pores and the impact-resistant polymer in the core layer that is transformed from solid to liquid behavior can be used as a plasticizer to soften the fiber membrane, increasing the wearable comfort.
[0010] The electrospun fiber membrane can attenuate more than 60% of the impact force, and the pressure sensitivity is as high as 202.3kPa. -1 , achieving a temperature sensing resolution of 0.1°C and a 2 The skin temperature was reduced by 17°C under white light illumination intensity of 10°C; the electrospun fiber membranes had high structural stability, with a pressure sensing performance retention rate of >98% after 10,000 bending cycles, exhibiting excellent waterproof properties, and their impact resistance retention rate was >90% after 50 cycles of washing and drying.
[0011] The present invention adopts coaxial spinning to controllably form a core-shell structure, that is, the core layer and shell layer polymers are nested and exist independently. 1. The polymer of the shell layer can support the structure of the impact-resistant polymer of the core layer (the impact-resistant polymer of the core layer has a low modulus under static force, such as polyborosiloxane, which will flow like a liquid and may not even be able to be formed into filaments alone). 2. The core layer and the shell layer produce different functionalities, and not blending the two can prevent them from affecting each other functionally. 3. The impact resistance of the core layer impact-resistant polymer depends on the intermolecular force, and blending with other substances will reduce the impact resistance.
[0012] Preferably, the electrospun fiber membrane has a fiber orientation perpendicular to the roller axis, a single-layer fiber membrane thickness of 20-100 microns, and a fiber diameter of 0.2-3 microns. The electrospun fiber membrane has good impact resistance when it is very thin. Fibers with thick fiber diameters have better impact resistance, and fine diameters have better pressure sensing performance. The electrospun fiber membrane prepared by the present invention can have both good impact resistance and pressure sensing performance within this diameter range.
[0013] Preferably, the radiation cooling polymer, i.e., the shell polymer, is any one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyvinylidene fluoride, polyvinyl alcohol, and polyurethane. The radiation cooling polymer serves as the main body and supporting material of the electrospun fiber shell layer and provides a good foundation for radiation cooling performance.
[0014] Preferably, the ionic liquid is any one or more of 1-ethyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dicyanamide salt, 1-butyl-3-methylimidazolium dicyanamide salt, 1-butyl-3-methylimidazolium bis-trifluoromethanesulfonyl imide salt, and 1-butyl-3-methylimidazolium tetrafluoroborate. The ionic liquid is selected to be an ionic liquid that can form a polymer electrolyte with the shell polymer, which provides mechanical sensing properties and thermoelectric properties for the prepared electrospun fiber membrane.
[0015] Preferably, the impact-resistant high molecular polymer, i.e., the core layer polymer, is polyborosiloxane or polyacrylamide / organic silicon blended gel. The core layer polymer, as the main material of the core layer of the electrospun fiber, provides excellent impact resistance and further enhances the radiant cooling performance. Preferably, the core layer polymer is polyborosiloxane.
[0016] The second object of the present invention is to protect the preparation method of the electrospun fiber membrane, comprising:
[0017] Preparing a shell spinning solution: preparing a shell polymer into a shell solution with a concentration of 100-200 mg / mL, adding an ionic liquid, mixing and stirring for 4-8 hours to obtain a shell spinning solution; wherein the shell polymer is a radiation cooling polymer, and the mass ratio of the shell polymer to the ionic liquid is 1:0.2-1.5;
[0018] Preparing a core layer spinning solution: preparing a core layer polymer into a core layer spinning solution with a concentration of 300-900 mg / mL; the core layer polymer is an impact-resistant high molecular polymer with shear thickening properties;
[0019] Preparation of electrospun fiber membrane: The prepared core layer spinning solution and shell layer spinning solution are coaxially spun and subjected to a voltage of 7-15kV to obtain an electrospun fiber membrane; wherein the mass ratio of the core layer spinning solution to the shell layer spinning solution is 0.5-2:1. Too little shell layer spinning solution cannot carry the impact-resistant polymer inside. Too much shell layer spinning solution will have a weak impact-resistant effect.
[0020] First of all, electrospinning can only be performed with spinning solution within a certain viscosity range. Electrospinning fiber membrane cannot be obtained at all if the viscosity is lower or higher than this range, and the viscosity is directly related to the spinning solution concentration. Therefore, the present invention sets the shell layer spinning solution and the core layer spinning solution of the above concentration. In addition, within the spinnable range, the silk released from high concentration has a thicker diameter and a smaller porosity, and the flexibility will be relatively weak, the sensing performance will be slightly worse, but the impact resistance will be better. On the contrary, it will have better sensing performance and slightly worse impact resistance. The concentration ratio of the core layer and the shell layer will also affect the emphasis of multiple functions. Different functions are achieved by different components and contents; which component will be increased to strengthen this function, while the proportion of other components will be reduced, and other functions will be weakened. The concentration range set by the present invention can have multiple functions at the same time. If it exceeds this range, spinning will not be possible, or some functions cannot meet the requirements.
[0021] During coaxial spinning, the voltage will affect the diameter of the formed filaments, which will directly affect the strength of the membrane, and therefore will also affect the pressure sensing performance of the generated membrane. If the voltage is too high or too low, the electrospun fiber membrane cannot be prepared.
[0022] Preferably, when preparing the shell spinning solution, the shell solvent used is a solvent in which the corresponding radiation cooling polymer can be dissolved, including but not limited to DMF, THF, ethanol, water and mixed solutions thereof.
[0023] Preferably, when preparing the core layer spinning solution, the core layer solvent used is a solvent that can dissolve the corresponding impact-resistant high molecular polymer, including but not limited to DMF, THF and a mixed solution thereof.
[0024] Preferably, when preparing the electrospun fiber membrane, the shell layer spinning solution is extruded through the shell layer of the coaxial spinning needle at a rate of 0.001 to 0.02 mL / min.
[0025] Preferably, when preparing the electrospun fiber membrane, the core layer spinning solution is extruded through the core layer of the coaxial spinning needle at a rate of 0.002 to 0.01 mL / min.
[0026] The shell layer spinning solution and the core layer spinning solution are extruded at this rate ratio, which ensures the ratio of the amount of the shell layer spinning solution and the core layer spinning solution, and ensures that the prepared electrospun fiber membrane can simultaneously take into account impact resistance, sensor sensitivity, radiation cooling performance, and waterproof performance.
[0027] Preferably, the method for preparing the shell solution is:
[0028] The radiation cooling polymer is heated and stirred at 35-80° C. and dissolved in the shell solvent to prepare a shell solution with a concentration of 100-200 mg / mL.
[0029] The third object of the present invention is to protect the application of the electrospun fiber membrane in multifunctional electronic fabrics, wearable devices, smart sportswear, space suits, and military equipment.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention selects specific radiation cooling polymers and ionic liquids as the main components of the shell spinning solution, selects impact-resistant high molecular polymers with shear thickening properties as the main components of the core spinning solution, and prepares an electrospun fiber membrane with a porous structure and a core-shell structure through coaxial spinning. The electrospun fiber membrane takes into account impact resistance, sensor sensitivity, radiation cooling performance, robustness, and waterproof performance. The electrospun fiber membrane prepared by the present invention has ultra-high pressure sensitivity, ultra-high temperature sensitivity, ultra-high impact resistance, ultra-high radiation cooling performance, excellent waterproofness, wearable comfort and structural stability: its pressure sensitivity can reach 202.3kPa -1 ; Temperature sensing resolution as low as 0.1°C; At a thickness of 800 microns, it can reduce the impact force by 60%, which is 6-10 times that of daily fabrics; It can 2 The white light intensity can reduce skin temperature by 17°C; the pressure sensing performance retention rate is >98% after 10,000 bending cycles; and their impact resistance retention rate is >90% after 50 cycles of washing and drying.
[0032] 2. The electrospun fiber membrane prepared by the present invention, when the electrospun fiber membrane is subjected to stress and compression deformation, the air in the pores between the fibers is first compressed, and then the low modulus shell polymer of the core-shell structure fiber and the low modulus core layer impact polymer at low shear rate are strained, and continue to absorb part of the stress. When the stress increases to a certain extent, the modulus of the impact polymer of the core layer continues to increase, absorbing the main large stress. This compression process increases the capacitance change during the force process, thereby increasing the pressure sensing sensitivity. Moreover, this process increases the absorbable impact force and enhances the impact resistance. The role of the porous structure and the core-shell structure, the air in the pores and the impact polymer in the core layer that is transformed from solid to liquid behavior can be used as a plasticizer to soften the fiber membrane, while increasing the air permeability and moisture permeability of the membrane, and enhancing the wearable comfort. The electrospun fiber membrane prepared by the present invention is a polymer fiber membrane, which is spinnable and convenient for spinning conductive fibers such as carbon nanotube fibers as electrodes to prepare electronic fabrics with a full textile structure.
[0033] 3. The present invention uses impact-resistant polymers and radiation refrigeration polymers to construct an electrospun fiber membrane under a coaxial electrospinning method. The electrospun fiber membrane is a multifunctional, high-performance electrospun fiber membrane with a core-shell structure. The preparation method is simple, green and environmentally friendly, and convenient for mass preparation. When the present invention prepares the core layer spinning solution, the core layer polymer used has shear thickening properties and a relatively low modulus under low stress; the shell layer polymer used has impact resistance, so the prepared electrospun fiber membrane is relatively soft and has good impact resistance. The present invention prepares the shell layer spinning solution and the core layer spinning solution separately, and then uses the electrospinning technology to continuously and evenly extrude the two spinning solutions from the shell layer and the core layer of the coaxial electrospinning needle, respectively, and obtains an electrospun fiber membrane with a core-shell structure under a certain voltage. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a transmission electron microscopy image (100.0 nm) of a single filament of the electrospun fiber membrane prepared in Example 5 of the present invention;
[0035] Figure 2 This is a transmission electron microscopy image (1.0 μm) of a single filament of the electrospun fiber membrane prepared in Example 5 of the present invention;
[0036] Figure 3 The capacitance change curve of the single-layer sample of the electrospun fiber membrane prepared in Example 5 of the present invention after different compression times at a pressure of 1.6 kPa;
[0037] Figure 4 The radiative cooling performance of the electrospun fiber membrane prepared in Example 5 of the present invention after being washed 0 times;
[0038] Figure 5 The radiative cooling performance of the electrospun fiber membrane prepared in Example 5 of the present invention after being washed 5 times;
[0039] Figure 6 The radiative cooling performance of the electrospun fiber membrane prepared in Example 5 of the present invention after washing 50 times;
[0040] Figure 7 The impact force on the electrospun fiber membranes prepared from different groups;
[0041] Figure 8 The device is prepared from the electrospun fiber membrane obtained in Example 5 of the present invention. DETAILED DESCRIPTION
[0042] The technical solutions in the present invention will be described clearly and completely below in combination with the specific implementation of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] The methods described in the embodiments of the present invention are conventional methods unless otherwise specified. The materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified.
[0044] In the following description of the embodiments of the present invention, the term "and / or" is used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, B exists alone, and A and B exist at the same time. A and B may be singular or plural; the single symbol " / " means "or".
[0045] In the following description of various embodiments of the present invention, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of A, B or C", or "at least one of A, B and C" can represent any one of A, B, C, or A+B, or A+C, or B+C, or A+B+C, where A, B, C can be single or multiple, respectively.
[0046] In the following description of the embodiments of the present invention, the order of serial numbers does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of this embodiment.
[0047] In the following description of each embodiment of the present invention, the numerical range should be understood to also specifically disclose each intermediate value between the upper and lower limits of the range. Any stated value or intermediate value in the stated range and any other stated value or each smaller range between the intermediate values in the stated range are also included in this embodiment, and the upper and lower limits of the smaller range can be independently included or excluded in the range.
[0048] Unless otherwise stated, the technical / scientific terms used in the present embodiment have the same meanings as those generally understood by those skilled in the art to which the present application belongs. Although the present application only describes preferred methods and materials, any similar or equivalent methods and materials may also be used in the implementation or testing of the present application. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of any conflict with any incorporated document, the content of this specification shall prevail.
[0049] PVDF-HFP: poly(vinylidene fluoride-co-hexafluoropropylene), PBDMS: polyborosiloxane, [EMIM][TFSI]: 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, [EMIM][BF 4]: 1-ethyl-3-methylimidazolium tetrafluoroborate, PVDF: polyvinylidene fluoride, DMF: N,N-dimethylacetamide, THF: tetrahydrofuran, PU: polyurethane.
[0050] Example 1
[0051] A method for preparing an electrospun fiber membrane comprises the following steps:
[0052] (1) Preparation of shell spinning solution: PVDF-HFP was dissolved in DMF under heating and stirring at 35°C to obtain a shell solution with a concentration of 100 mg / mL. [EMIM][TFSI] with a concentration of 150 mg / mL was added to the shell solution, and heating and stirring at 35°C was continued for 4 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:0.2.
[0053] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 300 mg / mL.
[0054] (3) Preparation of electrospun fiber membrane: The shell layer spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.001 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.002 mL / min, and the electrospun fiber membrane was obtained after 7 kV voltage, roller collection, and electrospinning for 12 hours. The electrospun fiber membrane has a fiber orientation perpendicular to the roller axis, and the thickness of the single-layer electrospun fiber membrane is 100 μm and the fiber diameter is 1 μm.
[0055] (4) The electrospun fiber membrane is spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0056] Example 2
[0057] A method for preparing an electrospun fiber membrane comprises the following steps:
[0058] (1) Preparation of shell spinning solution: PVDF-HFP was dissolved in DMF under heating and stirring at 45°C to obtain a shell solution with a concentration of 100 mg / mL. 150 mg / mL of [EMIM][TFSI] was added to the shell solution, and the solution was heated and stirred at 45°C for 5 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:0.2.
[0059] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 500 mg / mL.
[0060] (3) Preparation of electrospun fiber membrane: The shell layer spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.001 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.002 mL / min, and the electrospun fiber membrane was obtained after 7 kV voltage, roller collection, and electrospinning for 10 hours. The electrospun fiber membrane has a fiber orientation perpendicular to the roller axis, and the thickness of the single-layer electrospun fiber membrane is 80 μm and the fiber diameter is 1 μm.
[0061] (4) The electrospun fiber membrane is spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0062] Example 3
[0063] A method for preparing an electrospun fiber membrane comprises the following steps:
[0064] (1) Preparation of shell spinning solution: PVDF-HFP was dissolved in DMF by heating and stirring at 55°C to obtain a shell solution with a concentration of 150 mg / mL. 150 mg / mL of [EMIM][TFSI] was added to the shell solution, and the solution was heated and stirred at 55°C for 6 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:1.0.
[0065] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 700 mg / mL.
[0066] (3) Preparation of electrospun fiber membrane: The shell layer spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.01 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.005 mL / min, and the electrospun fiber membrane was obtained after 11 kV voltage, roller collection, and electrospinning for 8 hours. The electrospun fiber membrane has a fiber orientation perpendicular to the roller axis, and the thickness of the single-layer electrospun fiber membrane is 60 μm and the fiber diameter is 1.5 μm.
[0067] (4) The electrospun fiber membrane is spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0068] Example 4
[0069] A method for preparing an electrospun fiber membrane comprises the following steps:
[0070] (1) Preparation of shell spinning solution: PVDF-HFP was dissolved in DMF under heating and stirring at 65°C to obtain a shell solution with a concentration of 200 mg / mL. 150 mg / mL of [EMIM][TFSI] was added to the shell solution, and the solution was heated and stirred at 65°C for 7 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:1.5.
[0071] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 900 mg / mL.
[0072] (3) Preparation of electrospun fiber membrane: The shell layer spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.02 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.01 mL / min, and the electrospun fiber membrane was obtained after 15 kV voltage, roller collection, and electrospinning for 4 hours. The electrospun fiber membrane has a fiber orientation perpendicular to the roller axis, and the thickness of the single-layer electrospun fiber membrane is 20 μm and the fiber diameter is 2 μm.
[0073] (4) The electrospun fiber membrane is spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0074] Example 5
[0075] A method for preparing an electrospun fiber membrane comprises the following steps:
[0076] (1) Preparation of shell spinning solution: PVDF-HFP was dissolved in DMF under heating and stirring at 80°C to obtain a shell solution with a concentration of 200 mg / mL. 150 mg / mL of [EMIM][TFSI] was added to the shell solution, and the solution was heated and stirred at 80°C for 8 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:1.5.
[0077] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 900 mg / mL.
[0078] (3) Preparation of electrospun fiber membrane: The shell layer spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.02 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.01 mL / min, and the electrospun fiber membrane was obtained after being subjected to a voltage of 15 kV, collected by a roller, and electrospun for 12 hours. The electrospun fiber membrane had a fiber orientation perpendicular to the roller axis, and the thickness of a single-layer electrospun fiber membrane was 100 μm and the fiber diameter was 2 μm.
[0079] (4) The electrospun fiber membrane is spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0080] When the thickness of the electrospun fiber membrane prepared in this embodiment is 800 μm, it can attenuate more than 60% of the impact force, and the pressure sensitivity is as high as 202.3 kPa. -1 , achieving a temperature sensing resolution of 0.1°C and a 2 The skin temperature was reduced by 17°C under white light illumination intensity of 10000℃. At the same time, the electrospun fiber membrane has high structural stability, and the pressure sensing performance retention rate is >98% after more than 10,000 bending cycles; it shows excellent waterproofness, and after 50 cycles of washing and drying, their impact resistance retention rate is >90%.
[0081] Based on Example 3, a single factor comparison test was performed:
[0082] Example 6
[0083] A method for preparing an electrospun fiber membrane comprises the following steps:
[0084] (1) Preparation of shell spinning solution: PVDF was dissolved in a mixed solution of DMF and THF at 55°C with heating and stirring to obtain a shell solution with a concentration of 150 mg / mL. The volume ratio of DMF to THF in the mixed solution was 1:1. 150 mg / mL of [EMIM][BF 4 ], and continue to heat and stir at 55℃ for 6h to obtain the shell spinning solution. 4 ] is 1:1.0.
[0085] (2) Preparation of core layer spinning solution: THF was added to PBDMS to prepare core layer spinning solution with a concentration of 700 mg / mL.
[0086] (3) Preparation of electrospun fiber membrane: The shell spinning solution prepared in (2) was extruded through the shell layer of the coaxial spinning needle at a rate of 0.01 mL / min, and the core layer spinning solution prepared in (3) was extruded through the core layer of the coaxial spinning needle at a rate of 0.005 mL / min, and the electrospun fiber membrane was obtained after 11 kV voltage, roller collection, and electrospinning for 8 h. The electrospun fiber membrane was spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0087] Example 7
[0088] A method for preparing an electrospun fiber membrane comprises the following steps:
[0089] (1) The polyurethane was dissolved in DMF under heating and stirring at 55°C to obtain a shell solution with a concentration of 150 mg / mL. 150 mg / mL of [EMIM][TFSI] was added to the shell solution, and the mixture was heated and stirred at 55°C for 6 h to obtain a shell spinning solution. The mass ratio of the shell polymer to [EMIM][TFSI] was 1:1.0.
[0090] (2) THF was added to PBDMS to prepare a core layer spinning solution with a concentration of 700 mg / mL.
[0091] (3) The shell spinning solution prepared in (2) and the core spinning solution prepared in (3) were extruded through the core layer and shell layer of the coaxial spinning needle at a rate of 0.003 mL / min: 0.005 mL / min, and then subjected to 15 kV voltage, roller collection, and electrospinning for 8 h to obtain the electrospun fiber membrane. The electrospun fiber membrane was spun into two groups of carbon nanotube fiber electrodes to obtain a wearable electronic fabric that can measure body temperature and pulse.
[0092] Comparative Example 1 (Replacing Shell Polymer)
[0093] (1) Black nylon was dissolved in a mixed solution of DMF and THF (volume ratio 1:1) under heating and stirring at 60° C. to obtain solution 1 with a concentration of 100 mg / mL.
[0094] (2) Add 150 mg / mL of [EMIM][TFSI] to solution 1, and continue heating and stirring at 60° C. for 5 h to obtain a shell spinning solution.
[0095] (3) THF was added to PBDMS to prepare solution 2 with a concentration of 900 mg / mL.
[0096] The electrospun fiber membrane was extruded through a spinning needle at a rate of 0.003 mL / min, and then collected by a roller at a voltage of 15 kV and electrospun for 12 hours to obtain the electrospun fiber membrane. According to the test, the electrospun fiber membrane absorbs heat under sunlight and cannot radiate cooling.
[0097] Comparative Example 2 (Replacing the core layer polymer)
[0098] (4) PVDF-HFP was dissolved in a mixed solution of DMF and THF (volume ratio 1:1) with heating and stirring at 60° C. to obtain solution 1 with a concentration of 100 mg / mL.
[0099] (5) Add 150 mg / mL of [EMIM][TFSI] to solution 1, and continue heating and stirring at 60° C. for 5 h to obtain a shell spinning solution.
[0100] (6) DMF was added to PU to prepare solution 2 with a concentration of 100 mg / mL.
[0101] (7) The electrospun fiber membrane was obtained by extruding the fiber through a spinning needle at a rate of 0.003 mL / min, applying a voltage of 15 kV, collecting the fiber through a roller, and electrospinning for 12 h. The electrospun fiber membrane was found to reduce the impact force by only 5%.
[0102] Comparative Example 3 (lower than the concentration of the core layer spinning solution set)
[0103] (1) PVDF-HFP was dissolved in a mixed solution of DMF and THF (volume ratio 1:1) with heating and stirring at 60° C. to obtain solution 1 with a concentration of 100 mg / mL.
[0104] (2) Add 150 mg / mL of [EMIM][TFSI] to solution 1, and continue heating and stirring at 60° C. for 5 h to obtain a shell spinning solution.
[0105] (3) DMF was added to PU to prepare solution 2 with a concentration of 100 mg / mL.
[0106] The electrospun fiber membrane was obtained by extruding the fiber through a spinning needle at a rate of 0.003 mL / min, passing through a voltage of 15 kV, collecting the fiber through a roller, and electrospinning for 12 hours. According to the test, the electrospun fiber membrane can only reduce the impact force by 15%.
[0107] Comparative Example 3 (lower than the extrusion rate of the shell spinning solution set)
[0108] (1) PVDF was dissolved in a mixed solution of DMF and THF (volume ratio 1:1) at 60° C. with heating and stirring to obtain solution 1 with a concentration of 100 mg / mL.
[0109] (2) Add 150 mg / mL of [EMIM][TFSI] to solution 1, and continue heating and stirring at 60° C. for 5 h to obtain a shell spinning solution.
[0110] (3) THF was added to PBDMS to prepare solution 2 with a concentration of 800 mg / mL.
[0111] (4) The shell layer is extruded through the spinning needle at a rate of 0.001 mL / min, and the core layer is extruded through the spinning needle at a rate of 0.005 ml / min mL / min, and then the electrospun fiber membrane is obtained after 15 kV voltage, roller collection, and electrospinning for 12 hours. After testing, the pressure sensing sensitivity coefficient of the electrospun fiber membrane is only 20 kPa. -1 .
[0112] During electrospinning, the viscosity of the spinning solution is limited, that is, the concentration of the spinning solution has certain requirements. If the concentration of the shell spinning solution is too low or too high, electrospinning cannot be performed.
[0113] Comparative Example 4 (using only shell spinning solution)
[0114] (1) PVDF-HFP was dissolved in a mixed solution of DMF and THF (volume ratio 1:1) with heating and stirring at 60° C. to obtain solution 1 with a concentration of 100 mg / mL.
[0115] (2) Add 150 mg / mL of [EMIM][TFSI] to solution 1, and continue heating and stirring at 60° C. for 5 h to obtain a shell spinning solution.
[0116] (3) Extruding through a coaxial spinning needle at a rate of 0.003 mL / min, passing through a 15 kV voltage, collecting on a roller, and electrospinning for 12 hours to obtain the electrospun fiber membrane. According to the test, the electrospun fiber membrane can only reduce the impact force by 5%, and the radiation cooling effect can only reduce the temperature by 12 degrees under one standard sunlight.
[0117] Results test:
[0118] Since the performance of the electrospun fiber membranes prepared in Examples 1 to 4, Examples 6 and 7 of the present invention is substantially consistent with the performance of the electrospun fiber membrane prepared in Example 5, only the electrospun fiber membrane prepared in Example 5 is tested below.
[0119] Figure 1 and Figure 2 The transmission electron microscope images of the single filament of the electrospun fiber membrane prepared in Example 5 of the present invention at 100 nm and 1.0 μm are shown in FIG. It can be seen from the figure that the electrospun fiber membrane has a core-shell structure. The transmission electron microscope model is JEM-2800 produced by JEOL Ltd.
[0120] Figure 3 This is the capacitance change curve of the single-layer sample of the electrospun fiber membrane prepared in Example 5 of the present invention after different compression times under a pressure of 1.6 kPa, which reflects the good sensing performance and cycle stability of the electrospun fiber membrane.
[0121] The compression process uses a universal mechanical testing machine (Shimadzu AGS-X, Japan) to give a certain force, and the capacitance test uses TH2832 from Tonghui Electronics of China.
[0122] Figure 4-6 They are respectively the states of the electrospun fiber membrane prepared in Example 5 of the present invention after different times of water washing. The sample was photographed under simulated sunlight with a light intensity of 300 watts per square meter using an infrared thermal imager, which reflects the good radiation cooling performance and water washing resistance of the electrospun fiber membrane.
[0123] Figure 7The impact force of a 370g weight on the electrospun fiber membranes of different groups at heights of 10cm, 15cm, 20cm, 25cm, and 30cm reflects the good impact resistance of the electrospun fiber membranes. The sensor uses a custom-made piezoelectric sensor from Allison.
[0124] Figure 8 The device is prepared using the electrospun fiber membrane prepared in Example 5 of the present invention, which demonstrates its practical application feasibility.
[0125] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0126] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An electrospun fiber membrane, characterized in that: Its raw material composition is: A shell spinning solution, wherein the main components of the shell spinning solution are a radiation cooling polymer and an ionic liquid; A core layer spinning solution, wherein the core layer spinning solution is mainly composed of an impact-resistant high molecular polymer with shear thickening properties; The shell layer spinning solution and the core layer spinning solution are coaxially spun to prepare an electrospun fiber membrane.
2. The electrospun fiber membrane according to claim 1, characterized in that: The electrospun fiber membrane has: Fiber orientation perpendicular to the roller axis; Single-layer fiber membrane thickness of 20-100 microns; and, a fiber diameter of 0.2-3 microns.
3. The electrospun fiber membrane according to claim 1, characterized in that: The radiation cooling polymer is any one or more of poly(vinylidene fluoride-co-hexafluoropropylene), polyvinylidene fluoride, polyvinyl alcohol, and polyurethane.
4. The electrospun fiber membrane according to claim 1, characterized in that: The ionic liquid is any one or more of 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium tetrafluoroborate, 1-ethyl-3-methylimidazolium dicyanamide, 1-butyl-3-methylimidazolium dicyanamide, 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and 1-butyl-3-methylimidazolium tetrafluoroborate.
5. The electrospun fiber membrane according to claim 1, characterized in that: The impact-resistant high molecular polymer is polyborosiloxane or polyacrylamide / organic silicon blended gel.
6. A method for preparing an electrospun fiber membrane according to claim 1, characterized in that: include: Preparing a shell spinning solution: preparing a radiation cooling polymer into a shell solution with a concentration of 100-200 mg / mL, adding an ionic liquid, and mixing to obtain a shell spinning solution; wherein the mass ratio of the radiation cooling polymer to the ionic liquid is 1:0.2-1.5; Preparing a core layer spinning solution: preparing an impact-resistant high molecular polymer into a core layer spinning solution with a concentration of 300-900 mg / mL; Preparation of electrospun fiber membrane: The prepared core layer spinning solution and shell layer spinning solution are coaxially spun and subjected to a voltage of 7-15kV to obtain an electrospun fiber membrane; wherein the mass ratio of the core layer spinning solution to the shell layer spinning solution is 0.5-2:
1.
7. The method for preparing the electrospun fiber membrane according to claim 6, characterized in that: When preparing the electrospun fiber membrane, the shell layer spinning solution is extruded through the shell layer of the coaxial spinning needle at a rate of 0.001 to 0.02 mL / min.
8. The method for preparing the electrospun fiber membrane according to claim 6, characterized in that: When preparing the electrospun fiber membrane, the core layer spinning solution is extruded through the core layer of the coaxial spinning needle at a rate of 0.002-0.01 mL / min.
9. The method for preparing the electrospun fiber membrane according to claim 6, characterized in that: The method for preparing the shell solution is: The radiation cooling polymer is heated and dissolved at 35-80° C. to prepare a shell solution with a concentration of 100-200 mg / mL.
10. Use of the electrospun fiber membrane according to claim 1 in multifunctional electronic fabrics, wearable devices, smart sportswear, space suits, and military equipment.
Citation Information
Patent Citations
Wearable flexible stress sensor and preparation method and application thereof
CN109238522A
Polyborosiloxane with shear thickening behavior and preparation method thereof
CN116874792A
Preparation method of thickening fiber for flexible protective material
CN117306019A
High-thermal-conductivity phase-change energy-storage waterproof moisture-conducting nanofiber membrane and preparation method thereof
CN117364348A
Breathable electronic skin and preparation method thereof
CN117387803A
Cited By
Multi-layer coaxial piezoelectric sensing fiber, preparation method thereof and flexible wearable fabric
CN119824577A
A core-shell structure fiber-based composite radiative cooling film and a preparation method thereof
CN122942253A