Flame-retardant modified carbon fiber, preparation method thereof and application of flame-retardant modified carbon fiber in flame-retardant

By using a random copolymer of focused piperazine phosphate-melamine polyphosphate for carbon fiber surface modification, the problem of flame retardant modification in carbon fiber reinforced polymer materials is solved, and the coordinated improvement of mechanical properties, antistatic properties and flame retardant properties is achieved. , reduce the amount of flame retardant used.

CN118996859APending Publication Date: 2024-11-22CHONGQING COPOLYFORCE NEW MATERIALS CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411372555.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to optimize mechanical properties, antistatic properties and flame retardant properties in carbon fiber reinforced polymer materials at the same time, and the addition of a large amount of flame retardant will affect the mechanical properties, and research on surface flame retardant modification methods is relatively lacking.

Method used

The surface modification of the carbon fibers was prepared by using the random copolymer of the focused piperazine phosphate-melamine polyphosphate, and the random copolymer of the focused piperazine phosphate-melamine polyphosphate was prepared by thermal polymerization and dehydration reaction, and the amino-based coupling agent was used for amino acids. Modification forms flame retardant modified carbon fibers, combined with piperazine pyrophosphate and melamine polyphosphate act as bridge and anchoring in polypropylene, enhancing the flame retardant and mechanical properties of the material.

Benefits of technology

It effectively suppresses the "candle wick effect", improves the flame retardant and mechanical properties of carbon fiber and polypropylene composite materials, and enhances the antistatic ability, reduces the amount of flame retardant added, and achieves the multiple performance improvement of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996859A_ABST
    Figure CN118996859A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flame-retardant polypropylene materials, in particular to flame-retardant modified carbon fibers, a preparation method thereof and application of the flame-retardant modified carbon fibers to flame-retardant reinforced polypropylene. The invention relates to a flame-retardant modified carbon fiber. The surface of the carbon fiber is modified with a focused piperazine phosphate-melamine polyphosphate random copolymer. The flame-retardant modified carbon fiber can be further applied to preparation of flame-retardant reinforced polypropylene, so that the technical problem that the mechanical property, the antistatic property and the flame-retardant property of carbon fiber modified polypropylene in the prior art cannot be optimized at the same time is solved. According to the scheme, the flame-retardant modified carbon fiber can eliminate or inhibit the candlewick effect and enhance the flame retardance; after the random copolymer is modified, the compatibility of the carbon fiber and the flame-retardant polypropylene can be improved, and the mechanical property of the composite material is improved; hydroxyl groups in the modified material and water molecules in air form an intermolecular force, so that the antistatic capability of the material is improved. Therefore, the flame-retardant modified carbon fiber provided by the scheme has ideal application and popularization prospects and value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame-retardant polypropylene materials, and in particular to flame-retardant modified carbon fiber and a preparation method thereof and application of the flame-retardant reinforced polypropylene thereof. Background Art

[0002] Carbon fiber (CF) is light in weight, fine in fineness and high in tensile strength. It also has the properties of general carbon materials, such as high temperature resistance, friction resistance, electrical conductivity, thermal conductivity, and small expansion coefficient. The carbon fiber composite material formed by compounding it with resin, metal, ceramic and other matrices also has a series of excellent properties such as high specific strength, specific modulus, fatigue resistance, thermal conductivity, electrical conductivity, etc., and is widely used in modern industry.

[0003] Polymer materials contain a large amount of hydrocarbon elements and are flammable. For polymer composites with added carbon fibers (polymer / CF composites), the polymer melt will infiltrate the CF surface at high temperatures and generate interfacial tension, producing a "wick effect", that is, the polymer melt will quickly infiltrate, spread and flow through the CF surface to the combustion area, further increasing the fire hazard of the polymer composites, making the flame retardant modification of polymer composites with added CF much more difficult, and limiting their development and application.

[0004] Polymer materials have excellent comprehensive properties and are widely used in transportation, electronics, defense industry and other fields. However, polymer materials have a large volume resistivity and are prone to generate and carry static electricity during use, which poses potential hazards. Among them, polypropylene (PP) is a general-purpose plastic that is inexpensive, resistant to high temperatures, has excellent corrosion resistance and comprehensive properties. However, in the chemical and coal industries, there are high requirements for the mechanical properties and antistatic properties of PP materials to meet the requirements of working pressure and antistatic during use and achieve safe production. Carbon fiber reinforced polypropylene composites combine the advantages of both, improve the shortcomings and deficiencies of raw materials, and focus on improving the mechanical properties and antistatic properties of the materials. They have broad application prospects in the fields of automobiles, ships, aerospace, transportation and so on.

[0005] In order to reduce the flammability of CF-reinforced polymer materials, the current more widespread solution is to suppress the "wick effect" by adding sufficient high-quality flame retardants to polymer / CF composites. However, the addition of a large amount of flame retardants will seriously affect the mechanical properties of polymer materials, resulting in a decrease in the gain effect of CF in polymer materials. In recent years, the method of surface flame-retardant modification of CF is still in its infancy, and there are few reports on related research. Therefore, the exploration and research of surface flame-retardant modification of CF has broad prospects. Summary of the invention

[0006] The present invention is intended to provide a flame retardant modified carbon fiber to solve the technical problem in the prior art that the mechanical properties, antistatic properties and flame retardant properties of carbon fiber modified polypropylene cannot be optimized at the same time.

[0007] In order to achieve the above object, the present invention adopts the following technical scheme:

[0008] A flame retardant modified carbon fiber, the surface of the carbon fiber is modified with a random copolymer of focused piperazine phosphate-melamine polyphosphate as shown in formula (10); in formula (10), MPP represents melamine polyphosphate with a chemical formula as shown in formula (8), and PAPP represents focused piperazine phosphate with a chemical formula as shown in formula (1);

[0009]

[0010] Among them, 500<m<10000, 500<n<10000, x>0, y>0, p>0, and the mass ratio of PAPP and MPP is 1:0.2-5.

[0011] Furthermore, the flame retardant modified carbon fiber comprises 80-160 parts by weight of carbon fiber modified by amino reaction and 0.1-5 parts by weight of focused piperazine phosphate-melamine polyphosphate random copolymer.

[0012] The present technical solution also provides a method for preparing a flame retardant modified carbon fiber, comprising the following steps performed in sequence:

[0013] S1: focusing piperazine phosphate and melamine polyphosphate in a mass ratio of 1:0.2-5, under the reaction conditions of 200-280°C and 0.1-1.5MPa nitrogen atmosphere, undergoing a thermal polymerization dehydration reaction for 30-180min to obtain a focusing piperazine phosphate-melamine polyphosphate random copolymer;

[0014] Preferably, the focused piperazine phosphate and melamine polyphosphate are in a mass ratio of 1:0.7, and are subjected to a thermal polymerization dehydration reaction for 180 minutes under the reaction conditions of 250° C. and 0.4 MPa nitrogen atmosphere to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer;

[0015] S2: Use 1-5 parts by mass of an amino coupling agent to perform surface modification on 100 parts by mass of carbon fiber to obtain amino-modified carbon fiber; use 0.1-5 parts by mass of focused piperazine phosphate-melamine polyphosphate random copolymer to perform surface modification on 80-160 parts by mass of amino-modified carbon fiber to obtain flame-retardant modified carbon fiber.

[0016] Further, in S1, focused piperazine phosphate is obtained by the following method: piperazine diphosphate is heat treated for 30-240 min in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a condition of 120-320° C. to thermally polymerize and dehydrate and condense into focused piperazine phosphate.

[0017] Furthermore, in S1, melamine polyphosphate is obtained by the following method: melamine phosphate is heat-treated for 60-300 min in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize and dehydrate to condense into melamine polyphosphate.

[0018] Further, in S2, the carbon fiber is dispersed in an ethanol solution, and then an amino coupling agent is added, and the mixture is reacted at 60-100° C. for 4-8 hours to obtain amino-modified carbon fiber.

[0019] Further, in S2, the amino-modified carbon fiber is dispersed in a solvent, and then the amino-modified carbon fiber is added and reacted at 20-50° C. for 2-12 hours to obtain a flame-retardant modified carbon fiber.

[0020] The technical solution also provides an application of flame-retardant modified carbon fiber in the preparation of flame-retardant reinforced polypropylene. The raw materials of the flame-retardant reinforced polypropylene include, by weight: 30-60 parts of polypropylene, 5-60 parts of flame-retardant modified carbon fiber, 5-20 parts of piperazine pyrophosphate, 5-20 parts of melamine polyphosphate, 0.5-5 parts of flame retardant synergist, 1-6 parts of maleic anhydride grafted PP, 0.5-3 parts of coupling agent, 0.3-3 parts of lubricant, and 0.2-0.5 parts of antioxidant.

[0021] Furthermore, the polypropylene has a melt index of any one or a mixture of melt index>0g / 10min and <100g / 10min under the conditions of temperature 230°C and load 2.16kg; the 1% thermal weight loss of melamine polyphosphate is ≥360°C; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-water zinc borate, zinc oxide, and zirconium phosphate; the coupling agent is a silane coupling agent, including at least one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006 and KH-9130; the lubricant includes at least one of white oil, silicone oil, polyethylene wax, ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax; the antioxidant includes at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098.

[0022] Furthermore, the flame retardant reinforced polypropylene is prepared by the following method: piperazine pyrophosphate, melamine polyphosphate and a flame retardant synergist are added to a mixer and stirred at room temperature for 5-30 minutes; the temperature of the mixer is increased to 80-160°C, and a coupling agent is added and stirred for 10-30 minutes; after cooling to room temperature, polypropylene, a lubricant, a nucleating agent and an antioxidant are added and stirred for 5-30 minutes to obtain a material mixture; the material mixture is extruded by a twin-screw extruder at an extrusion temperature of 170-250°C, flame retardant modified carbon fiber is added by side feeding, and flame retardant reinforced polypropylene granules are obtained after extrusion, drawing, pelletizing and screening dehydration.

[0023] In summary, the present invention modifies the surface of carbon fiber, and coats the macromolecular intumescent flame retardant with excellent carbonization effect on the surface of carbon fiber, so that the polymer / CF composite material quickly forms an intumescent, dense and hard carbon layer on the surface of CF at high temperature, thereby greatly inhibiting the "wick effect"; and after the CF surface is modified with a focused piperazine phosphate-melamine polyphosphate random copolymer (PAPP-co-MPP) with a certain molecular chain, the compatibility of carbon fiber and flame-retardant polypropylene can be improved, which plays a bridge and anchoring role between CF and other flame retardants / polypropylene, thereby improving the mechanical properties of its flame-retardant enhanced polypropylene, and the flame retardant has hydroxyl groups, and the hydroxyl groups on the surface of some strips and the water molecules in the air form intermolecular forces, thereby improving the antistatic ability of the material. Focused piperazine phosphate and melamine polyphosphate are prepared in the form of random copolymers, which can give full play to the synergistic effect of the two in enhancing mechanical properties, improving flame retardant properties and increasing antistatic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the amino modification and flame retardant modification of carbon fiber in Example 1. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.

[0026] Example 1: Preparation process of modified carbon fiber

[0027] (1) Focus on the synthesis of piperazine phosphate (PAPP)

[0028] The structure of the focused piperazine phosphate is shown in formula (1), n=500-10000, and it is synthesized from piperazine diphosphate (formula (4)). The synthesis of piperazine diphosphate is a conventional method in the prior art (using a conventional reactor in the prior art), specifically, phosphoric acid (formula (2)) and piperazine (formula (3)) are used in a molar ratio of 2.0-2.2:1, under reaction conditions of 60-150°C and 0.1-1.0MPa (in a reaction system with water or alcohol as solvent), and the reaction is carried out for 30-300 minutes to obtain. The reaction equation is shown in formula (5).

[0029] The piperazine diphosphate obtained and purified by the above-mentioned chemical reaction is heat-treated in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 120-320° C. for 30-240 min to undergo thermal polymerization, dehydration, and condensation to obtain piperazine phosphate (Formula (1)). The reaction equation is shown in Formula (6).

[0030]

[0031] (2) Synthesis of melamine polyphosphate (MPP)

[0032] Using deionized water as solvent, melamine (ME) and H3PO4 are reacted by acid-base neutralization to prepare melamine phosphate (MP) with high purity, high whiteness and high thermal stability, and then MP is subjected to high-temperature thermal polymerization to obtain melamine polyphosphate (MPP). The above synthesis process can be found in the inventor's previously published paper "Zhong Zhiqiang, Synthesis of Melamine Polyphosphate and Properties of Flame-Retardant Polypropylene, Engineering Plastics Application, 2018". Specifically, in this embodiment, the method for preparing melamine phosphate is: the molar ratio of ME to H3PO4 is 1:1.05, the reaction time is 2.0h, the reaction temperature is 95°C, and the molar ratio of ME to deionized water is 3:97. Melamine phosphate (Formula (7)) was synthesized under the above conditions.

[0033] Then, melamine phosphate is used to synthesize melamine polyphosphate (MPP). Melamine phosphate is heat treated at 220-360° C. for 60-300 min, in an inert gas environment (such as nitrogen) and under a pressure of 0.05-0.3 MPa, and thermally polymerized and dehydrated to form melamine polyphosphate (MPP, formula (8), 500<m<10000), and the reaction formula is shown in formula (9).

[0034]

[0035] (3) Focus on the synthesis of piperazine phosphate (PAPP)-melamine polyphosphate (MPP) random copolymer (PAPP-co-MPP)

[0036] Focused piperazine phosphate and melamine polyphosphate are reacted at a mass ratio of 1:0.2-5 under reaction conditions of 200-280°C and 0.1-1.5MPa (nitrogen atmosphere) for 30-180 minutes, and then thermally polymerized and dehydrated to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer (PAPP-co-MPP), the structural formula of which is shown in Formula (10), and the reaction equation of which is shown in Formula (11). The polymerization degrees of focused piperazine phosphate (PAPP, Formula (6)) and melamine polyphosphate (MPP, Formula (8)) are both greater than 500 and less than 10000, that is, 500<m<10000, and 500<n<10000. In Formula (10), x>0, y>0, and p>0, and in PAPP-co-MPP, the mass ratio of PAPP to MPP is 1:0.2-5.

[0037]

[0038] (4) Amide modification of carbon fiber (CF-NH2)

[0039] Disperse 100 g of carbon fiber CF (T300 (6K), Toray, Japan, cut to a length of 2.5-7.5 mm) in ethanol / water (250-750 ml, for example, a 450:50 ethanol solution), add 1-5 wt % of an amino coupling agent (KH550, etc.) under high-speed stirring (200-1500 rpm), raise the temperature from room temperature to 60-100 ° C and react for 4-8 hours. After the reaction is completed, filter, wash and dry at 80 ° C to obtain CF-NH2.

[0040] (5) Preparation of flame-retardant modified carbon fiber (CF-NH2-FR)

[0041] CF-NH2 (80-160 g) is dispersed in 200-1000 mL of solvent (ethanol, water, DMF, DMSO, acetonitrile and other organic solvents), PAPP-co-MPP (0.1-5 g) is added to the solution, and the reaction is continued at 20-50 ° C for 2-12 hours, and the stirring speed is maintained at 50-1500 rpm. After the reaction is completed, filter, wash and dry at 80 ° C to obtain CF-NH2-FR.

[0042] The schematic diagram of the synthesis process of steps (4) and (5), the schematic diagram of the amino modification of carbon fiber (CF-NH2) and its flame retardant modification (CF-NH2-FR) are shown in detail. Figure 1 .

[0043] Example 2: Preparation process of flame retardant reinforced polypropylene

[0044] The flame-retardant carbon fiber reinforced polypropylene composition comprises the following raw material components in parts by weight: 30-60 parts of polypropylene, 5-60 parts of CF-NH2-FR, 5-20 parts of piperazine pyrophosphate (i.e., focused piperazine phosphate, commercially available or prepared according to the aforementioned method), 5-20 parts of melamine polyphosphate (commercially available or prepared according to the aforementioned method), 0.5-5 parts of flame retardant synergist, 1-6 parts of maleic anhydride grafted PP, 0.5-3 parts of coupling agent, 0.3-3 parts of lubricant, and 0.2-0.5 parts of antioxidant. In addition to having good flame retardancy, the flame-retardant polypropylene composition also has very excellent precipitation resistance.

[0045] The polypropylene is any one or a mixture of the following: a melt index of >0 g / 10 min and <100 g / 10 min under the conditions of a temperature of 230° C. and a load of 2.16 kg.

[0046] The 1% thermal weight loss of the melamine polyphosphate is ≥360°C.

[0047] The flame retardant synergist is any one of anhydrous zinc borate, zinc sulfide, 3.5-hydrate zinc borate, zinc oxide, and zirconium phosphate, or a mixture of several of them.

[0048] The coupling agent is a silane coupling agent, which can be any one of aminosilane coupling agent KH-9120, isocyanate silane coupling agent KT-930, epoxy silane coupling agent KH-1006 and KH-9130, or a mixture of several of the silane coupling agents.

[0049] The lubricant is one or more of white oil, silicone oil, polyethylene wax, ethylene bis stearamide (EBS), pentaerythritol stearate, silicone and amide wax.

[0050] The antioxidant is antioxidant 168, antioxidant 1010 or antioxidant 1098.

[0051] The preparation process is as follows:

[0052] Step 1: Add piperazine pyrophosphate, melamine polyphosphate and flame retardant synergist into a mixer and stir at room temperature for 5-30 minutes;

[0053] Step 2: In the mixture of step 1, increase the temperature of the mixer to 80-160°C, ensure that the temperature of the material in the mixer also reaches the set temperature, then add the coupling agent and continue stirring for 10-30 minutes;

[0054] Step 3: After cooling the mixture in step 2 to room temperature, add polypropylene, lubricant, maleic anhydride grafted PP and antioxidant, and stir for 5-30 minutes;

[0055] Step 4: The mixture of step 3 is extruded by a twin-screw extruder at a temperature of 170-250°C. CF-NH2-FR is added by side feeding. The mixture is then subjected to the processes of strip drawing and pelletizing, and then sieved and dehydrated to obtain flame-retardant reinforced polypropylene granules.

[0056] Experimental Example 1

[0057] Phosphoric acid and piperazine are mixed in a molar ratio of 2.05:1, and reacted for 210 minutes at 80°C and 0.1MPa in an ethanol aqueous solution environment (ethanol volume fraction 50%, phosphoric acid mass fraction of ethanol aqueous solution can be selected to be 5%-30%, 15% in specific experimental operation), and then purified and dried to obtain the intermediate diphosphate piperazine. The intermediate diphosphate piperazine is heat treated at 290°C and 0.1MPa nitrogen atmosphere for 240 minutes, and thermally polymerized and dehydrated to form focused phosphate piperazine (PAPP, 500<n<10000). Melamine phosphate is synthesized according to the method of Example 1, and melamine phosphate is heat treated at 320°C for 240 minutes, and thermally polymerized and dehydrated to form melamine polyphosphate (MPP, 500<m<10000) in an inert gas environment (nitrogen) and a pressure environment of 0.15MPa.

[0058] The focused piperazine phosphate obtained in the above steps and melamine polyphosphate were mixed (according to the mass ratio of PAPP:MPP = 1:0.7), and thermally polymerized at 250°C for 180min under a nitrogen atmosphere of 0.4MPa to obtain PAPP-co-MPP. After a large number of experimental studies, the PAPP-co-MPP prepared according to the above technical parameters was applied to carbon fiber modification, and a polypropylene composite material was prepared. The polypropylene composite material can obtain more excellent effects in mechanical properties, antistatic properties and flame retardant properties, which is the optimal parameter for preparing PAPP-co-MPP for carbon fiber modification and preparing polypropylene composite materials adopted in this scheme. As a comparison, for example, a polypropylene composite material prepared by a PAPP:MPP mass ratio of 1:0.6 and a pressure environment of 0.2MPa (except for the above differences, the rest is prepared by referring to the method of Experimental Example 1), and its flame retardancy UL 94 (1.0mm) is V-2 level.

[0059] Disperse 100g of carbon fiber CF (chopped CF, T300 (6K), Toray, Japan, length of about 5mm) in ethanol / water (500ml, 450:50), add 1wt% (1g) of amino coupling agent KH550 under high-speed stirring (about 1000rpm), raise the temperature from room temperature to 90℃ for 6h, and after the reaction is completed, filter, wash and dry at 80℃ to obtain CF-NH2.

[0060] CF-NH2 (100 g) was evenly dispersed in an ethanol solution (500 ml, 400:100), PAPP-co-MPP (1 g) was added to the solution, and the reaction was continued at 50 °C for 11 h, and the stirring speed was maintained at about 500 rpm. After the reaction was completed, CF-NH2-FR was obtained by filtering, washing, and drying at 80 °C.

[0061] The flame retardant reinforced polypropylene composition comprises the following raw material components in parts by weight: 57 parts of PP Z30S, 20 parts of CF-NH2-FR, 12 parts of piperazine pyrophosphate (synthesized by the above method), 6 parts of melamine polyphosphate (synthesized by the above method), 1 part of zinc sulfide, 2.5 parts of maleic anhydride ester PP (KT-1), 0.5 parts of coupling agent KH1006, 0.5 parts of ethylene bis stearamide, 0.2 parts of antioxidant 1010, and 0.3 parts of antioxidant 168. Among them, the addition amount of the flame retardant is 18% of the flame retardant (piperazine pyrophosphate + melamine polyphosphate).

[0062] Specifically, the flame retardant enhanced polypropylene composition is prepared according to the following method:

[0063] Step 1: Add piperazine pyrophosphate, melamine polyphosphate and flame retardant synergist into a mixer and stir at room temperature for 30 minutes;

[0064] Step 2: In the mixture of step 1, increase the temperature of the mixer to 140°C, ensure that the temperature of the material in the mixer also reaches the set temperature, then add the coupling agent and continue stirring for 30 minutes;

[0065] Step 3: After the mixture in step 2 is cooled to room temperature, polypropylene, lubricant, maleic anhydride ester PP and antioxidant are added and stirred for 30 minutes;

[0066] Step 4: The mixture of step 3 is extruded by a conventional twin-screw extruder in the prior art, CF-NH2-FR is added by side feeding, and then through the process of drawing and pelletizing, sieving and dehydrating to obtain flame-retardant reinforced polypropylene granules. The temperature of the twin-screw extruder is set to 170-250°C (preferably 180-220°C). More specifically, it can be set as follows: the twin-screw extruder is divided into 10 temperature zones, and the temperatures of each temperature zone are 180, 190, 200, 210, 220, 220, 210, 200, 190, 180°C in the order of material movement.

[0067] Experimental Example 2

[0068] This experimental example is basically the same as the experimental example 1, except that the amount of the flame retardant added is 15% (piperazine pyrophosphate + melamine polyphosphate).

[0069] The specific formula of the flame retardant reinforced polypropylene composition is: 60 parts of PP Z30S; 20 parts of CF-NH2-FR; 10 parts of piperazine pyrophosphate; 5 parts of melamine phosphate; 1 part of zinc sulfide; 2.5 parts of maleic anhydride ester PP; 0.5 parts of coupling agent KH1006; 0.5 parts of EBS; 0.2 parts of antioxidant 1010 and 0.3 parts of antioxidant 168.

[0070] Comparative Experiment Example 1

[0071] The same method as in Experimental Example 1 was used, but an equal amount of untreated chopped CF was used instead of CF-NH2-FR to prepare a flame retardant reinforced polypropylene composition.

[0072] Comparative Experiment Example 2

[0073] The same method as in Experimental Example 2 was used, but an equal amount of untreated chopped CF was used instead of CF-NH2-FR to prepare a flame retardant reinforced polypropylene composition.

[0074] Comparative Experiment 3

[0075] The flame retardant reinforced polypropylene composition was prepared in the same manner as in Experimental Example 1, except that CF-NH2 was used in an equal amount instead of CF-NH2-FR. The specific preparation method of CF-NH2 is shown in Experimental Example 1.

[0076] Comparative Experiment Example 4

[0077] The same method as in Experimental Example 1 is used, but an equal amount of PAPP-modified CF (CF-NH2-PAPP) is used to replace CF-NH2-FR to prepare a flame retardant reinforced polypropylene composition. The preparation method of CF-NH2-PAPP is similar to that in Experimental Example 1, except that an equal amount of PAPP-co-MPP in Experimental Example 1 is replaced by focused piperazine phosphate (PAPP), and the preparation method of focused piperazine phosphate is also the same as that in Experimental Example 1.

[0078] Comparative Experiment Example 5

[0079] The same method as in Experimental Example 1 is used, but an equal amount of MPP-modified CF (CF-NH2-MPP) is used to replace CF-NH2-FR to prepare a flame retardant reinforced polypropylene composition. The preparation method of CF-NH2-MPP is as in Experimental Example 1, except that an equal amount of PAPP-co-MPP in Experimental Example 1 is replaced by melamine polyphosphate (MPP), and the preparation method of melamine polyphosphate is also the same as in Experimental Example 1.

[0080] Comparative Experiment Example 6

[0081] The same method as in Experimental Example 1 is used, but CF (CF-NH2-PAPP / MPP) modified with PAPP and MPP is used in equal amounts instead of CF-NH2-FR to prepare a flame retardant reinforced polypropylene composition. The preparation method of CF-NH2-PAPP / MPP is similar to that in Experimental Example 1, except that 1 g of PAPP-co-MPP in Experimental Example 1 is replaced with a mixture of PAPP and MPP in a mass ratio of 1:0.7, and the preparation method of focused piperazine phosphate and melamine polyphosphate is also the same as that in Experimental Example 1.

[0082] Comparative Experiment Example 7

[0083] Basically the same as comparative experimental example 1, but without adding any flame retardant, the specific formula is:

[0084] PP Z30S 75 parts, short chopped CF 20 parts, zinc sulfide 1 part, maleic anhydride ester PP (KT-1) 2.5 parts, coupling agent KH1006 0.5 parts, ethylene bis stearamide 0.5 parts, antioxidant 1010 0.2 parts, antioxidant 168 0.3 parts. According to the above formula, a reinforced polypropylene composition was prepared.

[0085] The formula compositions of the experimental examples and comparative experimental examples are summarized in Table 1, and the experimental results are shown in Table 2.

[0086] Table 1: Composition of the formula of the experimental example and the comparative experimental example

[0087]

[0088]

[0089] The flame retardant polypropylene composite materials (flame retardant enhanced polypropylene compositions) synthesized in the experimental examples and comparative experimental examples were subjected to performance tests. The performance indicators include flame retardancy test, oxygen index (LOI) test, surface resistance, tensile strength, and notched impact strength. The flame retardancy test was conducted according to Test for Flammability of Plastic Materials for Parts in Devices and Appliances-UL 94. The reference standard for oxygen index (LOI) test is GB / T 2406. The reference standard for surface resistance is MT 113. The reference standard for tensile strength is GB / T1040. The reference standard for notched impact strength is GB / T1843.

[0090] Table 2: Test results of various properties of the flame retardant reinforced polypropylene compositions synthesized in the experimental examples and comparative experimental examples (the experimental results are the average values ​​of three independent repeated experiments)

[0091]

[0092] It can be seen from the above data that the flame-retardant polypropylene composite material prepared according to the technical solution has relatively ideal mechanical strength, antistatic properties and flame retardant properties (Experimental Example 1).

[0093] The carbon fiber used in the flame-retardant polypropylene composite material of comparative experimental example 1 is a traditional carbon fiber that has not been modified. When it is added to the flame-retardant polypropylene composite material, the mechanical properties, antistatic properties and flame retardant properties are not ideal compared with experimental example 1. The inventor analyzed the reason as follows: in terms of flame retardant properties, the newly synthesized focused piperazine phosphate-melamine polyphosphate (MPP) random copolymer (PAPP-co-MPP) of the present technical scheme has the acid source, carbon source and gas source required for the intumescent flame retardant, and is a new type of macromolecular intumescent flame retardant. After CF is modified with PAPP-co-MPP, it is added to the polypropylene composite material to increase the flame retardant properties of the composite material. CF is modified with PAPP-co-MPP on the surface to eliminate or inhibit the "wick effect" and enhance the flame retardant properties. In terms of mechanical properties, after the CF surface is modified with PAPP-co-MPP, the compatibility of carbon fiber and flame-retardant polypropylene can also be improved. It plays a bridge and anchoring role between carbon fiber and other flame retardants / polypropylene, thereby improving the mechanical properties of its flame-retardant enhanced polypropylene. In terms of antistatic performance, the conductivity of CF itself, coupled with the modification of the CF surface with PAPP-co-MPP, due to the hydroxyl group of the flame retardant, the hydroxyl groups on the surface of some strips and the water molecules in the air form intermolecular forces, which improves the antistatic ability of the material. It can be seen that the surface PAPP-co-MPP modification of CF has achieved triple effects, which was not expected by the inventors before the study. The comparison between Experimental Example 2 and Comparative Experimental Example 2 also shows the triple effects of the surface modification of CF with PAPP-co-MPP.

[0094] If the amount of flame retardant added is reduced (piperazine pyrophosphate + melamine polyphosphate, Experimental Example 2), the flame retardant properties of the material will deteriorate relative to those of Experimental Example 1. However, the flame retardant effect of Experimental Example 2 is similar to that of Comparative Example 1. Comparative Example 1 is a traditional carbon fiber case, and the flame retardant performance is equivalent to the level of Example 2 of this scheme, but the amount of flame retardant added in Example 2 is lower, and the antistatic effect and mechanical properties are better. This shows that the method of modifying the CF surface with PAPP-co-MPP can reduce the amount of a single flame retardant added because it can enhance the flame retardant effect of the composite material.

[0095] Compared with Experimental Example 1, in Comparative Experimental Example 3, only CF was aminated, and the mechanical properties, antistatic properties and flame retardant properties of the composite material deteriorated. Comparative Experimental Example 3 was aminated on the basis of Comparative Experimental Example 1, but the mechanical properties, antistatic properties and flame retardant properties did not change significantly, which shows that CF aminated modification is not suitable for preparing the composite material of this scheme.

[0096] Comparative Experimental Example 4 carried out PAPP modification of CF on the basis of Comparative Experimental Example 1, and Comparative Experimental Example 5 carried out MPP modification of CF on the basis of Comparative Experimental Example 1. Although the amounts of CF-NH2-FR, CF-NH2-PAPP, and CF-NH2-MPP were consistent in the process of preparing the composite material, and the amounts of PAPP-co-MPP, PAPP, and MPP were consistent in the process of modifying CF, the composite materials of Comparative Experimental Example 4 and Comparative Experimental Example 5 still had very significant differences in mechanical properties, antistatic properties, and flame retardant properties compared with Experimental Example 1. This shows that the use of PAPP and MPP to jointly modify CF has a synergistic effect in improving mechanical properties, antistatic properties, and flame retardant properties.

[0097] However, it is not possible to achieve the synergistic effect by simply modifying CF with PAPP and MPP. In Comparative Experiment 6, PAPP and MPP did not form a random copolymer, and the mechanical properties, antistatic properties, and flame retardant properties of the obtained composite material were not much different from those of Comparative Experiment 4 and Comparative Experiment 5, and the synergistic effect did not occur.

[0098] In addition, Comparative Experiment 7 used unmodified CF and did not add any flame retardant. Compared with Comparative Experiment 1 (using unmodified CF but adding flame retardant), it shows that the piperazine pyrophosphate and melamine polyphosphate flame retardants prepared in this scheme have a certain flame retardant effect, but in the case that CF is not modified with PAPP-co-MPP, the amount of flame retardant added in Comparative Experiment 1 is not enough to improve the flame retardant effect of the composite material to an ideal level.

[0099] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A flame retardant modified carbon fiber, characterized in that: The carbon fiber surface is modified with a focused piperazine phosphate-melamine polyphosphate random copolymer as shown in formula (10); in formula (10), MPP represents melamine polyphosphate with a chemical formula as shown in formula (8), and PAPP represents focused piperazine phosphate with a chemical formula as shown in formula (1); Among them, 500<m<10000, 500<n<10000, x>0, y>0, p>0, and the mass ratio of PAPP and MPP is 1:0.2-5.

2. The flame retardant modified carbon fiber according to claim 1, characterized in that: The raw materials include 80-160 parts by weight of carbon fibers modified by amino and 0.1-5 parts by weight of focused piperazine phosphate-melamine polyphosphate random copolymer.

3. The method for preparing a flame retardant modified carbon fiber according to claim 1 or 2, characterized in that: The method includes the following steps: S1: focusing piperazine phosphate and melamine polyphosphate in a mass ratio of 1:0.2-5, under the reaction conditions of 200-280°C and 0.1-1.5MPa nitrogen atmosphere, undergoing a thermal polymerization dehydration reaction for 30-180min to obtain a focusing piperazine phosphate-melamine polyphosphate random copolymer; Preferably, the focused piperazine phosphate and melamine polyphosphate are in a mass ratio of 1:0.7, and are subjected to a thermal polymerization dehydration reaction for 180 minutes under the reaction conditions of 250° C. and 0.4 MPa nitrogen atmosphere to obtain a focused piperazine phosphate-melamine polyphosphate random copolymer; S2: Use 1-5 parts by mass of an amino coupling agent to perform surface modification on 100 parts by mass of carbon fiber to obtain amino-modified carbon fiber; use 0.1-5 parts by mass of focused piperazine phosphate-melamine polyphosphate random copolymer to perform surface modification on 80-160 parts by mass of amino-modified carbon fiber to obtain flame-retardant modified carbon fiber.

4. The method for preparing a flame retardant modified carbon fiber according to claim 3, characterized in that: In S1, focused piperazine phosphate is obtained by the following method: piperazine diphosphate is heat treated for 30-240 min in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 120-320° C. to obtain focused piperazine phosphate by thermal polymerization and dehydration condensation.

5. The method for preparing a flame retardant modified carbon fiber according to claim 3, characterized in that: In S1, melamine polyphosphate is obtained by the following method: melamine phosphate is heat-treated for 60-300 minutes in a nitrogen atmosphere, a pressure environment of 0.05-0.3 MPa, and a temperature of 220-360° C. to thermally polymerize, dehydrate, and condense into melamine polyphosphate.

6. The method for preparing a flame retardant modified carbon fiber according to claim 3, characterized in that: In S2, the carbon fiber is dispersed in an ethanol solution, and then an amino coupling agent is added under stirring conditions of 200-1500 rpm, and the mixture is reacted at 60-100° C. for 4-8 hours to obtain amino-modified carbon fiber.

7. The method for preparing a flame retardant modified carbon fiber according to claim 6, characterized in that: In S2, the amino modified carbon fiber is dispersed in a solvent, and then the focused piperazine phosphate-melamine polyphosphate random copolymer is added and reacted at 20-50° C. for 2-12 hours to obtain a flame retardant modified carbon fiber.

8. Use of a flame retardant modified carbon fiber according to claim 1 or 2 in the preparation of flame retardant reinforced polypropylene, characterized in that: The raw materials include, by weight: 30-60 parts of polypropylene, 5-60 parts of flame-retardant modified carbon fiber, 5-20 parts of piperazine pyrophosphate, 5-20 parts of melamine polyphosphate, 0.5-5 parts of flame-retardant synergist, 1-6 parts of maleic anhydride grafted PP, 0.5-3 parts of coupling agent, 0.3-3 parts of lubricant and 0.2-0.5 parts of antioxidant.

9. The use of a flame retardant modified carbon fiber in the preparation of flame retardant reinforced polypropylene according to claim 8, characterized in that: The polypropylene has a melt index of any one or a mixture of melt index>0g / 10min and <100g / 10min under the conditions of temperature 230°C and load 2.16kg; the 1% thermal weight loss of melamine polyphosphate is ≥360°C; the flame retardant synergist includes at least one of anhydrous zinc borate, 3.5-water zinc borate, zinc oxide, and zirconium phosphate; the coupling agent is a silane coupling agent, including at least one of KH-9120, KT-930, KH-1006 and KH-9130; the lubricant includes at least one of white oil, silicone oil, polyethylene wax, ethylene bis stearamide, pentaerythritol stearate, silicone and amide wax; the antioxidant includes at least one of antioxidant 168, antioxidant 1010 and antioxidant 1098.

10. The use of a flame retardant modified carbon fiber in the preparation of flame retardant reinforced polypropylene according to claim 9, characterized in that: The flame retardant reinforced polypropylene is prepared by the following method: piperazine pyrophosphate, melamine polyphosphate and a flame retardant synergist are added into a mixer, and stirred at room temperature for 5-30 minutes; the temperature of the mixer is increased to 80-160°C, and a coupling agent is added and stirred for 10-30 minutes; after cooling to room temperature, polypropylene, a lubricant, a nucleating agent and an antioxidant are added, and stirred for 5-30 minutes to obtain a material mixture; the material mixture is extruded by a twin-screw extruder, the extrusion temperature is 170-250°C, flame retardant modified carbon fiber is added by side feeding, and flame retardant reinforced polypropylene granules are obtained after extrusion, drawing, pelletizing and screening dehydration.

Citation Information

Cited By

  • Flame-retardant polypropylene composite material for vehicles and preparation method of flame-retardant polypropylene composite material

    CN120623647A