Flexible protective material and preparation method thereof
By combining the shear-thickening fluid coating with fabric, using acrylic block low molecular weight copolymer as a dispersing solvent, the problems of poor bonding performance and slow response speed in the prior art are solved, and a high-performance flexible protective material is realized Prepared with faster response speed and better impact resistance.
Patent Information
- Application Number
- CN202411300651.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
AI Technical Summary
Existing flexible protective materials based on shear thickening fluids have shortcomings in bonding performance, response speed and impact resistance, and the preparation process is complex and time-consuming.
A method of preparing a combination of shear thickening fluid coating and fabrics, wherein the shear thickening fluid coating contains nanoparticles and a dispersion solvent, which comprises at least an acrylic block low molecular weight copolymer, which is combined with a spray or impregnation method. The fabric is combined to form a high-performance protective material.
It achieves higher bond strength, faster response speed and wider temperature application range, simplifies the preparation process, improves impact resistance and protective effect, and reduces the use of fabric fibers.
Smart Images

Figure CN118996864A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a flexible protective material and a preparation method thereof, belonging to the technical field of flexible protective materials. Background Art
[0002] Shear-thickening fluids (STFs) are soft materials with smart material properties that can withstand higher external forces than liquids and exhibit shape-changing properties different from solids, which gives them great potential in applications such as cushioning and shock absorption and human protection.
[0003] Existing new flexible protective materials based on shear thickening fluid (STF), such as an ultra-high molecular weight polyethylene fabric composite flexible protective material invented by Nanjing University of Science and Technology (CN103808210A), are impregnated with shear thickening fluid, the nanoparticles are SiO2 with a particle size of 500nm, and the dispersion medium is polyethylene glycol (PEG). At the same time, the modified discontinuous short fibers must be evenly dispersed in the shear thickening fluid, which increases the complexity of preparation. And the preparation process can only be done by dipping, which consumes more STF raw materials than the coating method and takes longer time. The shear thickening diluent used in a shear thickening liquid composite graphene sponge protective material (CN110655072A) is SiO2, polyethylene glycol (PEG) and ethanol. The interaction mainly depends on the special structure of the graphene sponge protective material, which is a good interaction that can be achieved with ordinary fabrics. A bulletproof composite fiber material and its preparation method (CN113122959A) use coaxial electrospinning to form a fiber web to suppress the fluidity of the STF material, and alternately overlap N layers of woven fabric and N-1 layers of fiber web. The preparation process is complicated, and the STF material cannot actually bond with the N layers of woven fabric.
[0004] Therefore, at present, the bonding performance between STF and fabric is poor, and the response speed and impact resistance need to be improved. Summary of the invention
[0005] The main purpose of the present invention is to provide a flexible protective material and a preparation method thereof to overcome the deficiencies of the prior art.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0007] An embodiment of the present invention provides a flexible protective material, which includes: a combined shear-thickening fluid coating and a fabric; the shear-thickening fluid coating includes nanoparticles and a dispersion solvent, wherein the dispersion solvent includes at least an acrylic block low molecular weight copolymer.
[0008] In some embodiments, the dispersing solvent includes a combination of a first component and a second component, wherein the first component includes any one or a combination of two of silica gel, hydroxy silicone oil, ethylene glycol, propylene glycol, butylene glycol, polyethylene glycol and polypropylene glycol, and the second component includes an acrylic block low molecular weight copolymer.
[0009] In some embodiments, the acrylic block low molecular weight copolymer comprises at least a first segment having a controlled molecular weight and position and a second segment having a controlled molecular weight and position; wherein the first segment comprises a segment formed by polymerization of at least any one of the monomers having a structure as shown in formula (I):
[0010]
[0011] Wherein, R includes H or CH3, and X includes any one or a combination of two or more of a cross-linkable silyl group, a hydroxyl group, a carboxyl group, a carbonyl group, a carbonate group, an isocyanate group, an epoxy group, a vinyl group, an amino group, a mercapto group, an acetoacetyl group, an alkoxymethylol group, and a cyclic ether group;
[0012] The second segment includes a segment formed by polymerization of at least one of the monomers having a structure as shown in formula (II):
[0013]
[0014] Wherein, R1 includes H or CH3, and R2 includes a branched or unbranched saturated alkyl group having 4 to 14 carbon atoms.
[0015] The embodiment of the present invention further provides a method for preparing the aforementioned flexible protective material, which comprises: combining a shear thickening fluid with a fabric to obtain the flexible protective material.
[0016] Compared with the prior art, the present invention has at least the following beneficial effects:
[0017] 1) The preparation method of the flexible protective material provided by the present invention is simple to form once, the shear thickening fluid has high bonding strength with the fabric, has faster response speed and impact resistance, and has a wider temperature application range; the preparation method of the present invention is easier to maintain, simple to package, more uniform STF distribution, and more uniform performance of the overall composite material;
[0018] 2) The preparation method of the present invention allows the impregnation of non-Newtonian fluids between fabric fibers or the formation of a coating structure on the fabric surface, thereby increasing the dissipation capacity of impact energy and the individual resistance of fabric fibers, and reducing the content of fabric fibers required for impact protection; compared with conventional STF protective equipment, the new generation of STF high-performance composite fabrics has significant advantages in response speed, strength of agglomeration structure and stability; at the same time, because its instantaneously formed aggregate structure has different fractal dimensions, covers nanometer to millimeter scales, and has extremely high strength, it has obvious advantages over conventional protective equipment in resisting ultra-high-speed irregular particles;
[0019] 3) The product prepared by the present invention is composed of STF and fabric fibers. The fabric is impregnated or coated with nanoparticles dispersed in a shear thickening fluid to form a coating on the surface. The method can be used to manufacture bulletproof fabrics and products used as bulletproof fabrics. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1a Structural diagram of flexible protective material prepared by coating method;
[0022] Figure 1b Structure diagram of flexible protective material prepared by dipping method;
[0023] Figure 2 is the H NMR image characterizing the dispersing solvent component B in Example 3 of the present invention;
[0024] Figure 3 is the H NMR image characterizing the dispersing solvent component B in Example 4 of the present invention;
[0025] Figure 4 is the H NMR image characterizing the dispersing solvent component B in Example 5 of the present invention;
[0026] Figure 5 is the H NMR image characterizing the dispersing solvent component B in Example 6 of the present invention;
[0027] Figure 6 is the H NMR image characterizing the dispersing solvent component B in Example 7 of the present invention;
[0028] Figure 7 is the H NMR image characterizing the dispersing solvent component B in Example 8 of the present invention;
[0029] Figure 8 is the H NMR image characterizing the dispersing solvent component B in Example 9 of the present invention;
[0030] Fig. 9 is the H NMR image characterizing the dispersing solvent component B in Example 10 of the present invention;
[0031] Fig.10 The response speed and viscosity peak curves of the STF samples prepared in Example 3, Comparative Examples 1-2, and 5-6 of the present invention;
[0032] Fig.11a This is a picture of the impact of tin foil without STF coating;
[0033] Fig.11b This is a diagram showing the impact of the tin foil coated with the traditional STF material in Comparative Example 2;
[0034] Fig.11c This is a diagram showing the state of the tin foil coated with the STF material in Example 3 of the present invention after being impacted;
[0035] Fig.12a This is a diagram showing the impact of a flexible material prepared using the shear thickening fluid prepared in Example 3 of the present invention;
[0036] Figure 12b This is a diagram of the flexible material prepared using the shear thickening fluid prepared in Comparative Example 1 after impact;
[0037] Fig.12c This is a diagram of the flexible material prepared using the shear thickening fluid prepared in Comparative Example 5 after impact;
[0038] Fig.13 Schematic diagram of flexibility testing method and device. DETAILED DESCRIPTION
[0039] In view of the shortcomings of the prior art, the inventor of this case proposed the technical concept of the present invention after long-term research, which mainly provides a flexible protective material with faster response speed and impact resistance and wider temperature application range. The technical solution, its implementation process and principle will be further explained as follows.
[0040] As one aspect of the technical solution of the present invention, a flexible protective material is involved, including a combined shear-thickening fluid and a fabric; wherein the shear-thickening fluid forms a wet coating on the surface of the fabric, which specifically includes nanoparticles and a dispersed solvent, wherein the dispersed solvent includes at least an acrylic block low molecular weight copolymer.
[0041] As a preferred embodiment of the preparation method of the present invention, the fabric may include any one or more combinations of aromatic polyamide fibers, graphite fibers, glass fibers, poly(p-phenylene terephthalamide) fibers, ultra-high molecular weight polyethylene fibers, aramid fibers, polyimide fibers, polyphenylene sulfide fibers, carbon fibers, basalt fibers, etc., but is not limited thereto.
[0042] Furthermore, the weight average molecular weight of the ultra-high molecular weight polyethylene fiber is 1 to 5 million g / mol.
[0043] In some preferred embodiments, the content of the shear thickening fluid in the flexible protective material is 0.5-50 wt %.
[0044] In some preferred embodiments, the thickness of the shear thickening fluid coating is 1-100 μm.
[0045] The present invention is a method for impregnating nanoparticles dispersed in a shear thickening fluid (STF) in a fiber fabric, which allows the impregnation of a non-Newtonian fluid between the fabric fibers or forms a coating structure on the fabric surface, increases the dissipation capacity of the impact energy and the individual resistance of the fabric fibers, and reduces the content of the fabric fibers required for impact protection. The composite structure can be seen in Figure 1a , Figure 1b Compared with conventional STF protective equipment, the new generation of STF high-performance composite fabrics has significant advantages in response speed, strength and stability of nanoparticle agglomeration structure; at the same time, because the instantaneous aggregation structure formed by nanoparticles has different fractal dimensions, covers nanometer to millimeter scales, and has extremely high strength, it has obvious advantages over conventional protective equipment in resisting ultra-high-speed irregular particles.
[0046] As a preferred embodiment of the present invention, the dispersing solvent includes a combination of a first component (hereinafter also referred to as "component A") and a second component (hereinafter also referred to as "component B"), wherein the first component includes any one or a combination of two of silica gel, hydroxy silicone oil, ethylene glycol, propylene glycol, butylene glycol, polyethylene glycol and polypropylene glycol, and the second component includes an acrylic block low molecular weight copolymer.
[0047] In some preferred embodiments, the mass ratio of the first component to the second component is 95:5 to 0:100.
[0048] In some preferred embodiments, the weight average molecular weight of the acrylic acid block low molecular weight copolymer is lower than 2000 g / mol.
[0049] In some preferred embodiments, the mass ratio of the nanoparticles to the dispersion solvent is 10:90 to 90:10.
[0050] In some preferred embodiments, the diameter of the nanoparticles is 10 to 1000 nm.
[0051] In some preferred embodiments, the nanoparticles include at least any one of inorganic nanoparticles and organic nanoparticles.
[0052] As a preferred embodiment of the present invention, the inorganic nanoparticles include any one or a combination of two or more of nano-silicon dioxide particles, titanium dioxide particles, calcium carbonate particles, calcium acetate particles, aluminum oxide particles, quartz powder, zinc oxide particles, iron oxide particles, silver particles, ferroferric oxide particles, ZrO2 particles, boric acid, carbon black, graphene, graphene oxide particles, etc., but are not limited thereto.
[0053] As a preferred embodiment of the present invention, the organic nanoparticles include any one or a combination of two or more of polymethyl methacrylate particles, polystyrene particles, polyvinyl chloride particles, starch particles, etc., but are not limited thereto.
[0054] As a preferred embodiment of the present invention, the nanoparticles are surface functionalized nanoparticles.
[0055] Furthermore, the nanoparticles are partially hollow nanoparticles, and hollowing can achieve lightweight and intelligence.
[0056] Specifically, the aforementioned surface functionalization refers to nanoparticles with special structural functions such as different geometric shapes and hollow structures, which form nanofilling materials with metastable structures of diamond-like crystals. The main feature is that the nanoparticles in the shear-thickening fluid are no longer simply physically stacked under the action of the external field, but through the fluid design and the local high stress brought by the high-speed projectile, the repulsive force is overcome and the potential energy barrier between the particles is broken through, forming a more stable nano-scale to micron-scale solid structure, thereby greatly improving the local impact resistance of the nanomaterial.
[0057] Furthermore, the aforementioned surface functionalization can be functional nanoparticles of different geometric shapes such as rods / needles, sheets, spindles, polyhedrons, etc.
[0058] Furthermore, the special agglomerate structure formed by the nanoparticles is similar to the foam-like structural characteristics of a honeycomb, so its theoretical specific strength is much higher than that of the conventional spherical nanoparticle stacking structure, achieving the advantage of lightweight while achieving the high functionality of the STF protective material.
[0059] In some more preferred embodiments, the acrylic block low molecular weight copolymer comprises at least a first segment having a controlled molecular weight and position and a second segment having a controlled molecular weight and position; wherein the first segment comprises a segment formed by polymerization of at least any one of the monomers having a structure as shown in formula (I):
[0060]
[0061] Wherein, R includes H or CH3, and X includes a cross-linkable functional group, preferably including any one or a combination of two or more of the cross-linkable silyl, hydroxyl, carboxyl, carbonyl, carbonate, isocyanate, epoxy, vinyl, amino, mercapto, acetoacetyl, alkoxymethylol and cyclic ether groups, but is not limited thereto.
[0062] Furthermore, the second segment includes a segment formed by polymerization of at least one of the monomers having a structure as shown in formula (II):
[0063]
[0064] Wherein, R1 includes H or CH3, and R2 includes a branched or unbranched saturated alkyl group having 4 to 14 carbon atoms.
[0065] As a preferred embodiment of the present invention, the second segment of the acrylic block low molecular weight copolymer includes a segment formed by polymerization of any one or a combination of two or more of a plurality of acrylic ester monomers, wherein the acrylic ester monomer includes any one or a mixture of two of acrylic esters and methacrylic esters.
[0066] In some more preferred embodiments, the acrylate includes any one or a combination of two or more of acrylates having a C1-C20 alkyl group, aromatic acrylates, cyclic acrylates, and the like.
[0067] Furthermore, the acrylic acid ester monomer preferably includes any one or a combination of two or more of methyl acrylate, ethyl acrylate, phenyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, n-nonyl acrylate, isobornyl acrylate, 2-propylheptyl acrylate, isodecyl acrylate, isostearyl acrylate, etc., but is not limited thereto.
[0068] In some more preferred embodiments, the methacrylate includes any one or a combination of two or more of methacrylate having a C1-C20 alkyl group, aromatic methacrylate, cyclic methacrylate, etc.
[0069] Furthermore, the methacrylate preferably includes any one or a combination of two or more of methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, phenyl methacrylate, acetoacetoxyethyl methacrylate, isobornyl methacrylate, isooctyl methacrylate, etc., but is not limited thereto.
[0070] The shear thickening fluid provided by the invention has a faster response speed and higher impact resistance.
[0071] As a preferred embodiment of the present invention, the method for preparing the shear thickening fluid comprises: uniformly dispersing nanoparticles in a dispersing solvent to obtain a stably dispersed shear thickening fluid.
[0072] In some preferred embodiments, the method for preparing the shear thickening fluid specifically comprises the following steps:
[0073] The component B and the component A are fully mixed to obtain a dispersion solvent, and the nanoparticles are then dispersed in the dispersion solvent. The nanoparticles are dispersed evenly to obtain a stably dispersed shear-thickening fluid.
[0074] The shear-thickening fluid prepared by the preparation method of the present invention has the advantages of high impact resistance, fast response rate, high degree of intelligence, and more uniform performance of the overall composite material. The "liquid-solid" response speed and viscosity peak are both improved by more than an order of magnitude.
[0075] As another aspect of the technical solution of the present invention, it also relates to a method for preparing the flexible protective material, comprising: combining a shear thickening fluid with a fabric to obtain the flexible protective material.
[0076] Furthermore, the bonding method includes at least any one of coating, dipping, etc.
[0077] In summary, the preparation method of the flexible protective material provided by the present invention has a high bonding strength between STF and fabric through simple one-time molding, and has a faster response speed and impact resistance; it has a wider temperature application range; the method of the present invention is easier to maintain, simple to package, more uniform STF distribution, and more uniform performance of the overall composite material.
[0078] As another aspect of the technical solution of the present invention, the flexible protective material prepared by the present invention is composed of STF and fabric fibers, and the fabric is formed by impregnating or coating the surface of nanoparticles dispersed in a shear thickening fluid to form a coating. This method can be used to manufacture bulletproof fabrics and products as bulletproof fabrics.
[0079] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification and the drawings.
[0080] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0081] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0082] The inorganic nanoparticles in the present invention include nano silicon dioxide particles, titanium dioxide particles, calcium carbonate particles, calcium acetate particles, aluminum oxide particles, quartz powder, zinc oxide particles, iron oxide particles, silver particles, ferroferric oxide particles, ZrO2 particles, boric acid, carbon black, graphene particles, and graphene oxide particles, all of which are common commercially available products.
[0083] The organic nanoparticles in the present invention include polymethyl methacrylate particles, polystyrene particles, polyvinyl chloride particles, and starch particles, all of which are common commercial products.
[0084] Example 1
[0085] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0086] (1) Preparation of polymethyl methacrylate nanosphere particles:
[0087] The nanomaterials are polymethyl methacrylate particles with a particle size of 100 to 120 nm;
[0088] The preparation method adopts soap-free emulsion polymerization: nitrogen protection is passed through a three-necked flask, a condenser is added, the reaction temperature is controlled at 80°C, 100mL H2O\5mL MMA monomer is added, the stirring speed is 800r / min, and after constant temperature for half an hour, 25mL of K2S208 (5mmol / L) aqueous solution is added, and the reaction is cooled to room temperature after 6 hours.
[0089] The emulsion is centrifuged, washed with ethanol for 2-3 times, and then vacuum dried to obtain polymethyl methacrylate nanosphere particles.
[0090] (2) Preparation of dispersion solvent:
[0091] The dispersion solvent consists of two components, A and B, where:
[0092] A is hydroxy silicone oil, with a mass content of 30wt%;
[0093] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 70 wt%;
[0094] The preparation method of component B is as follows:
[0095] Triethoxyvinylsilane (8.2wt%), methyl methacrylate (13.5wt%), ethyl acrylate (25.3wt%), ethyl acetate (50.6wt%), initiator: 4,4-azobis(4-cyanovaleric acid) (ACPA) (0.9wt%), azobisisobutyronitrile (1.5wt%), MAA monomer 20g, other raw materials are added in proportion;
[0096] All raw materials were added to a three-necked flask, stirred evenly, and nitrogen was introduced for 50 minutes to deoxygenate. The reaction was carried out at 65°C for 30 minutes. After the reaction was completed, the solvent (ethyl acetate) was stripped from the polymer solution by rotary evaporation at 65°C. The weight average molecular weight of the separated polymer was measured to be 1700 g / mol.
[0097] Component A and component B are mixed and stirred evenly. Component A is 30 g of hydroxy silicone oil and component B is 70 g. Stir evenly to obtain a dispersion solvent.
[0098] (3) Preparation of shear-thickening fluid:
[0099] Take 1g of polymethyl methacrylate nanosphere particles and add them to 9g of the above-mentioned dispersing solvent. Use strong dispersion (stirring speed is 5500r / min, time is 30min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 30min) to further disperse them evenly and remove bubbles to obtain a shear thickening fluid.
[0100] (4) Preparation of flexible protective materials:
[0101] A shear-thickening fluid is applied to the surface of a fabric material by spraying to obtain a fabric flexible protective material with a wet coating surface; wherein the fabric material is specifically an ultra-high molecular weight polyethylene (weight-average molecular weight of 2 million g / mol) fiber woven cloth with a fiber diameter of 1 to 17 μm, and the spraying process uses a manual spray gun with a spraying distance of 10 cm, and manual back and forth spraying, and the final sprayed coating thickness is controlled to be 10 μrm.
[0102] Example 2
[0103] The steps for preparing the shear thickening fluid in this example are the same as those in Example 1.
[0104] The difference from Example 1 is that: after the fabric is impregnated into the STF material by an impregnation method, a flexible protective material containing STF material is obtained, wherein the fabric material is specifically an aramid fiber woven cloth with a diameter of 1 to 10 μm, and the impregnation process parameters are to completely impregnate the fabric material into the STF material and take it out for 20 minutes.
[0105] Example 3
[0106] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0107] (1) 2 g of polyvinyl pyrrolidone, 0.5 g of azobisisobutylamidine hydrochloride, and 100 ml of distilled water were stirred at room temperature. After the solution was clarified, 11 ml of methyl methacrylate monomer was added and N2 was introduced for 1 h. Then, the mixture was stirred at 65°C at a stirring speed of 200 rpm for 18 h to obtain a polymethyl methacrylate emulsion (PMMA) with an average particle size of about 200 nm.
[0108] 10.0 g of the polymethyl methacrylate emulsion obtained above was taken and dissolved in 80 ml of anhydrous ethanol. Ultrasonic treatment was performed for 1 h. After sufficient dissolution, a suspension was obtained. 10 ml of ammonia water was added at 50° C. while stirring. After 10 min, 3 ml of an organic-inorganic silicon source was added. The silicon source was tetraethyl orthosilicate and methyltriethoxysilane in a volume ratio of 1:4. The reaction was performed for 3 h to obtain silicon dioxide-coated polymethyl methacrylate nanoparticles with an average particle size of 200 nm.
[0109] The silica-coated polymethyl methacrylate nanoparticles obtained above were washed with water and ethanol, centrifuged, dispersed in anhydrous ethanol, poured into a container and spread into a liquid film. After drying, they were soaked in 30 ml of toluene solution for 24 hours, and then the organic solvent was slowly removed. After natural drying, hollow nano-silica was obtained.
[0110] (2) Preparation of dispersion solvent:
[0111] The dispersion solvent consists of two components, A and B, where:
[0112] Component A is propylene glycol, with a mass content of 50wt%;
[0113] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 50 wt%;
[0114] The preparation method of component B is as follows:
[0115] Methacrylic acid (MAA) (4.3wt%), butyl acrylate (BA) (45.3wt%), ethyl acetate (48.0wt%), dibenzyl trithiocarbonate (DBTTC) (1.5wt%), initiator: 4,4-azobis(4-cyanovaleric acid) (ACPA) (0.9wt%), MAA monomer 20g, and other raw materials are added in proportion. All raw materials are added to a three-necked flask, stirred evenly, and nitrogen is introduced for 30min to deoxygenate. The reaction is carried out at 60°C. After the reaction is completed, the solvent (ethyl acetate) is stripped from the polymer solution at 60°C by rotary evaporation. The weight average molecular weight of the separated polymer is measured to be 1500g / mol. The H nuclear magnetic resonance data of the dispersed solvent component B are: δ0.81-0.95 (16H, 0.88 (dd, J=7.11, 7.11Hz), 0.89 (d, J=6.62Hz)), 1 .29-1.62 (10H, 1.39 (ddq, J=7.11, 7.11, 7.11Hz), 1.39 (ddq, J=7.11, 7.11, 7.11Hz), 1.55 (ddd, J=7.50, 7.40, 7.40Hz), 1.55 (dddd, J=7.50, 7.40, 7.40Hz)), 1.64-1.91 (8H, 1.73 (dddd, J=7.12, 7.12, 7.11, 7.11 Hz), 1.73 (dddd, J=7.12, 7.12, 7.11, 7.11Hz), 1.80 (ddddq, J=7.50, 7.50, 7.40, 7.40, 6.62Hz)), 2.18-2 .32(11H, 2.24(d, J=7.40Hz), 2.24(d, J=7.40Hz), 2.25(dd, J=7.40, 7.40Hz), 2.25(dd, J=7.40, 7.40Hz) ), 4.10-4.23 (5H, 4.17 (dd, J = 7.12, 7.12 Hz), 4.17 (dd, J = 7.12, 7.12 Hz)), 0.89 (16H, m), 1.39 (5H, q, J = 7.10 Hz), 1.55 (5H, q, J = 7.43 Hz), 1.73 (8H, m), 2.24 (11H, m), 4.17 (5H, t, J = 7.11 Hz), the H NMR spectrum showed that the polymer component was successfully prepared, see Figure 2 .
[0116] Component A and component B are mixed and stirred evenly. Component A is 50 g of propylene glycol and component B is 50 g. Stir evenly to obtain a dispersion solvent.
[0117] (3) Preparation of shear-thickening fluid:
[0118] Take 0.5g of hollow nano-silica, add it to 9.5g of the above-mentioned dispersing solvent, and use strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to disperse it evenly to obtain a shear thickening fluid.
[0119] (4) Preparation of flexible protective materials:
[0120] A shear-thickening fluid is applied to the surface of a fabric material by spraying to obtain a fabric flexible protective material with a wet coating surface; wherein the fabric material is specifically a polyimide fiber woven cloth with a fiber diameter of 10 μm, and the spraying process uses a manual spray gun with a spraying distance of 10 cm, and manual back and forth spraying, and the final coating thickness obtained by spraying is controlled to be 10 μm.
[0121] Example 4
[0122] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0123] (1) Preparation method of rod-shaped nano-silica: 15.00 g of polyvinyl pyrrolidone (number average molecular weight 4000) and 150 ml of n-pentanol were ultrasonically dissolved and mixed well. 15 ml of ethanol, 4.2 ml of water, and 1.5 ml of 0.18 mol / L sodium citrate solution were added and manually shaken. 3 ml of ammonia water (mass percent concentration of 26%) was added and manually shaken. Then 1.5 ml of tetraethyl orthosilicate (TEOS) was added and manually shaken. After being manually shaken, the mixture was placed in a water bath at 40° C. and allowed to stand for 30 min. The mixture was taken out and centrifuged and washed to obtain rod-shaped nano-silica;
[0124] (2) Preparation of dispersion solvent:
[0125] The dispersion solvent consists of two components, A and B, where:
[0126] Component A is silica gel, with a mass content of 95wt%;
[0127] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 5 wt%;
[0128] The preparation method of component B is as follows:
[0129] Allyl isocyanate (20.0wt%), phenyl acrylate (29.6wt%), ethyl acetate (48.0wt%), dibenzyl trithiocarbonate (1.5wt%), initiator: azobisisobutyronitrile (AIBN) (0.9wt%), phenyl acrylate monomer 20g, and other raw materials are added in proportion. All raw materials are added to a three-necked flask, stirred evenly, and nitrogen is introduced for 30 minutes to deoxygenate. The reaction is carried out at 60°C. After the reaction is completed, the solvent (ethyl acetate) is stripped from the polymer solution at 60°C by rotary evaporation. The weight average molecular weight of the separated polymer is measured to be 1600g / mol. The H NMR spectrum shows that the polymer component is successfully prepared. Figure 3 .
[0130] Component A and component B are mixed and stirred evenly, component A is 95g, component B is 5g, and stirred evenly to obtain a dispersion solvent.
[0131] (3) Preparation of shear-thickening fluid:
[0132] Take 1.0 g of rod-shaped nano-silica, add it to 9.0 g of the above-mentioned dispersing solvent, and use strong dispersion (stirring speed is 5000 r / min, time is 15 min) and ultrasonic dispersion (ultrasonic power is 40 KHz, time is 20 min) to disperse it evenly to obtain a shear thickening fluid.
[0133] (4) Preparation of flexible protective materials:
[0134] A shear-thickening fluid is applied to the surface of a fabric material by spraying to obtain a fabric flexible protective material with a wet coating surface; wherein the fabric material is specifically a polyphenylene sulfide fiber woven cloth with a fiber diameter of 10 μm, and the spraying process uses a manual spray gun with a spraying distance of 10 cm, and manual back and forth spraying, and the final sprayed coating thickness is controlled to be 10 μm.
[0135] Example 5
[0136] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0137] (1) Preparation method of hollow rod-shaped ferrosoferric oxide: 15.00 g of polyvinyl pyrrolidone (number average molecular weight 4000) and 150 ml of n-pentanol were dissolved by ultrasonication. After mixing evenly, 15 ml of ethanol, 4.2 ml of water, and 1.5 ml of 0.18 mol / L sodium citrate solution were added and manually shaken. Then, 3 ml of ammonia water (mass percentage concentration of 26%) was added and manually shaken. Then, 1.5 ml of tetraethyl orthosilicate (TEOS) was added and manually shaken. After being manually shaken, the mixture was placed in a water bath at 40° C. and allowed to stand for 30 min. The mixture was taken out and centrifuged and washed to obtain rod-shaped silica.
[0138] Dissolve 0.318g of trisodium citrate dihydrate in 20ml of ethylene glycol, then add 1.5g of anhydrous sodium acetate and 0.75g of deionized water, which is referred to as solution A; dissolve 0.819g of ferric chloride in 10ml of ethylene glycol, and continue to add 0.5ml of 15wt% rod-shaped silica aqueous solution, which is referred to as solution B; mix solution A and solution B, stir to fully mix to obtain a brown-black clear solution and place it in a high-temperature and high-pressure reactor with a volume of 50ml, set the temperature to 200℃, and react at this temperature for 10h. After the reaction is completed, separate and wash the obtained mixed solution to obtain rod-shaped silica coated with ferroferric oxide;
[0139] The rod-shaped silicon dioxide coated with ferroferric oxide was dissolved in a 5 mol / L sodium hydroxide aqueous solution and reacted with magnetic stirring for 10 h in a 55°C water bath. After the reaction was completed, the product was centrifuged and washed several times with deionized water and anhydrous ethanol to obtain the final product.
[0140] (2) Preparation of dispersion solvent:
[0141] The dispersion solvent consists of two components, A and B, where:
[0142] Component A is hydroxy silicone oil, with a mass content of 70wt%;
[0143] Component B is an acrylic acid block low molecular weight copolymer with a weight average molecular weight of less than 2000 g / mol and a mass content of 30 wt%;
[0144] The preparation method of component B is as follows:
[0145] Ethoxycarbonyl propylene (10.2wt%), 2-ethylhexyl acrylate (39.4wt%), ethyl acetate (48wt%), dibenzyl trithiocarbonate (1.5wt%), initiator: azobisisobutyronitrile (0.9wt%), ethoxycarbonyl propylene monomer 20g, and other raw materials are added in proportion. All raw materials are added to a three-necked flask, stirred evenly, and nitrogen is introduced for 30 minutes to deoxygenate. The reaction is carried out at 60°C. After the reaction is completed, the solvent (ethyl acetate) is stripped from the polymer solution by rotary evaporation at 60°C. The weight average molecular weight of the separated polymer is measured to be 1800g / mol. The H NMR spectrum shows that the polymer component is successfully prepared. Figure 4 .
[0146] Component A and component B are mixed and stirred evenly, component A is 70g, component B is 30g, and stirred evenly to obtain a dispersion solvent.
[0147] (3) Preparation of shear-thickening fluid:
[0148] Take 2.0g of rod-shaped silicon dioxide coated with ferrosoferric oxide, add it to 8.0g of the above-mentioned dispersing solvent, and use strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to disperse it evenly to obtain a shear thickening fluid.
[0149] (4) Preparation of flexible protective materials:
[0150] The fabric is impregnated into the STF material to obtain a flexible protective material containing the STF material, wherein the fabric material is specifically a glass fiber woven cloth with a diameter of 8 μm, and the impregnation process parameters are to completely impregnate the fabric material into the STF material and take it out after 20 minutes.
[0151] Example 6
[0152] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0153] (1) Preparation of graphene oxide: 30 mg of graphene oxide was weighed and dispersed in 300 ml of an alcohol solution of 1% by volume of 3-mercaptopropylethoxysilane, and stirred continuously at room temperature for 24 h. Then, the thiol-modified graphene oxide material was washed and separated.
[0154] (2) Preparation of dispersion solvent:
[0155] The dispersion solvent consists of two components, A and B, where:
[0156] Component A is ethylene glycol, with a mass content of 20wt%;
[0157] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 80 wt%;
[0158] The preparation method of component B is as follows:
[0159] Propylene oxide (15.8 wt%), n-hexyl acrylate (33.7 wt%), ethyl acetate (48 wt%), dibenzyl trithiocarbonate (1.5 wt%), initiator: benzoyl peroxide (BPO) (1.0 wt%), 20 g of propylene oxide monomer, and other raw materials added in proportion. All raw materials were added to a three-necked flask, stirred evenly, and nitrogen was introduced for 30 min to deoxygenate. The reaction was carried out at 70°C. After the reaction was completed, the solvent (ethyl acetate) was stripped from the polymer solution by rotary evaporation at 70°C. The weight average molecular weight of the separated polymer was measured to be 1600 g / mol. The H NMR spectrum showed that the polymer component was successfully prepared. Figure 5 .
[0160] Component A and component B are mixed and stirred evenly. Component A is 20 g and component B is 80 g. Stir evenly to obtain a dispersion solvent.
[0161] (3) Preparation of shear-thickening fluid:
[0162] Take 5.0 g of thiol-modified graphene oxide material, add it to 5.0 g of the above-mentioned dispersing solvent, and use strong dispersion (stirring speed is 5000 r / min, time is 15 min) and ultrasonic dispersion (ultrasonic power is 40 KHz, time is 20 min) to disperse it evenly to obtain a shear thickening fluid.
[0163] (4) Preparation of flexible protective materials:
[0164] The fabric is impregnated into the STF material to obtain a flexible protective material containing the STF material, wherein the fabric material is specifically a carbon fiber woven cloth with a diameter of 6 μm, and the impregnation process parameters are to completely impregnate the fabric material into the STF material and take it out after 30 minutes.
[0165] Example 7
[0166] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0167] (1) Preparation of polymethyl methacrylate particles:
[0168] Weigh 200g of methyl methacrylate monomer, add 500ml of deionized water, pour into a 2L four-necked flask, stir evenly at 800r / min on an electric stirrer, and slowly add 5g of azobisisobutyronitrile initiator into the four-necked flask. Place the four-necked flask in an oil bath set at 80°C, and continue stirring to react for 3h. Pour the reaction product into a large amount of ethanol (about 500ml) for precipitation, then use a vacuum filtration device to filter and collect the precipitate. Wash the precipitate several times with ethanol to remove unreacted monomers and impurities, and dry the washed product in a vacuum drying oven at 60°C for 8h to obtain polymethyl methacrylate particles.
[0169] (2) Preparation of dispersion solvent:
[0170] The dispersing solvent is composed of component B, wherein component B is an acrylic acid block low molecular weight copolymer, and the weight average molecular weight is less than 2000 g / mol;
[0171] The preparation method of component B is as follows:
[0172] Allylamine (30.2wt%), isooctyl methacrylate (19.1wt%), ethyl acetate (48wt%), dibenzyl trithiocarbonate (1.5wt%), initiator: benzoyl peroxide (1.2wt%), 20g of allylamine monomer, and other raw materials added in proportion. All raw materials were added to a three-necked flask, stirred evenly, and nitrogen was introduced for 30 minutes to deoxygenate. The reaction was carried out at 70°C. After the reaction was completed, the solvent (ethyl acetate) was stripped from the polymer solution by rotary evaporation at 70°C. The weight average molecular weight of the separated polymer was measured to be 1500g / mol. The nuclear magnetic resonance spectrum showed that the polymer component was successfully prepared. Figure 6 .
[0173] (3) Preparation of shear-thickening fluid:
[0174] Take 8.0g of polymethyl methacrylate particles, add them into 2.0g of the above-mentioned dispersing solvent, and disperse them evenly by strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to obtain a shear thickening fluid.
[0175] (4) Preparation of flexible protective materials:
[0176] The fabric is impregnated into the STF material to obtain a flexible protective material containing the STF material, wherein the fabric material is specifically an aromatic polyamide fiber woven cloth with a diameter of 5 μm, and the impregnation process parameters are to completely impregnate the fabric material into the STF material for 30 minutes and then take it out.
[0177] Example 8
[0178] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0179] (1) Preparation of polystyrene particles:
[0180] Add 500ml of deionized water to a four-necked flask, then add 10g of sodium dodecyl sulfate, stir it with an electric stirrer at a speed of 800r / min to fully dissolve it, then weigh 200g of styrene monomer, slowly add it dropwise to the above solution, and continue stirring for 30min to mix the system evenly. Place the four-necked flask in a constant temperature water bath, heat it to 70°C, and after the temperature stabilizes, add 5g of potassium persulfate initiator to the flask to start the polymerization reaction, and the reaction time is 4h. After the reaction is completed, the product is cooled to room temperature, and the product is filtered using a Buchner funnel and a suction flask to collect the solid product. Wash the collected product with a large amount of deionized water to remove unreacted monomers and impurities. Put the washed product into a drying oven and dry it at 60°C for 8h to obtain polystyrene particles.
[0181] (2) Preparation of dispersion solvent:
[0182] The dispersing solvent is composed of component B, wherein component B is an acrylic acid block low molecular weight copolymer, and the weight average molecular weight is less than 2000 g / mol;
[0183] The preparation method of component B is as follows:
[0184] Allyl mercaptan (13.6wt%), 2-propylheptyl acrylate (36wt%), toluene (48wt%), dibenzyl trithiocarbonate (1.5wt%), initiator: benzoyl peroxide (0.9wt%), propylene mercaptan monomer 20g, and other raw materials added in proportion; all raw materials are added into a three-necked flask, stirred continuously and evenly, nitrogen is introduced for 30min to deoxygenate, and the reaction is carried out at 60°C. After the reaction is completed, the solvent (toluene) is stripped from the polymer solution by rotary evaporation at 60°C, and the weight average molecular weight of the separated polymer is measured to be 1800g / mol. The H NMR spectrum shows that the polymer component is successfully prepared. Figure 7 .
[0185] (3) Preparation of shear-thickening fluid:
[0186] Take 9.0g of polystyrene particles, add them into 1.0g of the above-mentioned dispersing solvent, and disperse them evenly by strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to obtain a shear thickening fluid.
[0187] (4) Preparation of flexible protective materials:
[0188] The fabric is impregnated into the STF material to obtain a flexible protective material containing the STF material, wherein the fabric material is specifically a graphite fiber woven cloth with a diameter of 8 μm, and the impregnation process parameters are to completely impregnate the fabric material into the STF material for 20 minutes and then take it out.
[0189] Example 9
[0190] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0191] (1) Preparation of polyvinyl chloride particles:
[0192] Add 500ml of deionized water to a four-necked flask, then add 10g of polyvinyl alcohol, stir it with an electric stirrer at a speed of 800r / min to fully dissolve it, then weigh 200g of vinyl chloride monomer, slowly add it dropwise to the above solution, and continue stirring for 30min to mix the system evenly. Place the four-necked flask in a constant temperature water bath and heat it to 50°C. After the temperature stabilizes, add 5g of diisopropyl peroxydicarbonate initiator to the flask to start the polymerization reaction, and the reaction time is 5h. After the reaction is completed, use a Buchner funnel and a suction flask to filter the product, collect the solid product, and wash the collected product with a large amount of deionized water to remove unreacted monomers and impurities. Put the washed product into a drying oven and dry it at 50°C for 10h to obtain polyvinyl chloride particles.
[0193] (2) Preparation of dispersion solvent:
[0194] The dispersion solvent consists of two components, A and B, where:
[0195] Component A is polyethylene glycol, with a mass content of 10wt%;
[0196] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 90 wt%;
[0197] The preparation method of component B is as follows:
[0198] N-vinyl acetyl (12.5wt%), acetoacetoxyethyl methacrylate (37.3wt%), toluene (48wt%), dibenzyl trithiocarbonate (DBTTC) (1.2wt%), initiator: benzoyl peroxide (BPO) (1.0wt%), N-vinyl acetyl monomer 20g, and other raw materials are added in proportion. All raw materials are added to a three-necked flask, stirred evenly, and nitrogen is introduced for 30 minutes to deoxygenate. The reaction is carried out at 80°C. After the reaction is completed, the solvent (toluene) is stripped from the polymer solution by rotary evaporation at 80°C. The weight average molecular weight of the separated polymer is measured to be 1700g / mol. The H NMR spectrum shows that the polymer component is successfully prepared. Figure 8 .
[0199] Component A and component B are mixed and stirred evenly, component A is 10g, component B is 90g, and stirred evenly to obtain a dispersion solvent.
[0200] (3) Preparation of shear-thickening fluid:
[0201] Take 9.0g of polyvinyl chloride particles, add them into 1.0g of the above-mentioned dispersing solvent, and disperse them evenly by strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to obtain a shear thickening fluid.
[0202] (4) Preparation of flexible protective materials:
[0203] A shear-thickening fluid is applied to the surface of a fabric material by spraying to obtain a fabric flexible protective material with a wet coating surface; wherein the fabric material is specifically a basalt fiber woven cloth with a fiber diameter of 10 μm, and the spraying process uses a manual spray gun with a spraying distance of 10 cm, and manual back and forth spraying, and the final sprayed coating thickness is controlled to be 10 μm.
[0204] Example 10
[0205] This embodiment provides a method for preparing a flexible protective material, the main steps of which are:
[0206] (1) Starch granule preparation:
[0207] Weigh 20g starch, add 300ml deionized water, stir evenly at 500r / min on a magnetic stirrer to prepare a starch solution with a concentration of about 6.7%. Slowly add 5g sodium hydroxide solution dropwise to the above starch solution, and use a pH meter to monitor the pH value of the solution and adjust it to between 9-10. Transfer the solution with adjusted pH value to a 1L autoclave and seal it, set the temperature to 150°C, the pressure to 2MPa, and react for 2h. After the reaction is completed, let the reactor cool naturally to room temperature, open the lid of the reactor and take out the reaction product. Pour the product into about 300ml ethanol and wash it several times until the washing liquid is colorless to remove unreacted substances and impurities. Then put the washed product into a centrifuge, centrifuge it at 8000rpm for 15min, and collect the precipitate. Finally, put the precipitate into a dialysis bag, dialyze it in 1000ml deionized water for 12h, and replace the deionized water every 4h to remove residual small molecules to obtain pure nano starch particles.
[0208] (2) Preparation of dispersion solvent:
[0209] The dispersion solvent consists of two components, A and B, where:
[0210] Component A is polypropylene glycol, with a mass content of 40wt%;
[0211] Component B is an acrylic acid block low molecular weight copolymer, with a weight average molecular weight of less than 2000 g / mol and a mass content of 60 wt%;
[0212] The preparation method of component B is as follows:
[0213] 2-methoxypropylene (22.6wt%), isobornyl methacrylate (27.2wt%), toluene (48wt%), dibenzyl trithiocarbonate (DBTTC) (1.2wt%), initiator: benzoyl peroxide (BPO) (1.0wt%), 2-methoxypropylene monomer 20g, and other raw materials are added in proportion. All raw materials are added to a three-necked flask, stirred evenly, and nitrogen is introduced for 30 minutes to deoxygenate. The reaction is carried out at 80°C. After the reaction is completed, the solvent (toluene) is stripped from the polymer solution by rotary evaporation at 80°C. The weight average molecular weight of the separated polymer is measured to be 1800g / mol. The H NMR spectrum shows that the polymer component is successfully prepared. Fig. 9 .
[0214] Component A and component B are mixed and stirred evenly. Component A is 40 g and component B is 60 g. Stir evenly to obtain a dispersion solvent.
[0215] (3) Preparation of shear-thickening fluid:
[0216] Take 6.0g of starch granules, add them into 4.0g of the above-mentioned dispersing solvent, and disperse them evenly by strong dispersion (stirring speed is 5000r / min, time is 15min) and ultrasonic dispersion (ultrasonic power is 40KHz, time is 20min) to obtain a shear thickening fluid.
[0217] (4) Preparation of flexible protective materials:
[0218] A shear-thickening fluid is applied to the surface of a fabric material by spraying to obtain a fabric flexible protective material with a wet coating surface; wherein the fabric material is specifically a poly(p-phenylene terephthalamide) fiber woven cloth with a fiber diameter of 8 μm, and the spraying process uses a manual spray gun, the spraying distance is 10 cm, and the spraying is done manually back and forth, and the final coating thickness obtained by spraying is controlled to be 10 μm.
[0219] Comparative Example 1
[0220] The only difference between this comparative example and Example 1 is that the dispersion solvent in step (2) is completely replaced by polyethylene glycol (weight average molecular weight is 2000 g / mol), and the other conditions are the same as those in Example 1 to obtain a flexible protective material. The drop weight impact test results are shown in Tables 1 and Fig.10 , Figure 12b .
[0221] Comparative Example 2
[0222] (1) Traditional STF materials:
[0223] The solvent is polyethylene glycol (weight average molecular weight is 2000 g / mol), the nano material is nano silicon dioxide particles (particle size is 100 nm), the addition amount is 5 wt %, and the mixture is evenly mixed to obtain a traditional STF material (the specific preparation process is the same as that in Example 1).
[0224] (2) The steps for preparing the protective material are the same as those in Example 1.
[0225] For the test results of the response speed and viscosity peak of the STF material prepared in this comparative example, please refer to Fig.10 Curve 4 in .
[0226] When STF material is coated on the surface of tin foil (coating thickness 50 microns), the tin foil is subjected to an impact test (500g load, 10 joules kinetic energy impact, material appearance). For a comparison of the impact effects on tin foil, please refer to Figure 11a-Figure 11c .in, Fig.11a This is a picture of the impact of tin foil without STF material coating. Fig.11b This is a picture of the impact of tin foil coated with traditional STF material. Fig.11c This is a picture of the tin foil coated with the STF material in Example 3 after being impacted; it can be seen that the traditional STF material will still break after being impacted, while the STF material in the present invention can prevent the tin foil from being penetrated by the impacting object and maintain its morphology.
[0227] Comparative Example 3
[0228] The only difference between this comparative example and Example 1 is that the B component acrylic block low molecular weight copolymer is not added to the dispersion solvent. Other conditions are the same as those in Example 1 to prepare a flexible protective material.
[0229] Comparative Example 4
[0230] The only difference between this comparative example and Example 1 is that the dispersion solvent component B is replaced with polyethylene glycol (weight average molecular weight is 2000 g / mol), and the other conditions are the same as those in Example 1 to prepare a flexible protective material.
[0231] Comparative Example 5
[0232] The only difference between this comparative example and Example 1 is that the dispersing solvent in step (2) is completely replaced by ethylene glycol to obtain a shear-thickening fluid. The other conditions and steps are the same as those in Example 1.
[0233] The inventors of this case have studied the response speed and peak viscosity of the shear thickening fluid sample prepared in Example 3 (using TA's ARES rheometer, tested at room temperature 25°C, using the steady-state shear mode, and the shear rate set to 10 -1 ~10 31 / s, all data detection conditions are the same) for testing, please refer to the test results Fig.10 Curve 1 in .
[0234] For the test results of the response speed and viscosity peak of the shear thickening fluid sample prepared in Example 1, please refer to Fig.10 Curve 3 in .
[0235] For the test results of the response speed and viscosity peak of the shear thickening fluid sample prepared in Example 5, please refer to Fig.10 From curve 5 in the figure, we can see that the viscosity and response speed of the sample are lower, and there is no response at high shear speed.
[0236] The inventors of this case also applied the shear thickening fluid samples obtained in Example 3, Comparative Example 1 and Comparative Example 5 on the surface of 100mmx100mm aramid fabric by spraying, with a coating thickness of 10μm. The results after using 800N load pressure impact were referenced to Figure 12a-12c , Fig.12a For the protective material made using the shear thickening fluid in Example 3, Figure 12b For the protective material made by using the shear thickening fluid in Comparative Example 1, Fig.12c For the protective material made using the shear thickening fluid in Comparative Example 5, it can be seen that the shear thickening sample coated fabric prepared in Example 3 has better protective performance than the traditional shear thickening sample coated fabric prepared in Comparative Examples 1 and 5.
[0237] Comparative Example 6
[0238] The only difference between this comparative example and Example 1 is that the hollow nano-silicon dioxide is replaced by ordinary nano-silicon dioxide (with a particle size of 100 nm), and the other conditions are the same as those of Example 1 to obtain a protective material. The test results of the response speed and viscosity peak of the samples obtained in this comparative example can be found in Fig.10 From curve 2 in the figure, we can see that the viscosity and response speed of the sample are relatively low.
[0239] like Fig.13 As shown in the figure, the disk method is used to test the drape of the fabric and compare the flexibility of the fabric. This method is to place an area of A on the R The circular fabric is placed concentrically on a small disk of a certain size, with an area of A. r , measured projection area A of the draped fabric F , the calculation method of overhang coefficient F value is as follows:
[0240]
[0241] The drop weight impact test was carried out according to the standard (GB / T 9639.1-2008). A drop weight impact tester was used and the drop weight impact speed was set to 3m / s to obtain the maximum impact force.
[0242] The fabric was cut into 100 x 100 mm and subjected to a 500 g load, 10 J kinetic energy impact test to measure and calculate the depression ratio (displacement ratio).
[0243] Table 1 Performance test results of various embodiments and comparative examples
[0244]
[0245] As can be seen from Table 1, the flexible protective material prepared by the method of the present invention has better protective performance than the traditional dispersed solvent or the traditional flexible protective material preparation method while basically not losing flexibility. It can be seen that the dispersion solvent in Example 3 does not add A, which has little effect on the protective performance of the flexible protective material; the dispersion solvent in Comparative Example 3 does not add component B, and basically has no protective function. In Comparative Example 4, component B is replaced with polyethylene glycol, and the technical effect is equivalent to that of the traditional flexible protective material, highlighting that the components of the dispersed solvent system have a synergistic effect, and none of them can be missing.
[0246] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification. For example, in addition to the nanoparticles listed in Examples 1-10, they were replaced with titanium dioxide particles, calcium carbonate particles, calcium acetate particles, aluminum oxide particles, quartz powder, zinc oxide particles, iron oxide particles, silver particles, ZrO2 particles, boric acid, carbon black, etc., and experiments were also conducted, and relatively ideal results were obtained.
[0247] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A flexible protective material, characterized in that: include: A combined shear-thickening fluid coating and fabric; the shear-thickening fluid coating comprises nanoparticles and a dispersing solvent, wherein the dispersing solvent comprises at least an acrylic acid block low molecular weight copolymer.
2. The flexible protective material according to claim 1, characterized in that: The fabric comprises any one or more combinations of aramid fiber, graphite fiber, glass fiber, poly(p-phenylene terephthalamide) fiber, ultra-high molecular weight polyethylene fiber, aramid fiber, polyimide fiber, polyphenylene sulfide fiber, carbon fiber, and basalt fiber; preferably, the weight average molecular weight of the ultra-high molecular weight polyethylene fiber is 1 to 5 million g / mol; and / or, the thickness of the shear thickening fluid coating is 1 to 100 μm; And / or, the content of the shear thickening fluid in the flexible protective material is 0.5-50wt%.
3. The flexible protective material according to claim 1, characterized in that: The dispersing solvent comprises a combination of a first component and a second component, wherein the first component comprises any one or a combination of two of silica gel, hydroxy silicone oil, ethylene glycol, propylene glycol, butylene glycol, polyethylene glycol and polypropylene glycol, and the second component comprises an acrylic acid block low molecular weight copolymer; And / or, the weight average molecular weight of the acrylic acid block low molecular weight copolymer is lower than 2000 g / mol.
4. The flexible protective material according to claim 3, characterized in that: The mass ratio of the first component to the second component is 95:5 to 0:100; And / or, the mass ratio of the nanoparticles to the dispersion solvent is 10:90 to 90:10; and / or, the diameter of the nanoparticles is 10 to 1000 nm.
5. The flexible protective material according to claim 1, characterized in that: The nanoparticles include at least any one of inorganic nanoparticles and organic nanoparticles. The inorganic nanoparticles include any one of nano silicon dioxide particles, titanium dioxide particles, calcium carbonate particles, calcium acetate particles, aluminum oxide particles, quartz powder, zinc oxide particles, iron oxide particles, silver particles, ferroferric oxide particles, ZrO2 particles, boric acid, carbon black, graphene, and graphene oxide particles, or a combination of two or more thereof. The organic nanoparticles include any one of polymethyl methacrylate particles, polystyrene particles, polyvinyl chloride particles, and starch particles, or a combination of two or more thereof. And / or, the nanoparticles are surface functionalized nanoparticles; And / or, the nanoparticles are hollow nanoparticles.
6. The flexible protective material according to claim 1, characterized in that: The acrylic block low molecular weight copolymer comprises at least a first segment having a controlled molecular weight and position and a second segment having a controlled molecular weight and position; wherein the first segment comprises a segment formed by polymerization of at least any one of the monomers having a structure as shown in formula (I): Wherein, R includes H or CH3, and X includes any one or a combination of two or more of a cross-linkable silyl group, a hydroxyl group, a carboxyl group, a carbonyl group, a carbonate group, an isocyanate group, an epoxy group, a vinyl group, an amino group, a mercapto group, an acetoacetyl group, an alkoxymethylol group, and a cyclic ether group; The second segment includes a segment formed by polymerization of at least one of the monomers having a structure as shown in formula (II): Wherein, R1 includes H or CH3, and R2 includes a branched or unbranched saturated alkyl group having 4 to 14 carbon atoms.
7. The flexible protective material according to claim 6, characterized in that: The second segment of the acrylic acid block low molecular weight copolymer includes a segment formed by polymerization of any one or a combination of two or more of a plurality of acrylic acid ester monomers, wherein the acrylic acid ester monomer includes any one or a combination of two of acrylic acid ester and methacrylic acid ester; The acrylate includes any one or a combination of two or more of acrylates having a C1-C20 alkyl group, aryl acrylates, and cyclic acrylates; the methacrylate includes any one or a combination of two or more of methacrylates having a C1-C20 alkyl group, aryl methacrylates, and cyclic methacrylates.
8. The flexible protective material according to claim 7, characterized in that: The acrylic acid ester includes any one or a combination of two or more of methyl acrylate, ethyl acrylate, phenyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, n-hexyl acrylate, n-heptyl acrylate, n-octyl acrylate, n-nonyl acrylate, isobornyl acrylate, 2-propylheptyl acrylate, isodecyl acrylate, and isostearyl acrylate; And / or, the methacrylate includes any one or a combination of two or more of methyl methacrylate, ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, phenyl methacrylate, acetoacetoxyethyl methacrylate, isobornyl methacrylate, and isooctyl methacrylate; And / or, the method for preparing the shear thickening fluid comprises: uniformly dispersing the nanoparticles in a dispersing solvent to obtain a stably dispersed shear thickening fluid.
9. The method for preparing a flexible protective material according to any one of claims 1 to 8, characterized in that: include: Combining shear-thickening fluids with fabrics results in flexible protective materials.
10. The preparation method according to claim 9, characterized in that: The bonding method includes at least any one of coating and dipping.
Citation Information
Cited By
Bulletproof and stab-resistant composite material and preparation method thereof
CN119615620A
A bulletproof and stab-proof composite material and preparation method thereof
CN119615620B
Preparation method and application of flexible ballistic protection knitted fabric
CN119800700A