Cracking wet-process polyurethane impregnation slurry, cracked ceramic texture suede microfiber leather and preparation method thereof

By using a combination of cracked wet-process polyurethane impregnation slurry and specific resins, the problem of suede microfiber synthetic leather being unable to achieve a cracked style has been solved, and suede microfiber leather with a natural cracked ceramic texture has been prepared, improving the visual appeal and feel of the product.

CN118996869APending Publication Date: 2024-11-22ANAN CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411246639.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Regular suede microfiber synthetic leather cannot achieve a cracked surface effect because it lacks a coating layer.

Method used

Using a crackled wet-process polyurethane impregnation slurry, a microporous membrane is formed by combining ultra-high modulus resins and ultra-low modulus resins with different moduli and polyether contents. Then, easy-to-dye and difficult-to-dye polyurethane resin solutions are printed on the surface of the base fabric. Combined with a specific dyeing process, a raised and grooved visual effect is formed.

Benefits of technology

It achieves a natural and distinct crackled ceramic texture on the surface of suede microfiber synthetic leather, enhancing the product's visual appeal and tactile feel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses cracking wet-process polyurethane impregnation slurry, cracking ceramic grain suede microfiber leather and a preparation method of the cracking ceramic grain suede microfiber leather. The preparation method comprises the following steps: (1) preparing base cloth from blended sea-island fibers; (2) the base cloth is subjected to wet-process impregnation treatment, crack wet-process polyurethane impregnation slurry is adopted, the slurry is prepared from, by mass, 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and a solidification adjusting auxiliary agent, and the solidification adjusting auxiliary agent accounts for 1.8%-3.5% of the total mass of the resin; the modulus of the ultrahigh-modulus resin is 220-280 MPa, the content of polyether is 20-30%, the modulus of the ultralow-modulus resin is 10-35 MPa, and the content of polyether is 70-80%; (3) reducing, oiling and drying the base cloth to obtain a base with a cracking style on the surface; and (4) dyeing the base to obtain the suede superfine fiber synthetic leather with the cracking ceramic grain style. According to the invention, the problem that the conventional suede superfine fiber synthetic leather cannot be made into a cracking style due to no coating layer (grain layer) is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of synthetic leather, in particular to a crackle wet-process polyurethane impregnation slurry, a crackle ceramic-grain suede microfiber leather and a preparation method thereof. Background Art

[0002] Natural leather is animal skin processed by certain physical and chemical methods. It is composed of natural protein fibers tightly woven in three-dimensional space. Its surface has a special grain layer with natural grain and luster, and feels comfortable. Synthetic leather is a composite material that simulates the composition and structure of natural leather. It looks and feels like natural leather and can be used in place of natural leather in many scenarios.

[0003] Over the decades of development of the synthetic leather industry, the emergence of various new materials has also led to the continuous updating of synthetic leather products. The base fabric has evolved from woven fabrics to non-woven fabrics, and then to microfiber non-woven fabrics; the resin used has also evolved from polyvinyl chloride resin (PVC) to polyurethane resin (PU). As the latest generation of synthetic leather, microfiber polyurethane synthetic leather (hereinafter referred to as microfiber leather) has a three-dimensional composite structure of bundled microfibers that is very similar to the microstructure of natural leather. Since microfiber leather not only has the characteristics of genuine leather in terms of external appearance and internal structure, but is also easy to industrialize and mass-produce, microfiber leather has been widely used.

[0004] Microfiber leather is made of bundled microfibers and polyurethane resin through a special process. First, nylon microfibers with similar structure and performance to the bundled fibers in natural leather are used to make non-woven fabrics with a three-dimensional network structure, and then filled with polyurethane resin with excellent performance and an open microporous structure. After multiple processes such as impregnation, reduction extraction, oiling and drying, the base fabric substrate (also known as bass) is manufactured; the bass is then veneered, that is, the coating layer is bonded to the bass through the release paper transfer coating method to obtain a widely used microfiber leather. Suede microfiber polyurethane synthetic leather (hereinafter referred to as suede leather) is made directly from bass without a coating layer through post-processing, and therefore has good breathability, unique appearance, and is comfortable to wear, and is widely favored by consumers.

[0005] Today's society pursues more personalized style characteristics, and various styles are flourishing in the fashion field. The doomsday wasteland style is a unique style in the fashion field. Its design comes from the abandoned, desolate and dilapidated scenes of the doomsday world, creating a decadent, rebellious and eclectic fashion image. In order to show the sense of abandonment and dilapidation, clothing and accessories are often damaged, torn, worn and other elements to reflect the aesthetics of destruction. As a unique craft, the cracked style, with its careful destruction of the shape, the playful sense of harmony and refinement, and the feeling of being eroded by time and environment, sets off an atmosphere of dilapidation yet high-end.

[0006] Microfiber leather can add a specific medium during the veneer process to make the coating layer produce a cracking effect during the drying and curing process; or by adding functional additives and then using mechanical treatment methods, a microfiber leather product with a cracked surface can be obtained. However, since suede leather has no coating layer, it is difficult to produce a cracked surface effect through post-processing. The inventor of this case conducted in-depth research on this issue, which led to the creation of this case.

[0007] In view of this, this case conducted an in-depth study on the above-mentioned issues and proposed a cracked wet-process polyurethane impregnation slurry, cracked ceramic-patterned suede microfiber leather and its preparation method, from which this case arose. Summary of the invention

[0008] The purpose of the present invention is to provide a crackle wet-process polyurethane impregnation slurry, a crackle ceramic-grain suede microfiber leather and a preparation method thereof, so as to solve the problem that conventional suede microfiber synthetic leather cannot be made into a crackle style due to the lack of a coating layer (grain layer).

[0009] In order to achieve the above object, the solution of the present invention is:

[0010] A crackle wet-process polyurethane impregnation slurry is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and solidification regulating auxiliary agent, wherein the solidification regulating auxiliary agent accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35MPa and a polyether content of 70-80%.

[0011] The filler is one or more of calcium carbonate, talcum powder and barium sulfate.

[0012] A method for preparing a cracked ceramic pattern suede microfiber leather comprises the following steps:

[0013] (1) The base fabric is made of blended sea island fibers;

[0014] (2) The base fabric is subjected to wet impregnation treatment, and a crackle wet polyurethane impregnation slurry is used, which is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and solidification regulating aid, wherein the solidification regulating aid accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%;

[0015] (3) reducing the weight of the base fabric, applying oil and drying the base fabric to obtain a bass with a cracked surface;

[0016] (4) The bass is dyed to obtain a suede microfiber synthetic leather with a cracked ceramic pattern style.

[0017] In the step (4), a polyurethane resin solution is printed on the surface of the bass with a cracked style, and dried to solidify it; then the printed bass is dyed to obtain a suede ultrafine fiber synthetic leather with a cracked ceramic pattern style; the polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 150-250 parts of organic solvent, and 7-15 parts of anti-phenol yellow additive; the polyurethane resin of the polyurethane resin solution is a resin with a modulus of 50-75 MPa, and the dyeing performance of the resin of the polyurethane resin solution is better than the dyeing performance of the resin impregnated with the slurry in step (2).

[0018] In the step (4), the polyurethane resin solution is printed on the surface of the cracked bass, and the gap between the printing roller and the rubber roller is controlled to be 0.10-0.15 mm smaller than the original thickness of the bass.

[0019] In the step (4), dyeing is carried out by roller dyeing, the bass is immersed in a prepared dyeing liquid tank, the temperature is controlled at 35°C and kept warm for 120 minutes, and then the temperature is increased by one degree per minute. After the temperature reaches 97°C, it is kept warm for 30 minutes, then taken out and pressed.

[0020] In the step (1), PA slices and PE slices are mixed in a certain proportion, and the blended sea-island fibers are obtained by a spinning process; the blended sea-island fibers are obtained by a needle punching process to obtain a non-woven fabric, and then the base fabric is obtained by heat setting treatment.

[0021] In the step (1), the thickness of the obtained base fabric is controlled at 2.80-3.50 mm, and the density is controlled at 0.230-0.290 g / cm 3 .

[0022] In the step (2), the impregnated base fabric is treated with a DMF / water mixed solution to solidify the polyurethane slurry in the base fabric, and the base fabric after complete solidification is passed through a water washing tank to remove residual DMF. After the water washing is completed, the sugar content of the residual DMF in the base fabric is less than 0.5.

[0023] In the step (3), the washed base fabric is sent to an extraction tank for toluene reduction treatment to remove the PE with a marine structure in the base fabric fibers; the semi-finished product after the reduction is oiled and dried to obtain a bass with a cracked surface, and then the bass is softened by a continuous kneading machine.

[0024] A cracked ceramic pattern suede microfiber leather is prepared by adopting the preparation method of the cracked ceramic pattern suede microfiber leather described above.

[0025] After adopting the above scheme, the beneficial effects of the present invention compared with the prior art are:

[0026] 1. The suede leather of the present invention is prepared by using a cracked polyurethane impregnation slurry, which solves the problem that conventional suede ultrafine fiber synthetic leather cannot be made into a cracked style due to the lack of a coating layer (grain layer). The impregnation slurry uses two specific types of resins with different moduli and different polyether contents. Due to the different polyether content settings, the two resins can be in an incompatible state to form interface differences. Due to the different cohesive forces between molecules with different moduli, the internal stresses corresponding to the fine porous membranes formed during the solidification of polyurethane are also different, so the internal contraction force of the polyurethane resin in the local fiber mesh is also different. Therefore, the apparent morphology of the polyurethane resin + fiber mesh composite will also show the phenomenon of protrusions and gullies due to the uneven local contraction force, forming a cracked style texture effect.

[0027] 2. Furthermore, in the method for preparing the cracked ceramic pattern suede microfiber leather of the present invention, a polyurethane resin solution is printed on the surface of the cracked style bass before dyeing, and the resin is applied to the raised parts of the bass cracks; the polyurethane resin of the polyurethane resin solution is a resin with a modulus of 50-75MPa, and the dyeing performance of the resin of the polyurethane resin solution is better than the dyeing performance of the resin impregnated with the slurry in step (2). During dyeing, the raised parts of the bass surface are darker in color due to the easy-to-dye resin, while the cracks and gullies are lighter in color or colorless due to the difficult-to-dye resin, thereby obtaining a suede leather with a cracked ceramic pattern surface style with more distinct and natural patterns. DETAILED DESCRIPTION

[0028] The case is further described in detail below in conjunction with specific implementation methods.

[0029] This case involves a crack-forming wet-process polyurethane impregnation slurry, which is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and a solidification regulating aid, which accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35MPa and a polyether content of 70-80%.

[0030] In a preferred embodiment, the organic solvent is DMF.

[0031] In a preferred embodiment, the filler is one or more of calcium carbonate, talcum powder and barium sulfate.

[0032] The preparation method of the wet-process polyurethane impregnation slurry with crack pattern in this case is to first mix and stir the organic solvent, filler and additive in the said proportion, stir at 1400-1500r / min for 15-20min, then add the resin in the said proportion (including ultra-high modulus resin and ultra-low modulus resin), stir up and down at 1400-1500r / min for 40-50min to make it evenly stirred, so as to obtain the wet-process polyurethane impregnation slurry with crack pattern.

[0033] The crackle wet-process polyurethane impregnation slurry of the present invention is mainly used in the wet impregnation process of microfiber leather to form crackle patterns on synthetic leather. The preferred implementation application is to be used in the preparation of crackle suede microfiber leather, solving the problem that conventional suede microfiber synthetic leather cannot produce crackle style due to the lack of a finishing layer (grain layer).

[0034] The modulus of the ultra-high modulus resin is selected to be 220-280MPa and its polyether content is controlled at 20-30%, and the modulus of the ultra-low modulus resin is selected to be 10-35MPa and its polyether content is controlled at 70-80%; the two resins with different moduli and different polyether contents can be in an incompatible state to form interface differences due to different polyether content settings. Due to the different cohesive forces between molecules with different moduli, the internal stress corresponding to the fine porous membrane formed during the solidification of polyurethane is also different. Therefore, in the application, the local internal contraction force of the polyurethane resin in the attachment is also different, so the apparent morphology of the polyurethane resin + attachment complex will also show the phenomenon of protrusions and gullies due to uneven local contraction force, and finally present a cracked style. The attachment can have a variety of forms. In a preferred embodiment, the base fabric is made of blended sea island fiber, and the corresponding attachment is a PA fiber mesh.

[0035] A method for preparing a cracked ceramic pattern suede microfiber leather comprises the following steps:

[0036] (1) The base fabric is made of blended sea island fibers;

[0037] (2) The base fabric is subjected to wet impregnation treatment, and a crackle wet polyurethane impregnation slurry is used, which is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and solidification regulating aid, wherein the solidification regulating aid accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%;

[0038] (3) reducing the weight of the base fabric, applying oil and drying the base fabric to obtain a bass with a cracked surface;

[0039] (4) The bass is dyed to obtain a suede microfiber synthetic leather with a cracked ceramic pattern style.

[0040] In the preparation of the suede microfiber leather of the present invention, a unique crackle wet-process polyurethane impregnation slurry is used to perform wet impregnation treatment on the base fabric, wherein the modulus of the ultra-high modulus resin is selected to be 220-280MPa and the polyether content thereof is controlled at 20-30%, and the modulus of the ultra-low modulus resin is selected to be 10-35MPa and the polyether content thereof is controlled at 70-80%; two resins with different moduli and different polyether contents can be in an incompatible state to form interface differences due to different polyether content settings, and molecules with different moduli have different cohesive forces, and during the solidification process of the polyurethane, the internal stress corresponding to the formed microporous membrane is also different, so the local internal contraction force of the polyurethane resin in the PA fiber web is also different, so the apparent morphology of the polyurethane resin+PA fiber web composite will also show the phenomenon of protrusions and gullies due to the uneven local contraction force, and finally present a cracked style.

[0041] In the step (2), the crackle pattern wet-process polyurethane impregnation slurry is made of polyurethane resins that are not easy to dye, which is more conducive to matching with subsequent processes to produce crackle patterns with excellent quality.

[0042] In the step (2), the organic solvent is DMF, and the filler is one or more of calcium carbonate, talcum powder, and barium sulfate.

[0043] The wet impregnation treatment in step (2) is specifically performed by impregnating the base fabric obtained in step (1) into an impregnation tank filled with the impregnation slurry, and ensuring that the base fabric is completely impregnated with the slurry by a plurality of groups of rollers, wherein the gap is adjusted to be 15-20s less than the thickness of the base fabric; after the base fabric passes through the impregnation tank, the excess impregnation slurry on the front and back sides of the base fabric is scraped off with a scraper.

[0044] In the step (2), after the base fabric is wet impregnated, the impregnated base fabric is treated with a DMF / water mixed solution of a certain concentration (the solubility ratio of water to DMF is 60-70:30-40) to solidify the polyurethane slurry in the base fabric.

[0045] By adopting the above scheme, the polyurethane resin in the base fabric solidifies and forms a microporous membrane. The specific operation method is to place the impregnated base fabric into a pre-solidification tank at an angle perpendicular to the liquid surface for solidification treatment to ensure that the polyurethane resin in the base fabric can be completely solidified to form a microporous membrane so as to have a good feel; after the pre-solidification is completed, it enters the main solidification tank for further solidification, and the entire solidification process takes 20-35 minutes.

[0046] Furthermore, after the solidification treatment in step (2), the solidified base fabric is washed with water. The residual DMF in the base fabric is removed by washing with water, and the sugar content of the residual DMF in the base fabric after washing is strictly controlled to be less than 0.5, thereby preventing the residual DMF from damaging the morphology of the fine porous membrane of the polyurethane resin in the base fabric during the subsequent processing, thereby affecting the hand feel.

[0047] In the step (4), a further preferred solution is to print a layer of polyurethane resin solution on the surface of the bass with cracked style, and dry it to solidify it; then dye the printed bass to obtain suede ultrafine fiber synthetic leather with cracked ceramic pattern style. The polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 150-250 parts of organic solvent, and 7-15 parts of anti-phenol yellow additive. The polyurethane resin of the polyurethane resin solution is a resin with a modulus of 50-75MPa, and the dyeing performance of the resin of the polyurethane resin solution is better than the dyeing performance of the resin impregnated slurry in step (2). In a specific embodiment of the organic solvent, DMF is selected.

[0048] By adopting the above scheme, due to the difference in the resin dyeability of the polyurethane resin solution and the impregnation slurry, the protrusions and cracks on the surface of the synthetic leather are dyed in different shades, which is conducive to obtaining a more natural and distinct crack ceramic pattern surface style. Among them, the impregnation slurry preferably uses polyurethane resins that are not easy to dye, and the polyurethane resin solution preferably uses easy-to-dye resins with a modulus of 50-75MPa. After dyeing, the protrusions on the surface are darker in color due to the easy-to-dye resin, while the cracks and gullies are lighter in color or colorless due to the difficult-to-dye resin, thereby obtaining suede leather with a crack ceramic pattern surface style.

[0049] The easy-to-dye resin refers to a resin in which polyethylene glycol accounts for 10-25% of the molar ratio of the polyol component, and the non-dyeable resin is a resin without polyethylene glycol added. The polyurethane resin of the polyurethane resin solution is a resin with a modulus of 50-75MPa. The modulus range of the resin is limited to well balance the hand feel and surface treatment effect, ensuring that the final microfiber leather has a soft hand feel and a cracked ceramic pattern surface style effect that is obvious and realistic.

[0050] Furthermore, in step (4), the polyurethane resin solution is printed on the surface of the bass with a cracked style, and the gap between the printing roller and the rubber roller is controlled to be 0.10-0.15 mm smaller than the original thickness of the bass. This solution ensures that the printed material only acts on the raised parts of the bass cracks during the coating process, while the grooves of the cracks will not be coated with resin; this effect will result in a more obvious visual difference when dyeing is performed later.

[0051] Furthermore, in the step (4), the temperature of the base drying treatment is 100-120° C. and the drying time is 3-8 minutes.

[0052] Furthermore, in the step (4), the suede leather after printing is dyed by roller dyeing, the base is immersed in a prepared dyeing liquid tank, the temperature is controlled at 35°C and kept warm for 120 minutes, and then the temperature is increased by one degree per minute. After the temperature reaches 97°C, it is kept warm for 30 minutes, then taken out and pressed.

[0053] In the step (1), PA slices and PE slices are mixed in a certain proportion, and the blended sea-island fibers are prepared by a spinning process; a specific embodiment of the certain proportion is that the mass ratio of PA slices to PE slices is 50:50.

[0054] The above solution makes the bass relatively soft. When spinning sea-island fibers, the extrusion volume per unit time is less than that of ordinary fibers, and the melt residence time is longer. To avoid thermal degradation, the temperature cannot be too high, and the temperature is best controlled at 225-255℃.

[0055] Furthermore, in the spinning process of step (1), the filaments extruded from the spinneret are treated with an oil agent to improve their antistatic properties, and the drying temperature of the treated filaments is controlled at 60-85° C. to avoid affecting the processing of subsequent steps.

[0056] Furthermore, during the spinning process of step (1), the fibers treated with the oil agent are also subjected to a stretching treatment to improve the mechanical properties of the fibers; the stretching ratio is controlled at 3.0-3.8 times, and the stretched fibers are curled and cut to finally obtain blended sea island staple fibers.

[0057] In the step (1), the blended sea-island fibers are needle-punched to obtain a non-woven fabric, which is then heat-set to obtain a base fabric.

[0058] With the above solution, the interlayer force of the nonwoven fabric is relatively low and it is easy to produce a relatively obvious uniform split. The relevant process parameters need to be specially adjusted during the needle punching process to ensure that the fiber web composed of the sea-island fiber will not be seriously damaged. The process parameters are: the needle density is 155-350C / cm 2 The needle punching depth of 1#-7# is 10 / 10 / 8 / 4 / 4 / 0 / 0mm, and the weight of the needle-punched non-woven fabric is controlled to be 690-750g; the peel strength of the non-woven fabric is 25-50N / 5cm.

[0059] Furthermore, in the needling process of step (1), the last two needling machines of the fiber web are designed to perform 1-2 needling trimming steps, so that a sea-island fiber needle-punched nonwoven fabric with a better surface condition can be obtained.

[0060] Furthermore, in the heat setting treatment of step (1), the setting temperature is set to 95 / 115 / 125 / 135 / 140 / 142 / 143°C in 7 ovens, and the temperature is controlled within the requirement of ±5°C. The non-woven fabric is heated and set in ovens with different temperatures from low to high. Since the non-woven fabric after needle punching is loose and has a low apparent density, it is not conducive to subsequent processing. Therefore, the specific heat setting treatment is used to improve the stiffness and flatness of the non-woven fabric and increase the apparent density.

[0061] Furthermore, after the heat setting treatment in step (1), the thickness of the base fabric obtained by heat setting is controlled within 2.80-3.50 mm, and the density is controlled within 0.230-0.290 g / cm 3 The thickness of the base fabric used for post-processing should not be less than 2.80mm, otherwise it will easily affect the production of the post-process. The base fabric may be wrinkled during impregnation or the width may be too small, which may affect the surface of the bass.

[0062] In the step (3), the washed base fabric is sent to an extraction tank for toluene reduction treatment to remove the PE with a marine structure in the base fabric fibers. The method of using toluene for reduction is specifically as follows: the solidified and completely washed base fabric is passed through an extraction tank with a continuous roller filled with hot toluene (85°C ± 5°C) for 40-60 minutes, and after the reduction is completed, it is passed through a hot water tank (90-105°C) to remove the residual toluene, and the PE residue is controlled to be less than 1%.

[0063] Furthermore, in the process of extracting and reducing the base fabric in step (3), while ensuring complete reduction, the vehicle speed is controlled to be high as much as possible for continuous production to avoid excessive stretching of the base fabric due to long high-temperature treatment time and continuous tension of the production line, which affects the hand feel.

[0064] Furthermore, in the step (3), the semi-finished product after weight reduction is oiled and dried to obtain a bass with a cracked surface, and then the bass is softened by a continuous kneading machine.

[0065] The oiling treatment is that the reduced bass is squeezed and impregnated with the configured post-treatment agent through 4 rubber rollers, the liquid penetration rate is 50-90%, the temperature is controlled at 120-155°C, the whole oiling process takes 40-50 minutes, and the base fabric should maintain a natural contraction state throughout the process to avoid large differences in the weft direction of the bass.

[0066] After the drying treatment, the leather is further kneaded by a mechanical continuous kneading machine, the kneading frequency of which is controlled at 380-450 Hz, and the whole kneading process takes 30-40 minutes.

[0067] Embodiment 1

[0068] A method for preparing a cracked ceramic pattern suede microfiber leather comprises the following steps:

[0069] (1) PA slices and PE slices are mixed in a mass ratio of 50:50, and a blended sea-island fiber is obtained by a spinning process; the blended sea-island fiber is needle-punched to obtain a non-woven fabric, and then subjected to a heat setting treatment to obtain a base fabric;

[0070] (2) preparing a crack-forming wet-process polyurethane impregnation slurry, which is specifically composed of the following components in parts by mass: 30 parts of ultra-high modulus resin, 70 parts of ultra-low modulus resin, 10 parts of filler, 80 parts of DMF and a solidification regulating agent, wherein the solidification regulating agent accounts for 1.8% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%; the selected polyurethane resins are all non-dyeing resins;

[0071] The base fabric is impregnated with the polyurethane impregnation slurry, and then the impregnated base fabric is solidified by passing through a DMF / water mixed solution (the solubility ratio of water to DMF is 65:35) of a certain concentration, and the base fabric after complete solidification is passed through a water washing tank to remove residual DMF;

[0072] (3) The washed base fabric is sent to a draw-out tank for toluene reduction treatment, and the semi-finished product after reduction is oiled and dried to obtain a bass with a cracked surface, and then the bass is softened by a continuous kneading machine;

[0073] (4) Printing a layer of polyurethane resin solution on the surface of the bass with cracked style, and drying it to solidify it; the polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 150 parts of DMF, and 7 parts of anti-phenol yellow additive; the polyurethane resin is an easy-to-dye resin with a modulus of 50-75 MPa; dyeing the printed bass to obtain a suede microfiber synthetic leather with a cracked ceramic pattern style.

[0074] Embodiment 2

[0075] A method for preparing a cracked ceramic pattern suede microfiber leather comprises the following steps:

[0076] (1) PA slices and PE slices are mixed in a mass ratio of 50:50, and a blended sea-island fiber is obtained by a spinning process; the blended sea-island fiber is needle-punched to obtain a non-woven fabric, and then subjected to a heat setting treatment to obtain a base fabric;

[0077] (2) preparing a crack-resistant wet-process polyurethane impregnation slurry, which is specifically composed of the following components in parts by mass: 35 parts of ultra-high modulus resin, 65 parts of ultra-low modulus resin, 20 parts of filler, 100 parts of DMF and a solidification regulating agent, wherein the solidification regulating agent accounts for 2.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%; the selected polyurethane resins are all non-dyeable resins;

[0078] The base fabric is impregnated with the polyurethane impregnation slurry, the base fabric is impregnated in an impregnation tank filled with the impregnation slurry, and a plurality of rollers are passed to ensure that the base fabric is completely impregnated with the slurry, and the gap is adjusted to be 15s less than the thickness of the base fabric; after the base fabric passes through the impregnation tank, the excess impregnation slurry on the front and back of the base fabric is scraped off with a scraper;

[0079] Afterwards, the impregnated base fabric is solidified by passing a certain concentration of DMF / water mixed solution (the solubility ratio of water to DMF is 62:38) through the base fabric. The specific operation steps are as follows: the impregnated base fabric enters the pre-solidification tank at an angle perpendicular to the liquid surface for solidification treatment, and then enters the main solidification tank for further solidification after the pre-solidification is completed. The whole solidification process takes 20 minutes.

[0080] After the solidification is complete, the base fabric is passed through a water washing tank to remove the residual DMF; after the water washing is completed, the sugar content of the residual DMF in the base fabric is controlled to be less than 0.5;

[0081] (3) The washed base fabric is sent to a draw-out tank for toluene reduction treatment, and the semi-finished product after reduction is oiled and dried to obtain a bass with a cracked surface, and then the bass is softened by a continuous kneading machine;

[0082] (4) printing a layer of polyurethane resin solution on the surface of the cracked bass, wherein the gap between the printing roller and the rubber roller is controlled to be 0.10 mm smaller than the original thickness of the bass; then drying to solidify the bass, the bass drying treatment temperature is 100° C., and the drying time is 3 minutes;

[0083] The polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 200 parts of DMF, and 11 parts of anti-phenol yellowing additive; the polyurethane resin is an easily dyeable resin with a modulus of 50-75 MPa;

[0084] Afterwards, the suede leather after printing is dyed by roller dyeing. The bass is immersed in the configured dyeing liquid tank, and the temperature is controlled at 35°C for 120 minutes. Then the temperature is increased by one degree every minute. After it reaches 97°C, it is kept warm for 30 minutes, then taken out and pressed; finally, a suede microfiber synthetic leather with a cracked ceramic pattern is obtained.

[0085] Embodiment 3

[0086] A method for preparing a cracked ceramic pattern suede microfiber leather comprises the following steps:

[0087] (1) PA slices and PE slices are mixed in a mass ratio of 50:50, and a blended sea-island fiber is obtained by a spinning process; the blended sea-island fiber is needle-punched to obtain a non-woven fabric, and then subjected to a heat setting treatment to obtain a base fabric;

[0088] The acupuncture process is adjusted to process parameters: needle density is 155-350C / cm2, acupuncture depth 1#-7# is 10 / 10 / 8 / 4 / 4 / 0 / 0mm, and the weight of the needle-punched non-woven fabric is controlled to be 720g; the peel strength of the non-woven fabric is 35N / 5cm;

[0089] The heat setting treatment, the setting temperature is set to 95 / 115 / 125 / 135 / 140 / 142 / 143°C according to the 7 sections of the oven, and the temperature is controlled within the requirement of ±5°C. The non-woven fabric is heated and set in the ovens with different temperatures from low to high. The thickness of the base fabric obtained by heat setting is controlled at 3.50mm, and the density is controlled at 0.250g / cm 3 ;

[0090] (2) preparing a crack-resistant wet-process polyurethane impregnation slurry, which is specifically composed of the following components in parts by mass: 40 parts of ultra-high modulus resin, 60 parts of ultra-low modulus resin, 30 parts of filler, 120 parts of DMF and a solidification regulating agent, wherein the solidification regulating agent accounts for 3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%; the selected polyurethane resins are all non-dyeable resins;

[0091] The base fabric is impregnated with the polyurethane impregnation slurry, the base fabric is impregnated in an impregnation tank filled with the impregnation slurry, and a plurality of rollers are passed to ensure that the base fabric is completely impregnated with the slurry, and the gap is adjusted to be 20s less than the thickness of the base fabric; after the base fabric passes through the impregnation tank, the excess impregnation slurry on the front and back of the base fabric is scraped off with a scraper;

[0092] Afterwards, the impregnated base fabric is solidified by passing a certain concentration of DMF / water mixed solution (the solubility ratio of water to DMF is 70:30). The specific operation steps are as follows: the impregnated base fabric enters the pre-solidification tank at an angle perpendicular to the liquid surface for solidification treatment, and then enters the main solidification tank for further solidification after the pre-solidification is completed. The whole solidification process takes 35 minutes.

[0093] After the solidification is complete, the base fabric is passed through a water washing tank to remove the residual DMF; after the water washing is completed, the sugar content of the residual DMF in the base fabric is controlled to be less than 0.5;

[0094] (3) The washed base fabric is sent to a draw-out tank for toluene reduction treatment, and the semi-finished product after reduction is oiled and dried to obtain a bass with a cracked surface, and then the bass is softened by a continuous kneading machine;

[0095] The specific steps of toluene reduction treatment are as follows: the solidified and completely washed base fabric is passed through a continuous roller extraction tank containing hot toluene (85°C ± 5°C) for 50 minutes, and after the reduction is completed, the residual toluene is removed through a hot water tank (100°C) to control the PE residue to less than 1%;

[0096] The reduced bass is squeezed and impregnated with the prepared post-treatment agent through 4 rubber rollers, with a liquid penetration rate of 70%, the temperature is controlled at 135°C, and the entire oiling process takes 45 minutes.

[0097] After being softened and dried, the bass is kneaded by a mechanical continuous leather kneading machine. The kneading frequency is controlled at 400HZ and the whole kneading process takes 35 minutes.

[0098] (4) printing a layer of polyurethane resin solution on the surface of the cracked bass, wherein the gap between the printing roller and the rubber roller is controlled to be 0.13 mm smaller than the original thickness of the bass; then drying to solidify the bass, the bass drying treatment temperature is 110° C., and the drying time is 5 minutes;

[0099] The polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 200 parts of DMF, and 11 parts of anti-phenol yellowing additive; the polyurethane resin is an easily dyeable resin with a modulus of 50-75 MPa;

[0100] Afterwards, the suede leather after printing is dyed by roller dyeing. The bass is immersed in the configured dyeing liquid tank, and the temperature is controlled at 35°C for 120 minutes. Then the temperature is increased by one degree every minute. After it reaches 97°C, it is kept warm for 30 minutes, then taken out and pressed; finally, a suede microfiber synthetic leather with a cracked ceramic pattern is obtained.

[0101] The present invention also relates to a cracked ceramic pattern suede microfiber leather, which is prepared by the above-mentioned preparation method of the cracked ceramic pattern suede microfiber leather, so as to achieve a surface effect of the suede microfiber leather with a cracked style.

[0102] The above descriptions are only preferred embodiments of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.

Claims

1. A crack wet-process polyurethane impregnation slurry, characterized in that: The invention is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and solidification regulating auxiliary agent, wherein the solidification regulating auxiliary agent accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%.

2. The crack wet-process polyurethane impregnation slurry according to claim 1, characterized in that: The filler is one or more of calcium carbonate, talcum powder and barium sulfate.

3. A method for preparing a cracked ceramic suede microfiber leather, characterized in that: The following steps are involved: (1) The base fabric is made of blended sea island fibers; (2) The base fabric is subjected to wet impregnation treatment, and a crackle wet polyurethane impregnation slurry is used, which is composed of the following components in parts by mass: 20-40 parts of ultra-high modulus resin, 60-80 parts of ultra-low modulus resin, 10-30 parts of filler, 80-120 parts of organic solvent and solidification regulating aid, wherein the solidification regulating aid accounts for 1.8%-3.5% of the total mass of the resin; the ultra-high modulus resin has a modulus of 220-280 MPa and a polyether content of 20-30%, and the ultra-low modulus resin has a modulus of 10-35 MPa and a polyether content of 70-80%; (3) reducing the weight of the base fabric, applying oil and drying the base fabric to obtain a bass with a cracked surface; (4) The bass is dyed to obtain a suede microfiber synthetic leather with a cracked ceramic pattern style.

4. The method for preparing a cracked ceramic suede microfiber leather according to claim 3, characterized in that: In the step (4), a polyurethane resin solution is printed on the surface of the cracked bass and dried to solidify it; The printed bass is then dyed to obtain a suede microfiber synthetic leather with a cracked ceramic pattern style; The polyurethane resin solution is composed of the following components in parts by mass: 100 parts of polyurethane resin, 150-250 parts of organic solvent, and 7-15 parts of anti-phenol yellow additive; The polyurethane resin in the polyurethane resin solution has a modulus of 50-75 MPa, and the dyeing performance of the resin in the polyurethane resin solution is better than the dyeing performance of the resin impregnated slurry in step (2).

5. The method for preparing a cracked ceramic suede microfiber leather as claimed in claim 3 or 4, characterized in that: In the step (4), the polyurethane resin solution is printed on the surface of the cracked bass, and the gap between the printing roller and the rubber roller is controlled to be 0.10-0.15 mm smaller than the original thickness of the bass.

6. The method for preparing a cracked ceramic suede microfiber leather according to claim 3, characterized in that: In the step (4), dyeing is carried out by roller dyeing, the bass is immersed in a prepared dyeing liquid tank, the temperature is controlled at 35°C and kept warm for 120 minutes, and then the temperature is increased by one degree per minute. After the temperature reaches 97°C, it is kept warm for 30 minutes, then taken out and pressed.

7. The method for preparing a cracked ceramic suede microfiber leather according to claim 3, characterized in that: In the step (1), PA slices and PE slices are mixed and a spinning process is used to obtain a blended sea-island fiber; the blended sea-island fiber is needle-punched to obtain a non-woven fabric, which is then subjected to a heat-setting treatment to obtain a base fabric.

8. The method for preparing a cracked ceramic suede microfiber leather according to claim 3, characterized in that: In the step (1), the thickness of the obtained base fabric is controlled at 2.80-3.50 mm, and the density is controlled at 0.230-0.290 g / cm 3 .

9. The method for preparing a cracked ceramic suede microfiber leather according to claim 3, characterized in that: In the step (2), the impregnated base fabric is treated with a DMF / water mixed solution to solidify the polyurethane slurry in the base fabric, and the base fabric after complete solidification is passed through a water washing tank to remove residual DMF. After the water washing is completed, the sugar content of the residual DMF in the base fabric is less than 0.

5.

10. A cracked ceramic pattern suede microfiber leather, prepared by the preparation method of the cracked ceramic pattern suede microfiber leather according to any one of claims 3 to 9.