Biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sand area

By using sand barriers mixed with reflective fiber and polylactic fiber in the sand area, the problems of low efficiency and high cost of traditional sand barriers are solved, and the dual goals of improving photovoltaic power generation and sand prevention and control are achieved, which is convenient Material transportation and simple laying methods.

CN118997103APending Publication Date: 2024-11-22INNER MONGOLIA AGRICULTURAL UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411084961.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The construction efficiency of traditional polylactic fiber sand barriers in desert areas is low and expensive, making it difficult to fully utilize ecological and economic benefits, and at the same time, it is impossible to effectively increase the photovoltaic power generation.

Method used

The surface layer of reflective polylactic fiber fabric made of mixed reflective fiber and polylactic fiber is filled with sand and soil to form sand barriers, and is laid under double-sided solar photovoltaic panels in the sand area, and the reflection effect is used to increase the power generation.

Benefits of technology

It significantly improves the photovoltaic power generation in the sand area, enhances the sand prevention and control effect, is convenient and simple to lay, and has long-term and stable protective benefits and environmental protection characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118997103A_ABST
    Figure CN118997103A_ABST
Patent Text Reader

Abstract

The invention provides a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in a desert area, which is formed by filling a reflective polylactic acid fiber fabric surface layer with sandy soil and is used for photovoltaic desertification prevention and control engineering in a desert area. The reflective polylactic acid fiber fabric surface layer is formed by mixing and weaving reflective fibers and polylactic acid fibers, and the reflective fibers are prepared from transparent polyamide slices, have regular triangular sections and are used for realizing total reflection of incident light. The biodegradable reflective polylactic acid fiber sand-protecting barrier is laid under a double-sided solar photovoltaic panel on the earth surface of a desert area, the barrier body structure can be kept relatively stable for a long time, the protection benefit is exerted, the power generation amount of the double-sided solar photovoltaic panel can be improved by fully utilizing the reflective effect while sand prevention and control are achieved, and the service life of the sand-protecting barrier is prolonged. And an effective practical desertification control technology is provided for desertification prevention and control engineering practice under the photovoltaic panel in the desert area.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sand prevention and control, and specifically relates to a biodegradable reflective polylactic acid fiber sand barrier used for photovoltaic power generation in sandy areas. Background Art

[0002] Sand barriers are an important technical means of sand prevention and control projects. Laying sand barriers can maintain the relative stability of the wind-eroded sand surface of moving sand dunes, effectively control the movement of sand on the surface of sand dunes, and form a relatively stable wind-eroded concave surface within the effective protection range of the sand barriers, which is conducive to the survival and growth of artificial vegetation and the recovery of natural vegetation, and gradually achieve the effect of sand prevention and control.

[0003] Bio-based degradable fiber sand barriers are not restricted by transportation conditions and can be made from local materials. Different sand prevention and control technology systems can be formed according to different terrain conditions in desert areas. Polylactic acid fiber sand barriers are one of them. CN101614005A discloses a sand barrier made of biodegradable materials, wherein the biodegradable material is polylactic acid fiber (PLA) fabric. The sand barriers woven with the polylactic acid fiber fabric include flat sand barriers and low vertical sand barriers. However, this traditional polylactic acid fiber sand barrier, although it has a good effect of preventing wind and fixing sand, only solves the problem of sand prevention and control, and the laying efficiency is relatively low during on-site construction in desert areas, and the price is relatively expensive, so it is difficult to give full play to its ecological and economic benefits in desert areas.

[0004] In view of the different purposes of vigorously developing the photovoltaic industry, reflective properties are added to the bio-based degradable sand barrier materials, and then filled with sand from local materials to form a barrier body. According to the actual wind speed, wind direction, sand particle size and composition, and in accordance with different protection purposes such as consolidation, blocking and transportation, a complete sand control technology system suitable for local sand is formed. This is a new idea for photovoltaic sand control in desert areas. Reflective materials (also called retro-reflective materials or retro-reflective materials) are added to the production process of traditional environmentally friendly and pollution-free bio-based degradable fiber sandbag sand barriers. By implanting high-refractive glass beads or forming a micro-prism structure in the bio-based degradable fiber sand barrier material, the light is reflected back to the light source along the original path, forming retro-reflection (or retro-reflection). Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas in view of the deficiencies of the above-mentioned prior art. A reflective polylactic acid fiber fabric surface layer formed by a mix of reflective fibers and polylactic acid fibers is used as the basic material of the sand barrier. Local materials are used to fill sand to form a sand barrier. The reflective polylactic acid fiber sand barrier is laid flat under the double-sided solar photovoltaic panels in the sandy area to obtain a biodegradable reflective polylactic acid fiber sand barrier suitable for increasing photovoltaic power generation in the sandy area.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0007] A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas. The biodegradable reflective polylactic acid fiber sand barrier is formed by filling sand with a reflective polylactic acid fiber fabric surface layer, and is used for photovoltaic sand prevention and control projects in desert areas. The reflective polylactic acid fiber fabric surface layer is mixed with reflective fibers and polylactic acid fibers, and the content of the reflective fibers is 40% to 60%.

[0008] Preferably, the method for preparing the reflective fiber comprises the following steps:

[0009] The transparent polyamide slices are placed in a vacuum drying oven for drying, and the dried polyamide slices are spun into primary fibers with a regular triangle cross section using a spinning machine, and the primary fibers are then drafted to obtain transparent polyamide finished sheet fibers, namely reflective fibers.

[0010] Preferably, the transparency of the polyamide slice is 75% to 95%.

[0011] Preferably, the drying temperature of the vacuum drying oven is 95° C. to 105° C., and the drying time is 80 h to 100 h.

[0012] Preferably, the stretching temperature is 145° C. to 170° C., and the stretching ratio is 1.5 to 2 times.

[0013] Preferably, the reflective fiber has a fiber linear density of 60 dtex to 300 dtex.

[0014] Preferably, the polylactic acid fiber is made from biomass raw materials (corn starch, cassava starch, beet, sucrose, straw cellulose, etc.) fermented into small molecule lactic acid by microorganisms, and then dehydrated and condensed with a solvent by a direct polycondensation method to obtain high molecular weight polylactic acid (PLA) and then melt-spinned; the fiber linear density of the polylactic acid fiber is 30dtex to 60dtex.

[0015] Preferably, the reflective polylactic acid fiber fabric surface layer is cylindrical, and the diameter of the cylinder is 5.5 cm to 8.5 cm.

[0016] Preferably, the reflective polylactic acid fiber sand barrier is a flat sand barrier.

[0017] The present invention also provides a method for laying the reflective polylactic acid fiber sand barrier, comprising the following steps:

[0018] S1, mixing reflective fibers and polylactic acid fibers into a cylindrical shape with a diameter of 5.5 cm to 8.5 cm to obtain a reflective polylactic acid fiber fabric surface layer, wherein the reflective fiber content in the reflective polylactic acid fiber fabric surface layer is 40% to 60%;

[0019] S2, knotting the lower end of the reflective polylactic acid fiber fabric surface layer obtained in S1, and then putting it on the outside of the PVC tube, using the PVC tube to put sand into the reflective polylactic acid fiber fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier;

[0020] S3. Spread the reflective polylactic acid fiber sand barrier obtained in S2 under the double-sided solar photovoltaic panels in the sand area by format method or full coverage method according to different specifications, so as to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area.

[0021] The present invention has significant technical effects due to the adoption of the above technical solution:

[0022] 1. The present invention provides a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas. The basic material of the sand barrier is a biodegradable reflective polylactic acid fiber fabric surface layer. Local materials are used to fill sand to form a sand barrier, which is then laid under the double-sided solar photovoltaic panels on the surface of the desert area. The sand barrier is used for photovoltaic sand prevention and control projects in desert areas. While preventing and controlling sand, the reflective effect can be fully utilized to increase the power generation of the double-sided solar photovoltaic panels.

[0023] 2. On the basis of the traditional polylactic acid sand barrier, the present invention adds reflective fiber to make an environmentally friendly biodegradable reflective polylactic acid fiber sand barrier, wherein the reflective fiber is a transparent polyamide fiber prepared from transparent polyamide slices and has an equilateral triangle cross-section, which can achieve total reflection of incident light. The reflective polylactic acid fiber sand barrier of the present invention can reflect sunlight in the desert area to the back of the photovoltaic panel with double-sided power generation with strong reflection effect, which can increase the power generation of the photovoltaic panel.

[0024] 3. The reflective polylactic acid fiber sand barrier of the present invention can increase the surface roughness, reduce the wind speed near the ground, prevent the direct effect of airflow on the ground, increase the wind speed started by sand particles, increase the erosion resistance, change the law of wind and sand erosion and accumulation, and has obvious sand prevention and fixation effects.

[0025] 4. The reflective polylactic acid fiber sand barrier of the present invention is based on the research and development concept of low-carbon and environmental protection of the entire industry chain, focuses on the actual technical needs of the sand barrier application market, and provides an effective and practical sand control technology for the practice of sand control and sand control engineering, which can maintain the relative stability of the barrier structure for a long time and exert protective benefits. Moreover, compared with traditional sand barriers, bio-based degradable fiber sand barriers have excellent characteristics such as convenient material transportation, simple laying method, long on-site storage time, and green environmental protection.

[0026] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a 0.5m×0.5m format paved reflective polylactic acid fiber sand barrier diagram of Example 1 of the present invention;

[0028] Figure 2 It is a 1m×1m format paved reflective polylactic acid fiber sand barrier diagram of Example 2 of the present invention;

[0029] Figure 3 This is a fully covered reflective polylactic acid fiber sand barrier diagram of Example 3 of the present invention;

[0030] Figure 4 This is a comparison diagram of three reflective polylactic acid fiber sand barriers in Examples 1 to 3;

[0031] Figure 5 It is the fitting curve of the irradiance improvement efficiency of the reflective polylactic acid fiber sand barrier;

[0032] Figure 6 It is the trend of power generation of full-coverage reflective polylactic acid fiber sand barrier over time. DETAILED DESCRIPTION

[0033] Example 1

[0034] A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas, the manufacturing and laying method of which comprises the following steps:

[0035] S1. Preparation of reflective polylactic acid fiber fabric surface layer

[0036] S101, Reflective fiber preparation

[0037] The transparent polyamide slices are placed in a vacuum drying oven and dried at 95°C for 100 hours, and then the dried polyamide slices are spun into primary fibers with a regular triangle cross section by a spinning machine, and then the primary fibers are drafted by a drafting device at a temperature of 145°C with a drafting ratio of 2 times to obtain a transparent polyamide finished sheet fiber, i.e., a reflective fiber; the polyamide slices are a polymer prepared from diaminodicyclohexylmethane and dodecanedioic acid, purchased from Evonik of Germany, and have a transparency of 75% to 95%; the obtained reflective fiber has a fiber linear density of 60dtex to 300dtex;

[0038] S102. Preparation of reflective polylactic acid fiber fabric surface layer

[0039] 50% of the reflective fiber obtained from S101 and 50% of the polylactic acid fiber are mixed into a cylindrical shape with a diameter of 5.5 cm to obtain a reflective polylactic acid fiber fabric surface layer; wherein the fiber linear density of the polylactic acid fiber is 30dtex to 60dtex;

[0040] S2, putting the reflective polylactic acid fiber tubular fabric surface layer obtained in S1 on the outside of a PVC tube with a diameter of 157.5px to 187.5px and a length of 1500px to 1750px, tying a knot at the lower end of the tubular fabric surface layer, and then using the PVC tube to load sand into the reflective polylactic acid fiber tubular fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier;

[0041] S3, according to the format method, the reflective polylactic acid fiber sand barrier obtained in S2 is laid flat under the double-sided solar photovoltaic panel in the sand area in a specification of 0.5m×0.5m, to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area, see Figure 1 .

[0042] Example 2

[0043] A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas, the manufacturing and laying method of which comprises the following steps:

[0044] S1. Preparation of reflective polylactic acid fiber fabric surface layer

[0045] S101, Reflective fiber preparation

[0046] The transparent polyamide slices are placed in a vacuum drying oven and dried at 105° C. for 80 hours, and then the dried polyamide slices are spun into primary fibers with a regular triangle cross section by a spinning machine, and then the primary fibers are drafted by a drafting device at a temperature of 170° C., with a drafting ratio of 1.5 times, to obtain a transparent polyamide finished fiber sheet, i.e., a reflective fiber; the polyamide slices are a polymer prepared from diaminodicyclohexylmethane and dodecanedioic acid, purchased from Evonik of Germany, and have a transparency of 75% to 95%; the obtained reflective fiber has a fiber linear density of 60 dtex to 300 dtex;

[0047] S102. Preparation of reflective polylactic acid fiber fabric surface layer

[0048] 40% of the reflective fiber obtained from S101 and 60% of the polylactic acid fiber are mixed into a cylindrical shape with a diameter of 8.5 cm to obtain a reflective polylactic acid fiber fabric surface layer; wherein the fiber linear density of the polylactic acid fiber is 30dtex to 60dtex;

[0049] S2, putting the reflective polylactic acid fiber tubular fabric surface layer obtained in S1 on the outside of a PVC tube with a diameter of 157.5px to 187.5px and a length of 1500px to 1750px, tying a knot at the lower end of the tubular fabric surface layer, and then using the PVC tube to load sand into the reflective polylactic acid fiber tubular fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier;

[0050] S3, according to the format method, the reflective polylactic acid fiber sand barrier obtained in S2 is laid flat under the double-sided solar photovoltaic panel in the sand area in a specification of 1m×1m to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area, see Figure 2 .

[0051] Example 3

[0052] A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas, the manufacturing and laying method of which comprises the following steps:

[0053] S1. Preparation of reflective polylactic acid fiber fabric surface layer

[0054] S101, Reflective fiber preparation

[0055] The transparent polyamide slices are placed in a vacuum drying oven and dried at 100° C. for 90 hours. Then, the dried polyamide slices are spun into primary fibers with a regular triangle cross section by a spinning machine. The primary fibers are then stretched by a stretching device at 155° C. with a stretching ratio of 2 times to obtain a transparent polyamide finished fiber sheet, i.e., a reflective fiber. The polyamide slices are polymers prepared from diaminodicyclohexylmethane and dodecanedioic acid, purchased from Evonik of Germany, with a transparency of 75% to 95%. The obtained reflective fiber has a fiber linear density of 60 dtex to 300 dtex.

[0056] S102. Preparation of reflective polylactic acid fiber fabric surface layer

[0057] 60% of the reflective fiber obtained from S101 and 40% of the polylactic acid fiber are mixed into a cylindrical shape with a diameter of 6.5 cm to obtain a reflective polylactic acid fiber fabric surface layer; wherein the fiber linear density of the polylactic acid fiber is 30 dtex to 60 dtex;

[0058] S2, putting the reflective polylactic acid fiber tubular fabric surface layer obtained in S1 on the outside of a PVC tube with a diameter of 157.5px to 187.5px and a length of 1500px to 1750px, tying a knot at the lower end of the tubular fabric surface layer, and then using the PVC tube to load sand into the reflective polylactic acid fiber tubular fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier;

[0059] S3, using the full coverage method, the sand barrier obtained in S2 is laid flat under the double-sided solar photovoltaic panels in the sand area to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area, see Figure 3 .

[0060] Example 4

[0061] A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas, the manufacturing and laying method of which comprises the following steps:

[0062] S1. Preparation of reflective polylactic acid fiber fabric surface layer

[0063] S101, Reflective fiber preparation

[0064] The transparent polyamide slices are placed in a vacuum drying oven and dried at 102° C. for 95 hours, and then the dried polyamide slices are spun into primary fibers with a regular triangle cross section by a spinning machine, and then the primary fibers are drafted by a drafting device at a temperature of 165° C., with a drafting ratio of 1.5 times, to obtain a transparent polyamide finished fiber sheet, i.e., a reflective fiber; the polyamide slices are a polymer prepared from diaminodicyclohexylmethane and dodecanedioic acid, purchased from Evonik of Germany, and have a transparency of 75% to 95%; the obtained reflective fiber has a fiber linear density of 60 dtex to 300 dtex;

[0065] S102. Preparation of reflective polylactic acid fiber fabric surface layer

[0066] 45% of the reflective fiber obtained from S101 and 55% of the polylactic acid fiber are mixed into a cylindrical shape with a diameter of 7.5 cm to obtain a reflective polylactic acid fiber fabric surface layer; wherein the fiber linear density of the polylactic acid fiber is 30 dtex to 60 dtex;

[0067] S2, putting the reflective polylactic acid fiber tubular fabric surface layer obtained in S1 on the outside of a PVC tube with a diameter of 157.5px to 187.5px and a length of 1500px to 1750px, tying a knot at the lower end of the tubular fabric surface layer, and then using the PVC tube to load sand into the reflective polylactic acid fiber tubular fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier;

[0068] S3. According to the format method, the reflective polylactic acid fiber sand barrier obtained in S2 is laid flat under the double-sided solar photovoltaic panel in the sand area with a specification of 1.5m×1.5m to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area.

[0069] Figure 4The following are pictures of reflective polylactic acid fiber sand barriers laid under the solar photovoltaic panels in the sandy area using the three laying methods of Examples 1 to 3. The following results were obtained by studying the sand prevention and control effects and photovoltaic power generation efficiency of the reflective polylactic acid fiber sand barriers using the three laying methods:

[0070] The test shows that the reflective PLA fiber sand barrier can increase the surface roughness, reduce the wind speed near the ground, prevent the direct effect of airflow on the ground, increase the wind speed of sand particles, increase the anti-erosion ability, change the law of wind and sand erosion, and have a significant effect in preventing and fixing sand. Compared with the traditional PLA fiber sand barrier, the bio-based degradable reflective PLA fiber sand barrier provides an effective and practical sand control technology for the practice of sand control and sand control engineering under photovoltaic panels in desert areas. It can maintain the relative stability of the barrier structure for a long time and exert protective benefits. While preventing and fixing sand, it can also make full use of the reflective effect to increase the power generation of double-sided solar photovoltaic panels.

[0071] By monitoring the irradiance, the effects of different reflective polylactic acid fiber sand barriers on the efficiency of photovoltaic power generation irradiance improvement were compared. Figure 5 The data comparison clearly shows that the setting of sand barriers significantly improves the efficiency of photovoltaic irradiance. Among the three specifications of sand barriers, the fully covered sand barrier can efficiently reflect sunlight. Compared with the three specifications of sand barriers, the fully covered sand barrier has the best efficiency of improving photovoltaic irradiance, which is 94%. The efficiency of improving irradiance of the 0.5m×0.5m sand barrier is 38%, and the efficiency of improving irradiance of the 1m×1m sand barrier is only 30%.

[0072] By observing the changing trend of the total radiation in different time periods, from sunrise to sunset, with the change of the solar altitude angle, the radiation energy gradually increases and reaches the highest point at noon. At sunset, the area of ​​sunlight exposure gradually decreases. After laying the sand barrier, it is observed that the reflection effect of the sand barrier increases the sunlight energy absorbed by the solar panels. Under the full coverage of the sand barrier, the reflection effect is significantly enhanced, which significantly increases the radiation absorbed by the solar panels at noon compared to when the sand barrier is not laid. The cumulative radiation is 3.4MJ / m 2 The 0.5m×0.5m and 1m×1m sand barriers have relatively weaker reflection effects due to their smaller sizes. The accumulated radiation at noon is 2.7MJ / m 2 and 2.3MJ / m 2 .

[0073] The setting of sand barriers significantly improves the efficiency of photovoltaic power generation. Among the three specifications of sand barriers, the fully covered sand barriers can efficiently reflect sunlight, which greatly enhances the performance of power generation. The results are as follows: Figure 6As shown. At 6:00 when the sun rises, the solar panels begin the energy conversion process. The power generation increases from 0 to 50MV at 10:00 in the morning. From 10:00, the efficiency reaches the peak and remains stable for a period of time until after 12:00. The power generation output begins to gradually decline, from 12:00 to 13:00 to 45MV, and from 13:00 the decline rate slows down until it drops to 15:00. In the late stage of a growth cycle, the trend of slowing growth becomes particularly obvious, and from 16:00 the decline rate becomes faster, starting from 42MV and dropping all the way to 20:00 when the power output returns to zero.

[0074] By comparing the effects of reflective polylactic acid fiber sand barriers with different laying methods on the power generation efficiency of photovoltaic panels, the study found that full-coverage sand barriers have the best improvement effect, which can increase the power generation efficiency by up to 94%; 0.5m×0.5m sand barriers are second, with an improvement of 38%; and 1m×1m sand barriers can only increase the power generation efficiency by 30%.

[0075] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in sandy areas, characterized in that: The biodegradable reflective polylactic acid fiber sand barrier is formed by filling sand with a reflective polylactic acid fiber fabric surface layer, and is used in photovoltaic sand prevention and control projects in desert areas; the reflective polylactic acid fiber fabric surface layer is mixed with reflective fibers and polylactic acid fibers, and the content of the reflective fibers is 40% to 60%.

2. The reflective polylactic acid fiber sand barrier according to claim 1, characterized in that: The preparation method of the reflective fiber comprises the following steps: The transparent polyamide slices are placed in a vacuum drying oven for drying, and the dried polyamide slices are spun into primary fibers with a regular triangle cross section using a spinning machine, and the primary fibers are then drafted to obtain transparent polyamide finished sheet fibers, namely reflective fibers.

3. The reflective polylactic acid fiber sand barrier according to claim 2, characterized in that: The transparency of the polyamide slice is 75% to 95%.

4. The reflective polylactic acid fiber sand barrier according to claim 2, characterized in that: The drying temperature of the vacuum drying oven is 95° C. to 105° C., and the drying time is 80 h to 100 h.

5. The reflective polylactic acid fiber sand barrier according to claim 2, characterized in that: The stretching temperature is 145° C. to 170° C., and the stretching ratio is 1.5 to 2 times.

6. The reflective polylactic acid fiber sand barrier according to any one of claims 1 to 5, characterized in that: The fiber linear density of the reflective fiber is 60 dtex to 300 dtex.

7. The reflective polylactic acid fiber sand barrier according to claim 1, characterized in that: The fiber linear density of the polylactic acid fiber is 30 dtex to 60 dtex.

8. The reflective polylactic acid fiber sand barrier according to claim 1, characterized in that: The reflective polylactic acid fiber fabric surface layer is cylindrical, and the diameter of the cylinder is 5.5 cm to 8.5 cm.

9. The reflective polylactic acid fiber sand barrier according to claim 1, characterized in that: The reflective polylactic acid fiber sand barrier is a flat-laid sand barrier.

10. A method for laying a reflective polylactic acid fiber sand barrier as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: S1, mixing reflective fibers and polylactic acid fibers into a cylindrical shape with a diameter of 5.5 cm to 8.5 cm to obtain a reflective polylactic acid fiber fabric surface layer, wherein the reflective fiber content in the reflective polylactic acid fiber fabric surface layer is 40% to 60%; S2, knotting the lower end of the reflective polylactic acid fiber fabric surface layer obtained in S1, and then putting it on the outside of the PVC tube, using the PVC tube to put sand into the reflective polylactic acid fiber fabric surface layer, filling it tightly, and obtaining a reflective polylactic acid fiber sand barrier; S3. Spread the reflective polylactic acid fiber sand barrier obtained in S2 under the double-sided solar photovoltaic panels in the sand area by format method or full coverage method according to different specifications, so as to obtain a biodegradable reflective polylactic acid fiber sand barrier for photovoltaic power generation in the sand area.

Citation Information

Patent Citations

  • Sand-protecting barrier made from biodegradable materials and preparation method thereof

    CN101614005A