Repair method for port wharf steel pipe pile

By using an epoxy zinc-rich primer layer and a multi-layer fiber cloth on the steel pipe piles at the port terminal, combined with acid- and alkali-resistant anti-corrosion coatings, the problem of insufficient mechanical properties in the existing technology is solved, and the steel pipe piles are realized Efficient repair and anti-corrosion effects, with the functions of resisting seawater corrosion, anti-permeability, acid and alkali resistance and salt spray resistance.

CN118997134AInactive Publication Date: 2024-11-22GUANGZHOU MARITIME INST
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411105492.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When repairing steel pipe piles at port terminals, it is difficult to effectively improve their mechanical properties, and it is impossible to achieve the functions of resisting seawater corrosion, anti-permeability, acid and alkali resistance and salt spray resistance at the same time.

Method used

Epoxy zinc-rich primer is used as the sacrificial anode, combined with the first carbon fiber cloth and glass fiber cloth, and applied with anti-acid, anti-corrosion coating with acid and alkali resistance, anti-corrosion and anti-permeability functions to form a multi-layer structure to enhance the steel pipe Mechanical properties of piles.

Benefits of technology

Through this method, the mechanical properties of steel pipe piles are significantly improved, the accelerated corrosion of the primary battery reaction is avoided, the resistance to seawater corrosion is enhanced, the corrosion and reinforcement effect is achieved, and the resistance to seawater corrosion, anti-permeability, acid and alkali resistance is met. and salt spray resistance requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004990641510000071
    Figure BDA0004990641510000071
  • Figure BDA0004990641510000081
    Figure BDA0004990641510000081
Patent Text Reader

Abstract

The invention relates to a repairing method for a port wharf steel pipe pile. The repairing method comprises the steps of surface treatment; the surface is coated with an epoxy zinc-rich priming coat, and the surface of the epoxy zinc-rich priming coat is polished; a first cloth layer is pasted outside the epoxy zinc-rich primer, the first cloth layer comprises first carbon fiber cloth and first glass fiber cloth which are glued, and the outer side face of the first carbon fiber cloth is attached to and combined with the surface of the epoxy zinc-rich primer; the first glass fiber cloth is coated with a first anti-corrosion coating and dried; the first anticorrosive coating comprises the following components: 80-100 parts of a waterborne polyurethane emulsion, 60-70 parts of glass flakes, 5-8 parts of a coalescing agent, 1-3 parts of a flatting agent, 1-2 parts of a defoaming agent and 1-2 parts of a thickening agent. The effects of seawater corrosion resistance, permeation resistance, acid and alkali resistance, salt mist resistance, mechanical property improvement and the like can be achieved through simple design and technology, repairing of the steel pipe pile can be achieved, and corrosion prevention and reinforcement of the steel pipe pile can also be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for repairing underwater structures in marine port buildings, specifically a method for repairing steel pipe piles at port wharves. Background Technology

[0002] For steel pipe piles used in port terminals, the marine corrosion environment can be divided into five zones: the marine atmospheric zone, the splash zone, the tidal zone, the fully submerged zone, and the seabed mud zone. The splash zone is the most severely corroded zone. During the use of these steel pipe piles, corrosion gradually worsens over time, thus requiring repair. Repair solutions for corrosion in the splash zone need to consider not only acid and alkali resistance, antigen-antigen battery reaction, and salt spray resistance, but also the impact of corrosion on the mechanical properties of the steel pipe pile. Current technologies primarily use coatings and adhesives to bond cracks and coating gaps in the steel pipe pile, but these methods have limitations in restoring mechanical properties.

[0003] The invention patent application published on February 6, 2024, with publication number CN117511331A and titled "An epoxy heavy-duty anti-corrosion coating for marine splash zones and its preparation method" discloses an epoxy heavy-duty anti-corrosion coating for marine splash zones and its preparation method. Epoxy heavy-duty anti-corrosion coatings for marine splash zones consist of component A and component B in a weight ratio of 3-6:1. By weight, component A includes 30-50 parts bisphenol A type epoxy resin, 2-8 parts petroleum resin, 0.5-2 parts thixotropic agent, 3-8 parts pigment, 20-50 parts filler, 0.5-1.5 parts silane coupling agent, 1-3 parts reactive diluent, 3-10 parts primary solvent, and 0.2-0.5 parts leveling agent. By weight, component B includes 20-40 parts of an amine composite curing agent prepolymer synthesized from polyamide resin and bisphenol F epoxy resin, 20-40 parts amine curing agent, 20-50 parts secondary solvent, 2-5 parts accelerator, and 1-2 parts defoamer. However, this coating is only suitable for corrosion protection and cannot effectively improve the mechanical properties of the steel pipe piles to be repaired. Summary of the Invention

[0004] In order to solve the problems existing in the prior art, the present invention aims to provide a method for repairing steel pipe piles in port terminals.

[0005] The present invention discloses a method for repairing steel pipe piles at port terminals, comprising: Step 1, performing surface treatment on the area of ​​the steel pipe pile to be repaired before applying an epoxy zinc-rich primer; Step 2, applying an epoxy zinc-rich primer to the surface of the area and polishing the surface of the epoxy zinc-rich primer; Step 3, attaching a first fabric layer to the epoxy zinc-rich primer, the first fabric layer comprising a first carbon fiber fabric and a first glass fiber fabric stacked together, the first carbon fiber fabric and the first glass fiber fabric being bonded together, the outer side of the first carbon fiber fabric being adhered to and bonded to the surface of the epoxy zinc-rich primer; Step 4, applying a first anti-corrosion coating to the first glass fiber fabric and drying it; the first anti-corrosion coating comprises the following components: 80-100 parts of water-based polyurethane emulsion, 60-70 parts of glass flakes, 5-8 parts of film-forming aid, 1-3 parts of leveling agent, 1-2 parts of defoamer, and 1-2 parts of thickener.

[0006] Preferably, in step three, an epoxy adhesive is used to bond the outer side of the first carbon fiber cloth to the epoxy zinc-rich base coating, wherein the epoxy adhesive includes epoxy carbon fiber adhesive or epoxy two-component adhesive.

[0007] Preferably, the first anti-corrosion coating comprises the following components: 90 parts of water-based polyurethane emulsion, 65 parts of glass flakes, 7 parts of the film-forming aid, 2 parts of the leveling agent, 2 parts of the defoamer, and 2 parts of the thickener.

[0008] Preferably, the preparation method of the first anti-corrosion coating is as follows: water-based polyurethane emulsion, glass flakes, film-forming aid, leveling agent, defoamer, and thickener are placed in a container and stirred at a stirring speed of 1000 rpm-1500 rpm for 0.5-1 hours, and then used within 2-3 hours.

[0009] Preferably, the first glass fiber cloth and the glass flakes are treated with a silane coupling agent before use. The first glass fiber cloth is made of alkali-resistant glass fiber, and the glass flakes are alkali-resistant glass flakes.

[0010] Preferably, the first fiberglass cloth has a size of 1000g or 1200g and a model number of 300 / 3, 450 / 1, 450 / 2, or 450 / 3.

[0011] Preferably, the aspect ratio of the alkali-resistant glass flakes is 50-120.

[0012] Preferably, the silane coupling agent is an amide-based silane coupling agent.

[0013] Preferably, the film-forming aid is dipropylene glycol butyl ether.

[0014] Preferably, the leveling agent is polydimethoxysiloxane.

[0015] Preferably, the defoamer is an organosilicone defoamer.

[0016] Preferably, the thickener is titanium dioxide.

[0017] Beneficial effects

[0018] The present invention discloses a method for repairing steel pipe piles at port terminals. Its advantages lie in that the epoxy zinc-rich primer can act as a sacrificial anode to protect the steel pipe pile. When the adhesive on the surface of the epoxy zinc-rich primer is an insulator, the first carbon fiber cloth and the epoxy zinc-rich primer are insulated. When the adhesive becomes conductive due to seawater intrusion, the epoxy zinc-rich primer should provide more electrons to the steel pipe pile, which acts as the cathode, preventing the galvanic reaction caused by seawater simultaneously intruding into the epoxy zinc-rich primer and the surface of the steel pipe pile, thus accelerating the corrosion of the steel pipe pile. In this case, since the adhesive acts as a conductor, the first carbon fiber cloth can act as a conductor between the zinc powder in the epoxy zinc-rich primer, allowing the zinc powder to release electrons more quickly and provide them to the steel pipe pile, reducing or preventing corrosion from the galvanic reaction. The first carbon fiber cloth can improve the mechanical properties of the steel pipe pile; the first glass fiber cloth can serve as a support for the first carbon fiber cloth and a skeleton for the first anti-corrosion coating, thereby improving the mechanical properties of the first carbon fiber cloth and the first anti-corrosion coating, further increasing the mechanical properties of the steel pipe pile, and avoiding insufficient mechanical properties of the anti-corrosion coating and the resulting problems such as peeling and cracking; the first anti-corrosion coating contains water-based polyurethane with acid and alkali resistance, anti-corrosion and salt spray resistance, as well as anti-corrosion and anti-permeability glass flakes, which can resist seawater corrosion. In summary, the present invention can achieve the effects of seawater corrosion resistance, anti-permeability, acid and alkali resistance, salt spray resistance and improved mechanical properties with simple design and process, which can not only repair the steel pipe pile, but also prevent corrosion and reinforce the steel pipe pile. Detailed Implementation

[0019] The present invention discloses a method for repairing steel pipe piles at port terminals, comprising: Step 1, performing surface treatment on the area of ​​the steel pipe pile to be repaired before applying an epoxy zinc-rich primer; Step 2, applying an epoxy zinc-rich primer to the surface of the area and polishing the surface of the epoxy zinc-rich primer; Step 3, attaching a first fabric layer to the epoxy zinc-rich primer, the first fabric layer comprising a first carbon fiber fabric and a first glass fiber fabric stacked together, the first carbon fiber fabric and the first glass fiber fabric being bonded together, the outer side of the first carbon fiber fabric being adhered to and bonded to the surface of the epoxy zinc-rich primer; Step 4, applying a first anti-corrosion coating to the first glass fiber fabric and drying it; the first anti-corrosion coating comprises the following components: 80-100 parts of water-based polyurethane emulsion, 60-70 parts of glass flakes, 5-8 parts of film-forming aid, 1-3 parts of leveling agent, 1-2 parts of defoamer, and 1-2 parts of thickener.

[0020] The present invention discloses a method for repairing steel pipe piles at port terminals. Its advantages lie in that the epoxy zinc-rich primer can act as a sacrificial anode to protect the steel pipe pile. When the adhesive on the surface of the epoxy zinc-rich primer is an insulator, the first carbon fiber cloth and the epoxy zinc-rich primer are insulated. When the adhesive becomes conductive due to seawater intrusion, the epoxy zinc-rich primer should provide more electrons to the steel pipe pile, which acts as the cathode, preventing the galvanic reaction caused by seawater simultaneously intruding into the epoxy zinc-rich primer and the surface of the steel pipe pile, thus accelerating the corrosion of the steel pipe pile. In this case, since the adhesive acts as a conductor, the first carbon fiber cloth can act as a conductor between the zinc powder in the epoxy zinc-rich primer, allowing the zinc powder to release electrons more quickly and provide them to the steel pipe pile, reducing or preventing corrosion from the galvanic reaction. The first carbon fiber cloth can improve the mechanical properties of the steel pipe pile; the first glass fiber cloth can serve as a support for the first carbon fiber cloth and a skeleton for the first anti-corrosion coating, thereby improving the mechanical properties of the first carbon fiber cloth and the first anti-corrosion coating, further increasing the mechanical properties of the steel pipe pile, and avoiding insufficient mechanical properties of the anti-corrosion coating and the resulting problems such as peeling and cracking; the first anti-corrosion coating contains water-based polyurethane with acid and alkali resistance, anti-corrosion and salt spray resistance, as well as anti-corrosion and anti-permeability glass flakes, which can resist seawater corrosion. In summary, the present invention can achieve the effects of seawater corrosion resistance, anti-permeability, acid and alkali resistance, salt spray resistance and improved mechanical properties with simple design and process, which can not only repair the steel pipe pile, but also prevent corrosion and reinforce the steel pipe pile.

[0021] In specific implementation, the adhesive used to bond the first fabric layer overflows onto the outer periphery of the first fabric layer, ensuring that the first fabric layer is firmly bonded to the epoxy zinc-rich primer coating. The epoxy zinc-rich primer coating is a conventional epoxy zinc-rich primer coating; those skilled in the art can choose from conventional epoxy zinc-rich primer coatings according to actual needs. The first carbon fiber cloth and the first glass fiber cloth are fixed together by an adhesive bonding method, specifically epoxy adhesive. The drying method is a conventional drying method; those skilled in the art can select from conventional drying methods according to actual needs.

[0022] Preferably, in step three, an epoxy adhesive is used to bond the outer side of the first carbon fiber cloth to the epoxy zinc-rich base coating, wherein the epoxy adhesive includes epoxy carbon fiber adhesive or epoxy two-component adhesive.

[0023] In specific implementation, an epoxy adhesive with high adhesion is used to achieve the technical effect of bonding the outer side of the first carbon fiber cloth to the epoxy zinc-rich base coating. Specifically, the epoxy adhesive may include epoxy carbon fiber adhesive that can tightly bond the first carbon fiber cloth to the epoxy zinc-rich coating, or it may be a two-component epoxy adhesive with extremely strong adhesion and very convenient use. The epoxy adhesive has excellent waterproof and corrosion-resistant properties. If it is soaked in seawater with high salt content for a long time, the first carbon fiber cloth can accelerate the release of electrons from the zinc powder to the steel pipe pile, reducing or avoiding corrosion of the steel pipe pile due to loss of electrons caused by the galvanic reaction caused by seawater on the surface of the steel pipe pile.

[0024] Preferably, the first anti-corrosion coating comprises the following components: 90 parts of water-based polyurethane emulsion, 65 parts of glass flakes, 7 parts of the film-forming aid, 2 parts of the leveling agent, 2 parts of the defoamer, and 2 parts of the thickener.

[0025] In practice, the above scheme is a preferred formulation of the first anti-corrosion coating.

[0026] Preferably, the preparation method of the first anti-corrosion coating is as follows: water-based polyurethane emulsion, glass flakes, film-forming aid, leveling agent, defoamer, and thickener are placed in a container and stirred at a stirring speed of 1000 rpm-1500 rpm for 0.5-1 hours, and then used within 2-3 hours.

[0027] Preferably, the first glass fiber cloth and the glass flakes are treated with a silane coupling agent before use. The first glass fiber cloth is made of alkali-resistant glass fiber, and the glass flakes are alkali-resistant glass flakes.

[0028] In specific implementation, the first glass fiber cloth and the glass flakes are treated with a silane coupling agent to improve their compatibility with the organic components of the first anti-corrosion coating, making them easier to apply and form a film. The first glass fiber cloth is prepared using alkali-resistant glass fiber, and the alkali-resistant glass flakes are used to make them resistant to corrosion from alkaline seawater. The aspect ratio of the alkali-resistant glass flakes is 50-120. Those skilled in the art can select a certain range of aspect ratios, such as 100-120 or 90-110, according to actual needs.

[0029] Preferably, the first fiberglass cloth has a size of 1000g or 1200g and a model number of 300 / 3, 450 / 1, 450 / 2, or 450 / 3.

[0030] In practice, provided that the construction conditions and acceptance standards allow, try to select fiberglass cloth with larger size and model (450 / 1 model is larger than 300 / 3, and 450 / 3 model is larger than 450 / 1). This will enable the steel pipe pile to obtain better mechanical properties, impermeability and corrosion resistance.

[0031] Preferably, the silane coupling agent is an amide-based silane coupling agent.

[0032] In practice, using an amide-based silane coupling agent can improve the compatibility of the first glass fiber cloth and the glass flakes with the waterborne polyurethane containing amide groups.

[0033] Preferably, the film-forming aid is dipropylene glycol butyl ether.

[0034] Preferably, the leveling agent is polydimethoxysiloxane.

[0035] Preferably, the defoamer is an organosilicone defoamer.

[0036] Preferably, the thickener is titanium dioxide.

[0037] In practice, the titanium dioxide also has anti-corrosion properties.

[0038] The present application will be further described below with reference to specific embodiments and comparative examples, but the present application is not limited to the following embodiments. The materials and reagents used in the embodiments and comparative examples can be obtained commercially and are readily available.

[0039] Unless otherwise specified, the materials and reagents used are conventional products in the prior art and are readily available.

[0040] Example 1

[0041] A 150mm × 70mm × 0.5mm steel plate is selected, surface-treated, and coated with an epoxy zinc-rich primer. The surface of the epoxy zinc-rich primer is then sanded, and a first fabric layer is adhered. This first fabric layer comprises stacked first carbon fiber cloth and first glass fiber cloth, bonded together with epoxy adhesive. The outer side of the first carbon fiber cloth is attached to and bonded to the surface of the epoxy zinc-rich primer. A first anti-corrosion coating is applied to the outside of the first glass fiber cloth and dried. An anti-corrosion coating comprises the following components: 90 parts water-based polyurethane emulsion, 65 parts glass flakes, 7 parts film-forming aid, 2 parts leveling agent, 2 parts defoamer, and 2 parts thickener; the film-forming aid is dipropylene glycol butyl ether, the leveling agent is polydimethoxysiloxane, the defoamer is an organosilicon defoamer, and the thickener is titanium dioxide. The first glass fiber cloth has parameters of 1200g, type 450 / 3, and is made of alkali-resistant glass fiber. The glass flakes are made of alkali-resistant glass flakes with an aspect ratio of 100-120. The epoxy adhesive used to bond the first cloth layer is epoxy carbon fiber adhesive.

[0042] The preparation method of the first anti-corrosion coating is as follows: water-based polyurethane emulsion, glass flakes, film-forming aid, leveling agent, defoamer, and thickener are placed in a container and stirred at a stirring speed of 1200 rpm. After stirring for 0.5 hours, it is used within 3 hours.

[0043] Example 2

[0044] Unlike Example 1,

[0045] The first anti-corrosion coating comprises the following components: 80 parts of water-based polyurethane emulsion, 60 parts of glass flakes, 5 parts of film-forming aid, 1 part of leveling agent, 1 part of defoamer, and 1 part of thickener.

[0046] The first fiberglass cloth has the following parameters: 1000g, 300 / 3 type, and is made of alkali-resistant fiberglass. The glass flakes are also made of alkali-resistant glass flakes, with an aspect ratio of 70-80. The epoxy adhesive used to bond the first cloth layer is a two-component epoxy adhesive.

[0047] The preparation method of the first anti-corrosion coating is as follows: water-based polyurethane emulsion, glass flakes, film-forming aid, leveling agent, defoamer, and thickener are placed in a container and stirred at a stirring speed of 1000 rpm. After stirring for 1 hour, it is used within 2 hours.

[0048] The rest is the same as in Example 1.

[0049] Example 3

[0050] Unlike Example 1,

[0051] The first anti-corrosion coating comprises the following components: 100 parts of water-based polyurethane emulsion, 70 parts of glass flakes, 8 parts of film-forming aid, 1 part of leveling agent, 1 part of defoamer, and 1 part of thickener.

[0052] The first fiberglass cloth has parameters of 1200g, type 450 / 1, and is made of alkali-resistant fiberglass. The glass flakes are made of alkali-resistant glass flakes, and the aspect ratio is 90-110. The epoxy adhesive used to bond the first cloth layer is a two-component epoxy adhesive.

[0053] The preparation method of the first anti-corrosion coating is as follows: water-based polyurethane emulsion, glass flakes, film-forming aid, leveling agent, defoamer, and thickener are placed in a container and stirred at a stirring speed of 1500 rpm. After stirring for 1 hour, it is used within 2 hours.

[0054] The rest is the same as in Example 1.

[0055] Example 4

[0056] Unlike Example 1, in Example 4, the first glass fiber cloth and the glass flakes are ordinary glass fiber cloth and ordinary glass flakes, and are not made of alkali-resistant glass.

[0057] Comparative Example 1

[0058] Unlike Example 1, Comparative Example 1 has no epoxy zinc-rich coating.

[0059] Comparative Example 2

[0060] Unlike Example 1, Comparative Example 2 did not include the first carbon fiber cloth.

[0061] Comparative Example 3

[0062] Unlike Example 1, Comparative Example 3 did not include the first glass fiber cloth.

[0063] Comparative Example 4

[0064] Unlike Example 1, Comparative Example 4 did not have the first anti-corrosion coating.

[0065] Comparative Example 5

[0066] Unlike Example 1, the first anti-corrosion coating in Comparative Example 5 does not contain the alkali-resistant glass flakes, and the mass fraction of the alkali-resistant glass flakes is replaced by the corresponding mass fraction of the aqueous polyurethane emulsion.

[0067] The products of the examples and comparative examples were subjected to cyclic aging tests for 4200 hours, seawater immersion for 4200 hours, salt spray tests for 3000 hours, and adhesion strength tests. The test standards were based on the requirements of GB / T 31817 Technical Specification for Protective Coating of Wind Power Generation Facilities and ISO20340 standard. The test results are shown in Table 1.

[0068] Table 1 Test results of the examples and comparative examples

[0069]

[0070]

[0071] The test data from Examples 1 to 4 demonstrate that the method of this application can improve the corrosion resistance, durability, and other indicators of the steel pipe piles to meet relevant standard requirements, while the comparative examples do not. In Comparative Example 5, the lack of alkali-resistant glass flakes severely reduces its corrosion resistance and durability, and also significantly decreases its bond strength. Furthermore, according to the tensile test results, Example 1, which includes the first carbon fiber cloth, shows inferior mechanical properties compared to Comparative Example 2, which does not. Similarly, Example 1, which includes the first glass fiber cloth, shows inferior mechanical properties compared to Comparative Example 3, which does not.

[0072] The tensile strength and yield strength of the following examples and comparative examples were tested according to GB / T228.1-2010 standard.

[0073] Tensile strength, MPa Example 1 808 Comparative Example 2 475 Comparative Example 3 757

[0074] The tensile strength of the steel plate used in Example 1 is 370 MPa.

[0075] In the description of this invention, it should be understood that directional terms such as "front, back, up, down, left, right", "horizontal, vertical, horizontal" and "top, bottom" indicate the orientation or positional relationship, which are usually for the convenience of describing this invention and simplifying the description. Unless otherwise stated, these directional terms do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore should not be construed as limiting the scope of protection of this invention.

[0076] For those skilled in the art, various other corresponding changes and modifications can be made based on the technical solutions and concepts described above, and all such changes and modifications should fall within the protection scope of the claims of this invention.

Claims

1. A method for repairing steel pipe piles at a port terminal, characterized in that: include: Step 1: Surface treatment is performed on the part of the steel pipe pile that needs to be repaired before coating with epoxy zinc-rich primer; Step 2, coating the surface of the part with an epoxy zinc-rich primer, and polishing the surface of the epoxy zinc-rich primer; Step 3, pasting a first cloth layer on the outside of the epoxy zinc-rich primer, wherein the first cloth layer includes a first carbon fiber cloth and a first glass fiber cloth stacked together, the first carbon fiber cloth and the first glass fiber cloth are glued together, and the outer side of the first carbon fiber cloth is attached to and combined with the surface of the epoxy zinc-rich primer; Step 4, applying a first anti-corrosion coating on the first glass fiber cloth and drying it; The first anticorrosive coating comprises the following components: 80-100 parts of waterborne polyurethane emulsion, 60-70 parts of glass flakes, 5-8 parts of film-forming aid, 1-3 parts of leveling agent, 1-2 parts of defoaming agent and 1-2 parts of thickener.

2. The method for repairing steel pipe piles at a port terminal according to claim 1, characterized in that: In step three, epoxy glue is used to bond the outer side surface of the first carbon fiber cloth to the epoxy zinc-rich primer layer. The epoxy glue includes epoxy carbon fiber glue or epoxy two-component glue.

3. The method for repairing steel pipe piles at a port terminal according to claim 1, characterized in that: The first anti-corrosion coating comprises the following components: 90 parts of waterborne polyurethane emulsion, 65 parts of glass flakes, 7 parts of the film-forming aid, 2 parts of the leveling agent, 2 parts of the defoaming agent, and 2 parts of the thickener.

4. The method for repairing steel pipe piles at a port terminal according to claim 3, characterized in that: The first glass fiber cloth and the glass flakes are treated with a silane coupling agent before use; the first glass fiber cloth is made of alkali-resistant glass fibers, and the glass flakes are alkali-resistant glass flakes.

5. The method for repairing steel pipe piles at a port terminal according to claim 4, characterized in that: The size of the first glass fiber cloth is 1000g or 1200g, and the model is 300 / 3, 450 / 1, 450 / 2, 450 / 3.

6. The method for repairing steel pipe piles at a port terminal according to claim 4, characterized in that: The silane coupling agent is an amide silane coupling agent.

7. The method for repairing steel pipe piles at a port terminal according to claim 6, characterized in that: The film-forming aid is dipropylene glycol butyl ether.

8. The method for repairing steel pipe piles at a port terminal according to claim 1, characterized in that: The leveling agent is polydimethoxysiloxane.

9. The method for repairing steel pipe piles at a port terminal according to claim 1, characterized in that: The defoamer is an organosilicon defoamer.

10. The method for repairing steel pipe piles at a port terminal according to claim 1, characterized in that: The thickener is titanium dioxide.

Citation Information

Patent Citations

  • Epoxy heavy anti-corrosion coating for marine splash zone and preparation method of epoxy heavy anti-corrosion coating

    CN117511331A

  • Fiber reinforced composite material recycled masonry aggregate concrete steel pipe hollow pile

    CN108118692A

  • Green and environment-friendly waterproof coating and preparation method thereof

    CN118185446A

  • Steel pipe pile street lamp foundation

    CN118407455A

  • Anti-corrosion structure for marine steel pile

    CN214695768U