Method for improving deuterium and tritium retention resistance of tungsten alloy divertor and tungsten alloy divertor
By building a double-scale micro-nano composite structure on the surface of the tungsten alloy filter, changing the incident angle and reflection direction of the deuterium tritium ions, the problem of poor retention performance of the tungsten alloy filter is solved, and the steady state of the nuclear fusion reaction is achieved run.
Patent Information
- Application Number
- CN202410937520.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-22
AI Technical Summary
Tungsten alloy filters are prone to deuterium and tritium retention under high-temperature plasma bombardment, resulting in a decline in material performance. The existing methods cannot effectively improve the anti-deuterium and tritium retention performance, limiting the steady-state operation time and experimental development of nuclear fusion reactors.
The double-scale micro-nano composite structure is constructed on the surface of the tungsten alloy filter, including micron-level concave and convex surfaces and nano-level stripes. By changing the incident angle and reflection direction of deuterium and tritium ions, the retention of deuterium and tritium is reduced by using the ionic effect, combined with plasma splashing Theoretical model of the radiology and molecular dynamics simulation optimized structure.
It effectively reduces the retention of deuterium and tritium on the surface of tungsten alloy, improves the reflection coefficient and release effect, and ensures the steady-state operation of nuclear fusion reaction under high parameters and long pulses.
Smart Images

Figure CN119008042A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the deuterium and tritium retention resistance of a tungsten alloy divertor and a tungsten alloy divertor, belonging to the technical field of tungsten alloy divertors. Background Art
[0002] Nuclear fusion energy is clean and abundant, offering the best solution to humanity's energy needs. The tungsten alloy divertor in the tokamak device of current thermonuclear fusion reactors removes heat and helium ash from the fusion reaction, ensuring the integrity of the first-wall material. However, tungsten alloy divertors are directly exposed to the continuous bombardment of high-temperature plasma, and deuterium and tritium easily accumulate and aggregate on their surfaces, forming a large number of helium bubbles. This allows deuterium and tritium ions to penetrate the material, reducing the high-temperature mechanical properties of the tungsten alloy and causing warping and even tunneling, which is the primary cause of tungsten alloy divertor failure.
[0003] At present, the methods to improve the deuterium and tritium resistance of tungsten alloy divertor include: improving the shape accuracy of the divertor, regulating the grain size of tungsten alloy, and constructing a nano-scale dense oxide film. However, due to the limitations of geometric processing accuracy, the limited range of grain size adjustment, and the easy shedding of the oxide film, the above methods are still unable to make the deuterium and tritium retention on the divertor surface ≤700g, which limits the improvement of the steady-state operation time of the thermonuclear fusion reaction and restricts the construction and development of nuclear fusion experimental reactors. Summary of the Invention
[0004] The object of the present invention is to provide a method for improving the deuterium and tritium retention resistance of a tungsten alloy divertor, which can solve the problem that the current tungsten alloy divertor has poor deuterium and tritium retention resistance and cannot meet the use requirements.
[0005] Another object of the present invention is to provide a tungsten alloy divertor, which can solve the problem that the current tungsten alloy divertor has poor anti-deuterium and tritium retention performance and cannot meet the use requirements.
[0006] In order to achieve the above objectives, the technical solution adopted by the method of improving the resistance of tungsten alloy divertor to deuterium and tritium retention in the present invention is as follows:
[0007] A method for improving the deuterium and tritium retention resistance of a tungsten alloy divertor is disclosed. A dual-scale micro-nano composite structure is constructed on the deuterium and tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The dual-scale micro-nano composite structure is utilized to change the incident angle and reflection direction of the deuterium and tritium ions, thereby reducing the deuterium and tritium ion retention on the tungsten alloy surface.
[0008] The present invention constructs and regulates a dual-scale micro-nano composite structure on the surface of a tungsten alloy divertor, causing the surface to exhibit an "ion-repelling effect," effectively reducing the amount of deuterium and tritium retained on the tungsten alloy surface. When the micro-nano composite structure on the tungsten alloy surface is subjected to continuous bombardment by high-temperature plasma deuterium and tritium, the micron-scale fluctuations caused by the micron-scale structure can change the incident angle and reflection direction of the deuterium and tritium ions, increasing the reflection coefficient; the nanoscale structure can increase the specific surface area, further enhancing the reflection coefficient and release effect of the deuterium and tritium ions. The micron-scale and nanoscale structures on the tungsten alloy surface influence each other and synergize to effectively reduce the clustering and enrichment of deuterium and tritium plasma on the tungsten alloy surface, causing it to exhibit an "ion-repelling" effect, thereby reducing the amount of deuterium and tritium ion retention on the tungsten alloy surface.
[0009] Preferably, a plasma sputtering theoretical model of the composite micro-nano structure is established, and the dual-scale micro-nano composite structure is optimized in combination with molecular dynamics simulation; the plasma sputtering theoretical model is constructed based on SRIM software and TMAP software developed and optimized by LAMMPS software.
[0010] In this study, a theoretical model of plasma sputtering for composite micro- and nanostructures was established, combined with molecular dynamics simulations, to study the incident and reflected fluxes of deuterium and tritium ions for different types of micro- and nanostructures. This allowed the optimization of dual-scale micro- and nanostructured surfaces for both ion repellency and resistance to deuterium and tritium retention. Furthermore, microstructures of varying structural forms can be constructed at different curvatures, depending on the shape of the divertor surface, to ensure consistent reflection direction and reflection coefficient for the high-temperature plasma.
[0011] The technical solution adopted by the tungsten alloy divertor of the present invention is:
[0012] A tungsten alloy divertor is provided. A dual-scale micro-nano composite structure is constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanometer-scale stripes distributed on the micron-scale concave-convex surface.
[0013] The surface of the tungsten alloy divertor of the present invention is constructed with a dual-scale micro-nano composite structure, which exhibits an "ion-repelling effect" and can effectively reduce the retention of deuterium and tritium on the surface of the tungsten alloy. When the micro-nano composite structure on the surface of the tungsten alloy is subjected to continuous bombardment by high-temperature plasma deuterium and tritium, the micron-scale fluctuations caused by the micron-scale structure can change the incident angle and reflection direction of the deuterium and tritium ions, increasing the reflection coefficient; the nanoscale structure can increase the specific surface area, further improving the reflection coefficient and release effect of the deuterium and tritium ions. The micron-scale and nanoscale structures on the surface of the tungsten alloy influence each other and synergize to effectively reduce the clustering and enrichment of deuterium and tritium plasma on the surface of the tungsten alloy, causing it to exhibit an "ion-repelling" effect, thereby reducing the retention of deuterium and tritium ions on the surface of the tungsten alloy.
[0014] Preferably, the micron-scale concave-convex surface is formed by a plurality of micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor.
[0015] Preferably, the micron-sized pits are circular pits, square pits, or elliptical pits.
[0016] Preferably, the scale of the micron-scale pits is 10 to 50 μm, and the scale of the nanoscale stripes is 1 to 7 nm.
[0017] Preferably, the micron-sized pits have a recessed depth of 10 to 15 μm and an opening width of 16 to 25 μm.
[0018] Preferably, the density of micron-scale pits is 1.6×10 3 ~3.9×10 3 Pieces / mm 2 .
[0019] Preferably, the width of the nanoscale stripes is 5 to 7 nm, the distance between two adjacent nanoscale stripes is 4 to 7 nm, and the height of the nanoscale stripes is 3 to 5 nm.
[0020] Preferably, the density of the nanoscale stripes is 1.9×10 10 ~6.2×10 10 Pieces / mm 2 .
[0021] During the machining of the tungsten alloy divertor, the present invention combines a natural diamond tool with ultrasonic vibration, coupled with the spindle rotation and radial feed of an ultra-precision machine tool. This allows for the efficient and precise construction of a dual-scale micro-nano composite structure on the tungsten alloy divertor surface. The ultra-precision machine tool employed in the present invention has a kinematic accuracy of less than 15nm in the axial direction and less than 15nm in the radial direction, with a C-axis resolution of 0.026 arc seconds. Alcohol is used as the coolant during machining, and the tool's cutting edge has a circular arc profile waviness of less than 0.15μm.
[0022] In the present invention, the natural diamond tool can be sharpened or customized according to the shape of the processed surface micro-nano composite structure.
[0023] The tool motion trajectory of the ultrasonic elliptical vibration cutting method vibrates in the form of an ellipse. During the cutting process, the tool will generate two vibrations of different amplitudes with a certain phase difference in the circumferential and radial directions, and the tool and the cutting surface can be laterally separated, avoiding the problem of tool edge jumping caused by unidirectional vibration. Since there is a certain phase difference between the vibration of the tool in the diameter direction and the cutting direction, it moves in an elliptical shape in the XZ plane. During the cutting process, the tool's motion trajectory causes it to periodically contact and separate with the workpiece and chips, and the radial movement of the tool can reduce the extrusion force between the tool and the chips. At the same time, the friction between the tool and the chips pulls the chips outward, avoiding adhesion between the tool and the chips.
[0024] In the present invention, the reflection and release effects of micron-scale structures and nano-scale structures on deuterium and tritium ions are utilized, and the ion-repelling effect on the surface of the composite structure is regulated to improve the deuterium and tritium retention resistance of the tungsten alloy surface, thereby ensuring the steady-state operation of the nuclear fusion reaction under high parameters and long pulses. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the dual-scale micro-nano composite structure constructed on the surface of tungsten alloy in Example 1 of the present invention;
[0026] Figure 2 Schematic diagram of the dual-scale micro-nano composite structure constructed on the surface of tungsten alloy in Example 2 of the present invention;
[0027] Figure 3 Schematic diagram of the theoretical model of plasma sputtering corresponding to the present invention when there is no micro-nano composite structure on the surface of the material;
[0028] Figure 4 Schematic diagram of the theoretical model of plasma sputtering corresponding to the case where the material surface has a micro-nano composite structure in the present invention;
[0029] Figure 5 Schematic diagram of the test results of the deuterium and tritium ion retention resistance of the tungsten alloy divertor of each embodiment and comparative example of the present invention. DETAILED DESCRIPTION
[0030] The method of improving the resistance of tungsten alloy divertor to deuterium and tritium retention of the present invention is a pioneering invention. The present invention constructs and regulates a dual-scale micro-nano composite structure on the surface of tungsten alloy, so that the surface exhibits an "ion-repelling effect", thereby reducing the deuterium and tritium retention on the surface of tungsten alloy. When the micro-nano composite structure on the surface of tungsten alloy is subjected to continuous bombardment of high-temperature plasma deuterium and tritium, the micron-scale fluctuations caused by the micron-scale structure can change the incident angle and reflection direction of deuterium and tritium ions, thereby increasing the reflection coefficient; the nano-scale structure can increase the specific surface area, further improving the reflection coefficient and release effect of deuterium and tritium ions. The micron-scale structure and nano-scale structure on the surface of tungsten alloy influence each other and synergize to effectively reduce the clustering and enrichment of deuterium and tritium plasma on the surface of tungsten alloy, causing it to exhibit an "ion-repelling" effect, thereby reducing the deuterium and tritium ion retention on the surface of tungsten alloy.
[0031] This invention utilizes the reflection and release effects of micron- and nanoscale structures on deuterium and tritium ions. By regulating the ion-repelling effect on the composite structure's surface, the deuterium and tritium retention resistance of the tungsten alloy divertor can be improved. By establishing a theoretical model for plasma sputtering of composite micro- and nanostructures, the micro- and nanocomposite structures can be further optimized for ion-repelling and deuterium and tritium retention resistance. By varying cutting and ultrasonic vibration parameters, the morphology of the micro- and nanocomposite structures can be manipulated, further reducing the amount of deuterium and tritium retained on the tungsten alloy divertor surface and ensuring steady-state operation of nuclear fusion reactions under high-parameter, long-pulse conditions.
[0032] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0033] 1. Specific embodiments of the method for improving the resistance of tungsten alloy divertor to deuterium and tritium retention of the present invention are as follows:
[0034] Example 1
[0035] The method of improving the resistance of tungsten alloy divertor to deuterium and tritium retention in this embodiment specifically comprises the following steps: constructing a dual-scale micro-nano composite structure on the deuterium and tritium ion bombardment surface of the tungsten alloy divertor, wherein the dual-scale micro-nano composite structure comprises a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface, and utilizing the dual-scale micro-nano composite structure to change the incident angle and reflection direction of deuterium and tritium ions, thereby reducing the deuterium and tritium ion retention on the tungsten alloy surface; the dual-scale micro-nano composite structure constructed in this embodiment is as follows: Figure 1-2 shown. Figure 1 In the figure, 1 and 3 represent the micron-scale structure of the tungsten alloy surface, and 2 and 4 represent the nanoscale structure of the tungsten alloy surface.
[0036] This embodiment optimizes the dual-scale micro-nano composite structure by constructing a plasma sputtering theoretical model and combining it with molecular dynamics simulation. The specific method is as follows:
[0037] High-temperature deuterium and tritium ions emitted during nuclear fusion reactions enter the sheath through the sheath boundary. These incident deuterium and tritium ions continuously bombard the smooth surface or micro-nano composite structure of the tungsten alloy divertor. Some deuterium and tritium ions are reflected by the surface, while others accumulate and cluster on the smooth surface or micro-nano composite structure of the tungsten alloy divertor and become retained on the surface. These retained deuterium and tritium ions gradually penetrate into the interior of the tungsten alloy divertor material, degrading its thermodynamic properties.
[0038] When there is no micro-nano composite structure on the surface of the material, under the bombardment of high-temperature deuterium and tritium ions, the concentration calculation formula of deuterium and tritium ions on the smooth surface of tungsten alloy is:
[0039]
[0040] Where K0 is the surface recombination coefficient facing the plasma surface, J0_ is the surface recombination flux, J0 is the implanted H flux, R0 is the reflection coefficient, S0 is the smooth surface area of tungsten alloy, S S is the area of the sheath boundary, in this case, S0=S S , J S0 is the incident flux on the sample surface, J sheath is the incident flux at the sheath boundary.
[0041] When the surface of the material has a micro-nano composite structure, the surface area of the micro-nano structure surface is greater than the surface area of the smooth surface (S1>S0=S S ). Therefore, the incident flux on the microstructure surface is smaller than the incident flux on the sheath edge, that is:
[0042]
[0043] Among them, J 1_ is the surface recombination flux, J1 is the implantation flux, and J S1 is the surface incident flux, R1 is the reflection coefficient, and S1 is the total area of the tungsten alloy smooth surface and the micro-nanostructure surface.
[0044] The calculation formula for the concentration of deuterium and tritium ions on the surface of micro-nanostructures is:
[0045]
[0046] Where K0 is the surface recombination coefficient facing the plasma surface, J 1_ is the surface recombination flux, J1 is the implantation flux, R1 is the reflection coefficient, S1 is the total area of the smooth surface of the tungsten alloy and the surface of the micro-nanostructure, S S is the area of the sheath boundary, J sheath is the incident flux at the sheath boundary.
[0047] According to the above theoretical model, the retention of deuterium and tritium ions on the surface of tungsten alloy can be further reduced by regulating the morphology of the micro-nano composite structure on the surface of tungsten alloy. The post-processing programs SRIM (the Stopping and Range of lons in Maaer) and TMAP (Tritium Migration Analysis Program) of the simulation software LAMMPS were used to simulate and analyze the retention of deuterium and tritium ions on the optimized dual-scale micro-nano composite structure, and the micro-nano composite structure was further optimized. After optimization, the retention of deuterium and tritium on the surface of the tungsten alloy micro-nano structure was reduced from 1.2×10 19 D / m 2 Reduced to 2×10 18 D / m 2 .
[0048] When there is no micro-nano composite structure on the material surface, the corresponding plasma sputtering theoretical model is as follows Figure 3 As shown, 5 represents the high-temperature deuterium and tritium ions discharged from the nuclear fusion reaction, 6 represents the incident deuterium and tritium ions, 7 represents the deuterium and tritium ions reflected by the smooth surface of the tungsten alloy, 8 represents the smooth surface of the tungsten alloy, 9 represents the deuterium and tritium ions enriched and retained on the surface of the tungsten alloy, 10 represents the deuterium and tritium ions penetrating into the tungsten alloy material, and 11 represents the tungsten alloy divertor.
[0049] When there is a micro-nano composite structure on the surface of the material, the corresponding plasma sputtering theoretical model is as follows Figure 4 As shown, 5 represents the high-temperature deuterium and tritium ions discharged from the nuclear fusion reaction, 6 represents the incident deuterium and tritium ions, 7 represents the deuterium and tritium ions reflected by the tungsten alloy surface, 9 represents the deuterium and tritium ions enriched and retained on the tungsten alloy surface, 10 represents the deuterium and tritium ions penetrating into the tungsten alloy material, 11 represents the tungsten alloy divertor, and 12 represents the micro-nano composite structure surface of the tungsten alloy.
[0050] The specific embodiments of the tungsten alloy divertor of the present invention are as follows:
[0051] Example 2
[0052] The tungsten alloy divertor of this embodiment has a dual-scale micro-nano composite structure constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The structural schematic diagram of the dual-scale micro-nano composite structure of this embodiment is shown in FIG. Figure 1 As shown ( Figure 1 In the figure, 1 represents the micron-scale structure of the tungsten alloy surface, and 2 represents the nanoscale structure of the tungsten alloy surface). The micron-scale concave-convex surface is formed by multiple micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The micron-scale pits are elliptical pits with an indentation depth (the indentation depth refers to the vertical distance from the end of the pit on the substrate surface to the deepest part of the pit) of 15 μm and an opening width (the opening width refers to the maximum distance between two points on the contour line determined by the end of the pit on the substrate surface) of 25 μm. The distribution density of the elliptical pits is 1.6×10 3 Pieces / mm 2 The width of the nanoscale stripes is 5 nm, the distance between two adjacent nanoscale stripes is 7 nm, the height of the nanoscale stripes is 4 nm, and the distribution density of the nanoscale stripes is 1.9×10 10 Pieces / mm 2 ;
[0053] The processing method of the tungsten alloy divertor of this embodiment is as follows:
[0054] The tungsten alloy surface is cut using a natural diamond tool. During the cutting process, low-frequency vibration and ultrasonic elliptical vibration are applied to the natural diamond tool to achieve fast tool servo cutting and ultrasonic elliptical vibration cutting respectively.
[0055] In this embodiment, the cutting edge of the natural diamond tool is circular, the arc radius of the cutting edge is 1 mm, the arc profile waviness is 0.15 μm, the tool rake angle is 0°, and the relief angle is 15°;
[0056] The frequency of low-frequency vibration is 200 Hz, the direction of low-frequency vibration is parallel to the cutting depth direction, and the amplitude in the cutting depth direction is 10 μm;
[0057] The frequency of ultrasonic elliptical vibration is 45kHz, the amplitude in the cutting speed direction is 2μm, the amplitude in the cutting depth direction is 2μm, and the phase difference between the cutting speed direction and the cutting depth direction is 60°;
[0058] The cutting speed during cutting is 1 m / min, the cutting depth is 4 μm, and the feed rate is 8 μm / r.
[0059] In this embodiment, the motion accuracy of the ultra-precision machine tool used during processing is less than 15 nm in the axial direction, less than 15 nm in the radial direction, and a C-axis resolution of 0.026 arc seconds; alcohol is used as a coolant during processing.
[0060] Example 3
[0061] The tungsten alloy divertor of this embodiment has a dual-scale micro-nano composite structure constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The structural schematic diagram of the dual-scale micro-nano composite structure of this embodiment is shown in FIG. Figure 2 As shown ( Figure 2 In the figure, 3 represents the micron-scale structure of the tungsten alloy surface, and 4 represents the nanoscale structure of the tungsten alloy surface). The micron-scale concave-convex surface is formed by multiple micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The micron-scale pits are diamond-shaped pits with a recessed depth (the recessed depth refers to the vertical distance from the end of the pit on the substrate surface to the deepest part of the pit) of 12 μm and an opening width (the opening width refers to the maximum distance between two points on the contour line determined by the end of the pit on the substrate surface) of 20 μm. The distribution density of the diamond pits is 2.5×10 3 Pieces / mm 2 The width of the nanoscale stripes is 7 nm, the distance between two adjacent nanoscale stripes is 4 nm, the height of the nanoscale stripes is 5 nm, and the distribution density of the nanoscale stripes is 6.2×10 10 Pieces / mm 2 ;
[0062] The processing method of the tungsten alloy divertor of this embodiment is as follows:
[0063] The tungsten alloy surface is cut using a natural diamond tool. During the cutting process, low-frequency vibration and ultrasonic elliptical vibration are applied to the natural diamond tool to achieve fast tool servo cutting and ultrasonic elliptical vibration cutting respectively.
[0064] In this embodiment, the cutting edge of the natural diamond tool is circular, the cutting edge arc radius is 0.8 mm, the arc profile waviness is 0.1 μm, the tool rake angle is 2°, and the relief angle is 10°;
[0065] The frequency of the low-frequency vibration is 450 Hz, the direction of the low-frequency vibration is parallel to the cutting depth direction, and the amplitude in the cutting depth direction is 8 μm;
[0066] The frequency of ultrasonic elliptical vibration is 65kHz, the amplitude in the cutting speed direction is 1.5μm, the amplitude in the cutting depth direction is 1.5μm, and the phase difference between the cutting speed direction and the cutting depth direction is 90°;
[0067] The cutting speed during cutting is 1.5 m / min, the cutting depth is 6 μm, and the feed rate is 10 μm / r.
[0068] In this embodiment, the motion accuracy of the ultra-precision machine tool used during processing is less than 15 nm in the axial direction, less than 15 nm in the radial direction, and a C-axis resolution of 0.026 arc seconds; alcohol is used as a coolant during processing.
[0069] Example 4
[0070] The tungsten alloy divertor of this embodiment has a dual-scale micro-nano composite structure constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The micron-scale concave-convex surface is formed by multiple micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The micron-scale pits are circular pits with a recessed depth (the recessed depth refers to the vertical distance from the end of the pit located on the substrate surface to the deepest part of the pit) of 10 μm and an opening width (the opening width refers to the maximum distance between two points on the contour line determined by the end of the pit located on the substrate surface) of 16 μm. The distribution density of the circular pits is 3.9×10 3 Pieces / mm 2 The width of the nanoscale stripes is 6 nm, the distance between two adjacent nanoscale stripes is 6 nm, the height of the nanoscale stripes is 3 nm, and the distribution density of the nanoscale stripes is 2.75×10 10 Pieces / mm 2 ;
[0071] The processing method of the tungsten alloy divertor of this embodiment is as follows:
[0072] The tungsten alloy surface is cut using a natural diamond tool. During the cutting process, low-frequency vibration and ultrasonic elliptical vibration are applied to the natural diamond tool to achieve fast tool servo cutting and ultrasonic elliptical vibration cutting respectively.
[0073] In this embodiment, the natural diamond tool is a conical tool, which can effectively ensure the shape accuracy of the circular pit. The cutting edge arc radius is 0.55 mm, the arc profile waviness is 0.15 μm, the tool rake angle is 0°, and the clearance angle is 35°, which can effectively avoid interference and collision between the cutting edge clearance angle and the processed surface.
[0074] The frequency of the low-frequency vibration is 40 Hz, the direction of the low-frequency vibration is parallel to the cutting depth direction, and the amplitude in the cutting depth direction is 12 μm;
[0075] The frequency of ultrasonic elliptical vibration is 45kHz, the amplitude in the cutting speed direction is 2μm, the amplitude in the cutting depth direction is 2μm, and the phase difference between the cutting speed direction and the cutting depth direction is 60°;
[0076] The cutting speed during cutting is 16 m / min, the cutting depth is 10 μm, and the feed rate is 8 μm / r.
[0077] Comparative Example 1
[0078] The tungsten alloy divertor of this embodiment has a dual-scale micro-nano composite structure constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The micron-scale concave-convex surface is formed by multiple micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The micron-scale pits are circular pits with a recessed depth (the recessed depth refers to the vertical distance from the end of the pit located on the substrate surface to the deepest part of the pit) of 2 μm, an opening width (the opening width refers to the maximum distance between two points on the contour line determined by the end of the pit located on the substrate surface) of 4 μm, and a distribution density of 6×10 4 Pieces / mm 2 The width of the nanoscale stripes is 3 nm, the distance between two adjacent nanoscale stripes is 8 nm, the height of the nanoscale stripes is 2 nm, and the distribution density of the nanoscale stripes is 1.55×10 10 Pieces / mm 2 ;
[0079] The processing method of the tungsten alloy divertor of this comparative example is as follows:
[0080] The tungsten alloy surface is cut using a natural diamond tool. During the cutting process, low-frequency vibration and ultrasonic elliptical vibration are applied to the natural diamond tool to achieve fast tool servo cutting and ultrasonic elliptical vibration cutting respectively.
[0081] In this comparative example, the natural diamond tool is a cylindrical tool, the cutting edge shape is circular, the cutting edge arc radius is 1.5 mm, the arc profile waviness is 0.12 μm, the tool rake angle is -7°, and the relief angle is 15°;
[0082] The frequency of the low-frequency vibration is 10 Hz, the direction of the low-frequency vibration is parallel to the cutting depth direction, and the amplitude in the cutting depth direction is 3 μm;
[0083] The frequency of ultrasonic elliptical vibration is 15 kHz, the amplitude in the cutting speed direction is 1 μm, the amplitude in the cutting depth direction is 1 μm, and the phase difference between the cutting speed direction and the cutting depth direction is 15°;
[0084] The cutting speed during cutting is 30 m / min, the cutting depth is 4 μm, and the feed rate is 15 μm / r.
[0085] In this embodiment, the motion accuracy of the ultra-precision machine tool used during processing is less than 15 nm in the axial direction, less than 15 nm in the radial direction, and a C-axis resolution of 0.026 arc seconds; alcohol is used as a coolant during processing.
[0086] Comparative Example 2
[0087] The tungsten alloy divertor of this comparative example is different from the tungsten alloy divertor of Example 2 only in that the tungsten alloy divertor of this comparative example has no dual-scale micro-nano composite structure constructed on its surface, that is, it is a tungsten alloy divertor with a smooth surface.
[0088] Experimental example
[0089] In order to evaluate the anti-deuterium and tritium ion retention performance of the tungsten alloy divertors of various embodiments and comparative examples, the tungsten alloy divertors were subjected to continuous bombardment of deuterium and tritium in high-temperature plasma, and the retention of deuterium and tritium ions on the tungsten alloy surface was detected by thermal desorption spectrum (TDS) and nuclear reaction analysis (NRA) depth profile. The results are shown in Figure 2. Figure 5 shown. Figure 5 The smooth surface in the figure represents the tungsten alloy divertor processed in comparative example 2, the micro-nano structure represents the tungsten alloy divertor processed in comparative example 1, the optimized elliptical micro-nano structure represents the tungsten alloy divertor processed in embodiment 2, the optimized diamond-shaped micro-nano structure represents the tungsten alloy divertor processed in embodiment 3, and the optimized circular micro-nano structure represents the tungsten alloy divertor processed in embodiment 4.
Claims
1. A method for improving the resistance of tungsten alloy divertor to deuterium and tritium retention, characterized in that: A dual-scale micro-nano composite structure is constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanoscale stripes distributed on the micron-scale concave-convex surface. The dual-scale micro-nano composite structure is used to change the incident angle and reflection direction of the deuterium-tritium ions, thereby reducing the deuterium-tritium ion retention on the tungsten alloy surface.
2. The method for improving the resistance of tungsten alloy divertor to deuterium and tritium retention as claimed in claim 1, characterized in that: A theoretical model of plasma sputtering of composite micro-nano structures is established, and the dual-scale micro-nano composite structure is optimized by combining molecular dynamics simulation.
3. A tungsten alloy divertor, characterized in that: A dual-scale micro-nano composite structure is constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor. The dual-scale micro-nano composite structure includes a micron-scale concave-convex surface and nanometer-scale stripes distributed on the micron-scale concave-convex surface.
4. The tungsten alloy divertor according to claim 3, characterized in that: The micron-scale uneven surface is formed by multiple micron-scale pits constructed on the deuterium-tritium ion bombardment surface of the tungsten alloy divertor.
5. The tungsten alloy divertor according to claim 4, characterized in that: The micron-sized pits are circular pits, square pits, and elliptical pits.
6. The tungsten alloy divertor according to claim 4, characterized in that: The scale of micron-scale pits is 10 to 50 μm, and the scale of nanoscale stripes is 1 to 7 nm.
7. The tungsten alloy divertor according to claim 6, characterized in that: The depth of the micron-scale pits is 10 to 15 μm, and the opening width is 16 to 25 μm.
8. The tungsten alloy divertor according to claim 6 or 7, characterized in that: The density of micron-scale pits is 1.6×10 3 ~3.9×10 3 Pieces / mm 2 .
9. The tungsten alloy divertor according to claim 6, characterized in that: The width of the nanoscale stripes is 5 to 7 nm, the distance between two adjacent nanoscale stripes is 4 to 7 nm, and the height of the nanoscale stripes is 3 to 5 nm.
10. The tungsten alloy divertor according to claim 6 or 9, characterized in that: The density of nanoscale stripes is 1.9×10 10 ~6.2×10 10 Pieces / mm 2 .