Composite film sintered flat wire and preparation method thereof
By adding end-hydroxynitrile rubber graft-modified nanomontmorillonite and graphene oxide to the composite film sintered flat wire, the problem of insufficient adhesion performance between the polyimide film layer and the conductor flat wire is solved, and stretching is improved Adhesion and mechanical properties significantly improve the stability and adhesion of the film layer.
Patent Information
- Application Number
- CN202410384135.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-01
- Publication Date
- 2024-11-22
AI Technical Summary
The adhesion performance between the polyimide film layer of the sintered flat wire of the existing composite film and the flat wire of the conductor, especially the tensile adhesion performance, and the problem of insufficient mechanical properties.
Using nanomontmorillonite and graphene oxide grafted with end-hydroxynitrile rubber to the polyimide film layer, the adhesion performance is improved through layered microstructure and anchoring sites, and through end-hydroxynitrile rubber Energy absorption reduces the damage to the film by stress, and combines with polyperfluoroethylene acrylic adhesive layer to enhance adhesion.
The tensile adhesion performance between the polyimide film layer and the flat conductor wire is significantly improved, the film separation and deformation problems are reduced, the toughness and adhesion of the material are enhanced, and the protection effect of different usage environments is met.
Smart Images

Figure BDA0004770070830000071 
Figure BDA0004770070830000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, and in particular to a composite film sintered flat wire and a preparation method thereof. Background Art
[0002] Composite film sintered flat wire is generally prepared by laying at least one insulating layer on the surface of the copper-aluminum flat wire. Common insulating layers include glass film layers and polyimide film layers. The laid film layer needs to be cured by high-temperature sintering.
[0003] In some fields with specific use environments, protective films of different materials are also set on the surface of composite film sintered flat wire to achieve different protection effects. However, the adhesion between polyimide film and metal wire core is not good. F-46 has better adhesion effect and mechanical properties than polyimide. Therefore, most of the improved technical solutions adopted in the prior art are to set F-46 glue layer on the inner layer of polyimide film. Although this solution can improve the adhesion performance, there is still room for improvement in the adhesion performance, especially the tensile adhesion performance. Summary of the invention
[0004] In view of this, the present invention proposes a composite film sintered flat wire and a preparation method thereof, aiming to improve the film adhesion performance by improving the composite film material of the sintered flat wire.
[0005] The technical solution of the present invention is implemented as follows: the present invention provides a composite film sintered flat wire, which includes a conductor flat wire and a polyimide film layer arranged in sequence from inside to outside, wherein the raw materials of the polyimide film layer include polyimide, polyperfluoroethylene propylene and functional components, and the functional components include nano-montmorillonite grafted and modified by terminal hydroxyl nitrile rubber.
[0006] The layered microstructure of nano-montmorillonite can provide good adhesion performance, provide anchoring sites for the polyimide film layer to combine with the surface of the conductor flat wire, and improve the adhesion performance of the polyimide film layer. At the same time, end-hydroxy nitrile rubber is used as a structure similar to an anchoring rope to provide more active connection sites for the combination between the nano-montmorillonite and the polyimide film layer, avoiding the interface separation problem caused by different substrates. Moreover, when the polyimide film layer is subjected to large external stress, the end-hydroxy nitrile rubber can absorb energy through its own long chain, avoiding stress damage to the structure of the polyimide film layer, such as membrane separation.
[0007] In some embodiments, the preparation method of the nano-montmorillonite modified by grafting of terminal hydroxyl nitrile rubber includes: dissolving the terminal hydroxyl nitrile rubber in methanol to obtain a modified solution, adding the nano-montmorillonite to the modified solution, stirring and heating the solution, filtering and drying to obtain the modified nano-montmorillonite.
[0008] In the above embodiment, the modified solution is summarized, the mass concentration of the terminal hydroxyl nitrile rubber is 10%, the added amount of nano-montmorillonite is not more than the mass of the terminal hydroxyl nitrile rubber, the heating temperature of the above heating treatment is preferably 40-50°C, and the heating time is 30-60min.
[0009] In some embodiments, in the raw materials of the polyimide film layer, the mass ratio of polyimide: polyperfluoroethylene propylene is (3-5):1, and the mass ratio of modified nano-montmorillonite: polyperfluoroethylene propylene is (0.01-0.03):1.
[0010] In some embodiments, the functional component further comprises graphene oxide, and the average particle size of the graphene oxide is 1-10 μm.
[0011] In the above embodiments, graphene oxide not only has a good toughening effect, but also has a certain microscopic deformation ability. When the polyimide film layer is deformed by external force, it can absorb energy through deformation as much as possible, while also enhancing the toughness of the material and reducing the probability of membrane separation problems.
[0012] In some embodiments, the mass ratio of graphene oxide to polyperfluoroethylene propylene is (0.01-0.02):1.
[0013] In a second aspect, the present invention provides a method for preparing a composite thin film sintered flat wire, comprising the following steps:
[0014] Step 1: performing surface polishing on the conductor flat wire;
[0015] Step 2: Add the functional component to the molten polyperfluoroethylene propylene liquid under an inert atmosphere, stir evenly, introduce the polished conductor flat wire into the molten polyperfluoroethylene propylene liquid, make a polyperfluoroethylene propylene layer adhere to the surface of the conductor flat wire, and then anneal;
[0016] Step 3: Wrap the surface of the annealed flat wire with a polyimide film, and perform high-frequency sintering and welding on the wrapped flat wire to obtain a composite film sintered flat wire.
[0017] In some embodiments, in step 2, the annealing temperature is 450° C. and the annealing time is 20 s.
[0018] In some embodiments, in step three, the high-frequency sintering temperature is 300° C., and the pulling speed of the flat wire during sintering is 10 m / min.
[0019] In some embodiments, when the functional component includes graphene oxide, before adding the functional component in step 2, the graphene oxide and the nano-montmorillonite modified by grafting of hydroxy-terminated nitrile rubber are pre-mixed.
[0020] In some embodiments, the method of premixing graphene oxide with nano-montmorillonite modified by grafting of terminal hydroxyl-butadiene nitrile rubber comprises: while mixing and stirring graphene oxide with nano-montmorillonite modified by grafting of terminal hydroxyl-butadiene nitrile rubber, performing ultrasonic treatment.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The present invention aims to improve the adhesion effect between the polyimide film layer and the conductor flat wire, specifically the adhesion performance between the polyimide film layer and the conductor flat wire after tensile deformation. Therefore, a polyperfluoroethylene propylene adhesive layer is arranged between the polyimide film and the conductor flat wire, and at the same time, at least nano-montmorillonite grafted modified with terminal hydroxyl nitrile rubber is added to the adhesive layer. After adding this component, the polyimide film layer has good adhesion during the tensile deformation process, wherein the grafted nano-montmorillonite can provide a strong adhesion site with the conductor flat wire and form an elastic anchor with the adhesive layer, and the grafted terminal hydroxyl nitrile rubber also has good adhesion performance. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the embodiments of the present invention belong. If the definitions set forth in this section are contrary to or otherwise inconsistent with the definitions set forth in the patents, patent applications, published patent applications, and other publications incorporated herein by reference, the definitions listed in this section take precedence over the definitions incorporated herein by reference.
[0025] Unless otherwise specified, the methods used in the following examples are all conventional methods. Unless otherwise specified, the materials, reagents and instruments used are all conventional materials, reagents and instruments in the art, and can be obtained by those skilled in the art through commercial channels.
[0026] When an amount, concentration or other value or parameter is expressed as a range, a preferred range or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described herein, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range. In the present specification and claims, range definitions can be combined and / or interchanged, and if not otherwise stated, these ranges include all subranges contained therein.
[0027] The conductor flat wires used in the following examples and comparative examples are all 3.35 mm*9 mm flat copper wires.
[0028] Preparation of modified nano-montmorillonite:
[0029] First, 1 L of methanol solution of 10% hydroxy-terminated nitrile rubber was prepared, then heated to 45° C., 50 g of nano-montmorillonite was added to the solution, stirred for 60 minutes, filtered, dried at 90° C. to constant weight, and crushed to an average particle size of 200 nm.
[0030] First, the flat copper wire is surface polished;
[0031] Then, in an inert gas atmosphere, 1 kg of polyperfluoroethylene propylene was heated to 350°C, and 10 g of nano-montmorillonite modified with terminal hydroxyl nitrile rubber was added and stirred evenly. Then, the polished flat copper wire was introduced into the melt of polyperfluoroethylene propylene to make a uniform polyperfluoroethylene propylene layer adhere to the surface of the flat copper wire, and then annealed at 450°C for 20 seconds.
[0032] The surface of the annealed flat copper wire is wrapped with a polyimide film. After wrapping, the surface of the flat copper wire is evenly covered with 3kg of polyimide film. After wrapping, the flat wire is introduced into a high-frequency furnace for sintering. The high-frequency sintering temperature is 300°C and the flat wire pulling speed is 10m / min. After sintering, a composite film sintered flat wire is obtained.
[0033] Example 2
[0034] On the basis of Example 1, keeping other conditions unchanged, the surface of the rectangular copper wire was evenly covered with 5 kg of polyimide film after wrapping.
[0035] Example 3
[0036] On the basis of Example 1, keeping other conditions unchanged, the amount of the added nano-montmorillonite modified by the hydroxy-terminated nitrile rubber was 30 g.
[0037] Example 4
[0038] On the basis of Example 1, keeping other conditions unchanged, when adding the nano-montmorillonite modified by the terminal hydroxyl nitrile rubber, 10g of graphene oxide with an average particle size of 1 μm was also added.
[0039] Example 5
[0040] On the basis of Example 1, keeping other conditions unchanged, when adding the nano-montmorillonite modified by the terminal hydroxyl nitrile rubber, 20g of graphene oxide with an average particle size of 1 μm was also added.
[0041] Example 6
[0042] On the basis of Example 1, keeping other conditions unchanged, when adding the nano-montmorillonite modified by the terminal hydroxyl nitrile rubber, 10g of graphene oxide with an average particle size of 10μm was also added.
[0043] Example 7
[0044] On the basis of Example 1, keeping other conditions unchanged, before adding the terminal hydroxyl nitrile rubber modified nano-montmorillonite, the method further includes mixing the terminal hydroxyl nitrile rubber modified nano-montmorillonite with 10 g of graphene oxide with an average particle size of 10 μm, and performing ultrasonic treatment.
[0045] Comparative Example 1
[0046] On the basis of Example 1, the modified nano-montmorillonite was replaced with polyperfluoroethylene propylene of the same mass.
[0047] Comparative Example 2
[0048] On the basis of Example 1, the modified nano-montmorillonite was replaced with nano-montmorillonite of the same mass.
[0049] Comparative Example 3
[0050] On the basis of Example 1, the modified nano-montmorillonite was replaced with 8 g of nano-montmorillonite, and 2 g of terminal hydroxyl nitrile rubber was added.
[0051] In the above embodiments and comparative examples, the lengths of the prepared composite film sintered flat wires are the same. In order to verify the adhesion performance of the polyimide film layer on the surface of the sintered flat wire, 300 mm long sintered flat wires were taken respectively, and circular cutting was performed at the middle position to cut to the flat copper wire layer, and then stretched by 25% according to an effective stretching length of 200 mm. The length of the film layer that lost adhesion from the incision was counted, and the results were obtained as shown in the following table:
[0052]
[0053] In some other comparative examples, for example, when other conditions were kept unchanged on the basis of Example 1 and 40 g of modified nano-montmorillonite was added, the attached film layer after stretching had the problem of intermediate separation, so the length of the lost attached film layer could not be accurately counted, but the overall separation length was at least 2 mm, and in other comparative examples, when other conditions were kept unchanged on the basis of Example 4 and too much graphene oxide was added, the insulation performance of the film layer could not meet the requirements. In other comparative examples, when other conditions were kept unchanged on the basis of Example 4 and the size of the added graphene oxide reached 20 μm, the insulation performance also failed to meet the requirements.
[0054] At the same time, when the composite film sintered flat wires prepared in the above embodiment and the comparative example were subjected to torsion tests, the debonding sizes of various parts were counted. The torsion test was conducted according to the requirements of GB / T 23310-2009, and the results were shown in the following table:
[0055]
[0056] It is not difficult to see from the above data that the sintered flat wire of the present invention not only performs excellently in the tensile membrane separation effect, but also significantly improves the membrane separation problem after twisting.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite film sintered flat wire, characterized in that: The composite film sintered flat wire comprises a conductor flat wire and a polyimide film layer which are arranged in sequence from inside to outside, wherein the raw materials of the polyimide film layer comprise polyimide, polyperfluoroethylene propylene and functional components, and the functional components comprise nano-montmorillonite which is grafted and modified by terminal hydroxyl nitrile rubber.
2. The composite film sintered flat wire according to claim 1, characterized in that: The preparation method of the nano-montmorillonite grafted and modified by terminal hydroxyl-butadiene nitrile rubber comprises: dissolving the terminal hydroxyl-butadiene nitrile rubber in methanol to obtain a modified solution, adding the nano-montmorillonite into the modified solution, stirring and heating the solution, filtering and drying the solution to obtain the modified nano-montmorillonite.
3. The composite film sintered flat wire according to claim 1, characterized in that: In the raw materials of the polyimide film layer, the mass ratio of polyimide to polyperfluoroethylene propylene is (3-5):1, and the mass ratio of modified nano-montmorillonite to polyperfluoroethylene propylene is (0.01-0.03):
1.
4. The composite film sintered flat wire according to claim 1, characterized in that: The functional component also includes graphene oxide, and the average particle size of the graphene oxide is 1-10 μm.
5. The composite film sintered flat wire according to claim 4, characterized in that: The mass ratio of graphene oxide to polyperfluoroethylene propylene is (0.01-0.02):
1.
6. The method for preparing a composite thin film sintered flat wire according to any one of claims 1 to 5, characterized in that: The steps include: Step 1: performing surface polishing on the conductor flat wire; Step 2: Add the functional component to the molten polyperfluoroethylene propylene liquid under an inert atmosphere, stir evenly, introduce the polished conductor flat wire into the molten polyperfluoroethylene propylene liquid, make a polyperfluoroethylene propylene layer adhere to the surface of the conductor flat wire, and then anneal; Step 3: Wrap the surface of the annealed flat wire with a polyimide film, and perform high-frequency sintering and welding on the wrapped flat wire to obtain a composite film sintered flat wire.
7. The method for preparing a composite thin film sintered flat wire according to claim 6, characterized in that: In step 2, the annealing temperature is 450° C. and the annealing time is 20 seconds.
8. The method for preparing a composite thin film sintered flat wire according to claim 6, characterized in that: In step three, the high-frequency sintering temperature is 300° C., and the pulling speed of the flat wire during sintering is 10 m / min.