Self-supporting aluminum alloy cable for wind turbine generator and preparation process
By designing self-supporting aluminum alloy cables in the wind turbine, integrating steel stranded wire cores, aluminum alloy wire cores and fiber optic units, combined with high-efficiency aluminum alloy melt processing technology, the high cost and monitoring problems of wind turbine wire construction are solved, and the problem of wind turbine wire construction is realized. Low-carbon, environmentally friendly, efficient power and information transmission to ensure line safety and construction efficiency.
Patent Information
- Application Number
- CN202411257154.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
The overhead insulated wires of existing wind turbines have high costs, land waste and inability to monitor the line health during construction and use. The traditional aluminum alloy wire manufacturing method needs to be optimized to reduce costs and improve efficiency.
Using self-supported aluminum alloy cable design, integrated steel stranded wire core, aluminum alloy wire core and fiber optic unit, prepared by high-purity aluminum water and aluminum ingot batching, refining, degassing, rolling and drawing processes, combined with electromagnetic stirring and Double-stage foam ceramic filtration forms a high-efficiency, low-energy aluminum alloy wire core, and improves the performance of the cable through extrusion process and polyethylene sheath layer.
The steel stranded wire core load-bearing tension, optical fibers are used for communication and sensing, and the conductors are used for power transmission, reducing construction costs, improving construction efficiency, saving energy, improving the purity and conductivity of aluminum alloy cables, ensuring line safety monitoring and Low-carbon and environmentally friendly production.
Smart Images

Figure CN119008111A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of cables, and in particular to a self-supporting aluminum alloy cable for a wind turbine generator set and a preparation process thereof. Background Art
[0002] The electricity generated by wind turbines is transmitted to the power grid through cables. Overhead insulated wires are increasingly used in distribution networks. In recent years, the utilization rate of overhead insulated wires in power grid transformation has reached more than 70%. Traditional overhead insulated wires require the re-establishment of towers on the transmission lines, which is costly in terms of construction and labor, and causes waste of land along the lines. In addition, overhead insulated wires can only be used for power transmission and do not have communication and sensing functions.
[0003] For example: CN117410025A discloses a self-supporting optical fiber composite bundled overhead insulated cable, including a ground wire core assembly and an optical cable core assembly. The ground wire core assembly includes a high-tensile carbon fiber element, a conductor, a first insulating layer and a second insulating layer from the inside to the outside; the optical cable core assembly includes an optical fiber ribbon, a sleeve filler, a loose sleeve, a high-tensile carbon fiber element, an optical fiber sheath and a second insulating layer from the inside to the outside, and the high-tensile carbon fiber element is arranged in the optical fiber sheath. Among them, there is no steel stranded wire as a sling, and new overhead poles are required for cable laying, which is expensive; the cable is too long, and a newly customized pole is required for cable laying; the optical fiber does not directly contact the aluminum conductor, resulting in the inability to directly measure parameters such as the temperature during the operation of the conductor, and the inability to monitor the health and current carrying capacity of the cable.
[0004] CN108754248A discloses an aluminum alloy conductor for overhead stranded wire and a manufacturing method thereof, wherein the manufacturing method comprises the following steps: smelting and preparing aluminum alloy liquid, blowing refining in a furnace, online grain refinement, online degassing filtration, high-energy ultrasonic stirring, constant temperature continuous casting and rolling, online quenching, torque-free drawing and artificial aging. This solution requires the addition of lanthanum-cerium mixed rare earth to be optimized, which increases the cost of raw materials; there is no optical fiber for communication and line health monitoring. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a self-supporting aluminum alloy cable for wind turbines and a preparation process, which integrates optical fiber and transmission wire and can sense line safety; its preparation process meets low-carbon and environmental protection requirements, has low energy consumption and high preparation efficiency.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In the first aspect, an embodiment of the present invention provides a self-supporting aluminum alloy cable for a wind turbine, comprising a steel strand core, an aluminum alloy core and an outer sheath, wherein the steel strand core is a self-supporting steel strand containing optical fiber; a single-core or two-core or more aluminum alloy cores are arranged in parallel with the steel strand core, and the outer sheath is wrapped around the outside of the steel strand core and the aluminum alloy core; the gaps between the aluminum alloy cores are filled with optical fiber units and filling ropes.
[0008] As a further implementation, the aluminum alloy wire core includes a conductor, and a conductor shielding layer, an insulating layer and an insulating shielding layer are sequentially arranged on the outside of the conductor.
[0009] As a further implementation, the stranded steel wire core comprises a central tube, and multiple layers of steel wires are evenly twisted on the outer side of the central tube; an optical fiber is arranged in the central tube, and the central tube is filled with hydrogen absorbing fiber paste.
[0010] In a second aspect, an embodiment of the present invention further provides a process for preparing a self-supporting aluminum alloy cable for a wind turbine generator system, comprising:
[0011] The aluminum alloy melt is formed by using high-purity aluminum water and aluminum ingots through batching, mixing and homogenization, degassing and deslagging, and static processing;
[0012] The aluminum alloy melt is used to prepare an aluminum rod with a set diameter through continuous casting and rolling processes, and the aluminum rod is drawn to form a single wire with a set diameter range; a plurality of single wires are twisted into a conductor;
[0013] The conductor is wrapped with a conductor shielding layer, an insulating layer and an insulating shielding layer in sequence, and then twisted with the optical fiber unit and the filling rope to form an aluminum alloy wire core;
[0014] The aluminum alloy core and the steel strand core are arranged in parallel, and a polyethylene sheath layer is extruded on the outer layer through an extrusion process.
[0015] As a further implementation method, molten aluminum is poured into a melting furnace, and cold aluminum ingots are added for batching;
[0016] The composition requirements of the aluminum melt after batching are as follows: Si content within 0.1%, Fe content within 0.15%, Fe to Si content ratio of 1.3-1.8, copper content within 0.001%, Mg content within 0.01%, Zn content within 0.02%, V content within 0.02%, Ti content within 0.02%, other single component content within 0.015%, the total content of the components within 0.3%.
[0017] As a further implementation method, after the cold aluminum ingot is added, the aluminum melt in the furnace is stirred by electromagnetic stirring at the bottom of the melting furnace; after the cold material is completely melted, the aluminum melt is refined by the aluminum melt refining equipment in the furnace, and the refining agent is injected into the aluminum melt through the pulse gas of N2 or Ar, the pulse control time is 80 to 200ms, and the bubbles are broken by the graphite rotor, so that the aluminum melt in the furnace and the refining agent gas sprayed by the graphite rotor are evenly mixed.
[0018] As a further implementation method, after refining in the furnace, the molten metal that has been deslagging is sent to an online rotor degassing device for secondary refining and degassing; after secondary refining and degassing, the melt is filtered and deslagging is performed, wherein the filtering device uses a two-stage foam ceramic filter plate to perform double filtration on the aluminum melt.
[0019] As a further implementation method, after two online degassing and slag removal inside and outside the furnace, the aluminum melt is left to stand, cooled and solidified to form aluminum bars; the aluminum bars are first rough-rolled by a roller mill for 1-2 passes, then extended by 3-8 passes, and then rolled before the finished product for 9-12 passes, and finally rolled into finished aluminum rods by 3 passes.
[0020] As a further implementation method, multi-core insulated sheathed aluminum alloy conductors are twisted into cables, and during the twisting process, ETFE sheathed optical fiber units and filling rope materials are used to fill the twisted gaps, and finally a wrapping tape is used to wrap the gaps to prepare an aluminum alloy wire core with optical fiber.
[0021] As a further implementation method, acrylic resin is dipped on the outside of the optical fiber and cured by ultraviolet light to form an optical fiber buffer layer; a flexible nylon material is used to extrude a tight sleeve layer on the outside of the optical fiber to armor and protect the optical fiber, thereby preparing a tight sleeve optical fiber;
[0022] Aramid material is used to weave a tensile layer outside the tight-buffered optical fiber, and ETFE fluoroplastic is used to extrude a sheath outside the tensile layer.
[0023] The beneficial effects of the present invention are as follows:
[0024] (1) The steel stranded wire core in the self-supporting overhead insulated aluminum alloy cable of the present invention is used to bear tension, and the optical fiber is used for line communication and sensing. At the same time, the optical fiber can realize real-time health monitoring of the safety of the overhead line. The conductor is used to transmit electric energy, integrating optical fiber and power transmission wire into one. The steel core stranded wire is used as the bearing wire to improve the construction efficiency of the overhead insulated aluminum alloy cable, save construction costs, and can be completed in one construction, saving labor and improving construction speed.
[0025] (2) The present invention uses molten aluminum to directly cast aluminum rods, which saves energy, facilitates the composition control of aluminum wire, and realizes low-carbon and environmentally friendly production; an appropriate amount of aluminum ingots are added to molten aluminum, which reduces the excessively high temperature of the aluminum liquid and also has a better effect on grain refinement during the casting process.
[0026] (3) The present invention uses steel strands for tensile reinforcement, and the conductor strength does not need to be too high. The aluminum alloy composition avoids the introduction of a large amount of magnesium and silicon, which in turn leads to a decrease in conductivity. The aluminum wire has a low magnesium and silicon content, and the conductivity can be greater than 60%, thereby reducing line losses.
[0027] (4) The present invention adopts a furnace refining process and combines electromagnetic stirring to degas and deslag the aluminum melt in the furnace. The combined process of "gas + refining agent" has better degassing and deslaging effects and lower energy consumption; it adopts secondary online rotor degassing and deslaging to adsorb H2 and oxidized impurities in the aluminum melt through tiny bubbles to bring out the aluminum melt, making the degassing and deslaging effects more thorough and improving the purity of the melt; it adopts a two-stage foam ceramic filter plate device to perform double filtration on the aluminum melt, which has better filtering effects and higher purity of the aluminum melt.
[0028] (5) The present invention adopts a flat-vertical twin-roller rolling mill, which has a larger rolling reduction during rough rolling and a higher rolling accuracy during fine rolling. It compacts and welds the defects such as shrinkage cavities, looseness, voids and pores inside the aluminum strip, making the structure denser, improving the uniformity of the structure, and improving the strength and toughness of the later aluminum wire. The flat-vertical twin-roller rolling mill has lower wear on the rolls, and is more convenient to disassemble during roll maintenance, making the maintenance of the mill equipment more convenient and saving labor.
[0029] (6) The present invention configures different drawing processes according to the outer diameters of different aluminum wires, and the drawing pass configuration is more scientific and reasonable, and the aluminum wire drawing process is more energy-saving and efficient; high-conductivity aluminum rods are used to draw aluminum wires, and the product has lower resistance, smaller line loss, and is low-carbon and environmentally friendly; high-strength steel wire is used, which has higher tensile strength, and an optical fiber stainless steel tube is used in the center, which realizes the transmission of optical information and can also monitor the healthy operation status of the cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0031] Figure 1 is a schematic diagram of the structure of a self-supporting overhead insulated aluminum alloy cable according to one or more embodiments of the present invention;
[0032] Figure 2 is a schematic diagram of the structure of a steel strand core according to one or more embodiments of the present invention;
[0033] Figure 3 is a schematic diagram of an aluminum alloy wire core structure according to one or more embodiments of the present invention;
[0034] Figure 4is a schematic diagram of the structure of an optical fiber unit according to one or more embodiments of the present invention;
[0035] Figure 5 is a process flow diagram according to one or more embodiments of the present invention.
[0036] Among them, 1. Steel stranded wire core, 2. Aluminum alloy wire core, 3. Optical fiber unit, 4. Outer sheath;
[0037] 11. Central tube, 12. Optical fiber, 13. Steel wire; 21. Conductor, 22. Conductor shielding layer, 23. Insulating layer, 24. Insulating shielding layer. DETAILED DESCRIPTION
[0038] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0039] Embodiment 1:
[0040] This embodiment provides a self-supporting aluminum alloy cable for a wind turbine generator system. Figure 1 As shown, it includes a steel strand core 1, an aluminum alloy core 2 and an outer sheath 4, wherein the steel strand core 1 is a self-supporting steel strand containing an optical fiber 12, and the steel strand core 1 and the aluminum alloy core 2 are connected by a sling.
[0041] A single-core or two-core or more aluminum alloy wire core 1 and a steel stranded wire core 2 are arranged in parallel, and the aluminum alloy wire core 1 and the steel stranded wire core 2 are wrapped with an outer sheath 4 on the outside, and the outer sheath 4 is a polyethylene sheath layer extruded by an extruder.
[0042] The gaps between the stranded wire cores 2 are filled with optical fiber units 3 and filling ropes to ensure better roundness of the appearance and make the outer diameter of the cable more uniform. The central gaps between the stranded wire cores 2 are filled with optical fiber units 3 to facilitate the testing of the temperature and current carrying capacity of the conductor. Figure 4 As shown, the optical fiber unit 3 has an ETFE sheath.
[0043] like Figure 2 As shown, the stranded steel wire core 1 comprises a central tube 11, and multiple layers of steel wires 13 are evenly twisted outside the central tube 11; the central tube 11 is a seamless steel tube, an optical fiber 12 is arranged inside the central tube 11, and the central tube 11 is filled with hydrogen absorbing fiber paste.
[0044] like Figure 3As shown, the aluminum alloy wire core 2 includes a conductor 21, and a conductor 21 shielding layer 22, an insulating layer 23 and an insulating shielding layer 24 are sequentially arranged on the outside of the conductor 21, wherein the conductor 21 is prepared from high-purity aluminum liquid and aluminum ingots, and then refined, degassed, rolled, drawn and twisted. The conductor 21 shielding layer 22 is a semi-conductive water-resistant tape, the insulating layer 23 is a polyethylene insulating layer, and the insulating shielding layer 24 is an aluminum alloy tape layer.
[0045] The dimensions of the aluminum alloy core 2 and the steel strand core 1 are set according to actual requirements, for example: the outer diameter of the steel strand core 1 is 14.4mm, the size of the central tube 11 is Φ1.2mm, the optical fiber 12 is a 2-core G657 bending-resistant optical fiber, and the outer layer is evenly twisted with 3 layers of Φ1.2mm, high-strength steel wire 13 with a tensile strength of 2100Mpa, a total of 36 wires, and a tensile force of 85KN.
[0046] The total outer diameter of the aluminum alloy cable is 46mm, and it is formed by twisting three aluminum alloy wire cores 2 with an outer diameter of 18.2. The outer diameter of the single wire of the conductor 21 of a single aluminum alloy cable is 3mm, and it adopts a 1+6+12 structure, with a total of 19. The gap between the cores of the three single cables is filled with a 4-core optical fiber unit 3, of which one core is in the center and is in close contact with the three cables, and the remaining three core optical fibers are evenly distributed.
[0047] Optical fiber unit 3 uses G657 bending-resistant optical fiber, the thickness of the optical fiber outer acrylic resin is 0.03mm, the cold-resistant flexible nylon tight jacket layer is about 0.3mm thick, the outer diameter is Φ0.9mmm, the outer diameter of the braided layer is Φ1.2mmm, and the outer diameter of the ETFE fluoroplastic is Φ1.8mmm.
[0048] The cable of this embodiment has the characteristics of light weight, resistance to large tensile force, smooth and soft appearance. The steel strand core 1 is used to bear the tensile force, the optical fiber is used for line communication and sensing, the conductor is used to transmit electrical energy, and the optical fiber can realize real-time health monitoring of the safety of overhead lines.
[0049] Embodiment 2:
[0050] The present embodiment provides a preparation process for a self-supporting aluminum alloy cable for a wind turbine, wherein high-purity aluminum liquid and aluminum ingots are subjected to batching, mixing and homogenization, degassing and deslagging, and standing processes to form an aluminum alloy melt; the aluminum alloy melt is subjected to a continuous casting and rolling process to prepare an aluminum rod of a set diameter, and the aluminum rod is drawn to form a single wire of a set diameter range; a plurality of single wires are twisted into a conductor; after the outer side of the conductor is wrapped with a conductor shielding layer, an insulating layer and an insulating shielding layer in sequence, it is twisted with an optical fiber unit and a filling rope to form an aluminum alloy wire core; the aluminum alloy wire core and the steel stranded wire core are arranged in parallel, and a polyethylene sheath layer is extruded on the outer layer through an extrusion process.
[0051] Specifically, Figure 5 As shown, the following steps are included:
[0052] Aluminum alloy conductors use high-purity aluminum water and aluminum ingots, with an aluminum content of more than 99.7% (mass fraction). The aluminum water is poured into the melting furnace (the temperature of the aluminum water is 750℃-800℃) through the aluminum water transfer bag, and cold aluminum ingots are added for batching (accounting for 10-20% of the total amount) to improve the grain refinement of the aluminum rod. The aluminum content of the aluminum ingot is not less than 99.7% (mass fraction). The composition requirements of the aluminum melt after the batching in the furnace are: Si content within 0.1%, Fe content within 0.15%, Fe to Si content ratio of 1.3-1.8, copper content within 0.001%, Mg content within 0.01%, Zn content within 0.02%, V content within 0.02%, Ti content within 0.02%, other single component content within 0.015%, and the total content of components within 0.3%.
[0053] During the batching process, after adding the cold aluminum ingot, the aluminum melt in the furnace is stirred by the electromagnetic stirring at the bottom of the melting furnace. The stirring time is determined according to the weight of the aluminum melt in the furnace. The electromagnetic stirring time for each ton of aluminum is within 1 minute, and the total stirring time does not exceed 30 minutes. The temperature of the aluminum melt in the furnace is appropriately controlled at 700℃-750℃. After the cold material is completely melted, the aluminum melt is refined by the aluminum liquid refining equipment in the furnace. The refining agent is injected into the aluminum melt through the pulse gas of N2 or Ar. The pulse control time is 80-200ms, and the bubbles are broken by the graphite rotor, so that the aluminum melt in the furnace and the refining agent gas ejected by the graphite rotor are evenly mixed, increasing the contact area and contact time between the bubbles and the aluminum alloy liquid. The melt is dehydrogenated, deslag and other impurities are removed through the combined process of "gas + refining agent"; the refining time in the furnace is controlled at 60S-90S per ton of aluminum.
[0054] After refining in the furnace, the molten metal flows out of the melting furnace and enters the online rotor degassing device after slagging treatment. The silicon carbide rotor breaks up N2 or Ar to form a large number of dispersed bubbles that enter the aluminum melt. After the collision, capture, surface adsorption, and partial pressure of the dispersed bubbles, the hydrogen and oxide slag in the aluminum melt are brought out of the aluminum liquid surface to form slag during the gas floating process, completing the online secondary refining and degassing of the melt. After the secondary refining and degassing, the melt is filtered and deslagging. The filtering device uses a two-stage foam ceramic filter plate (the hole size of the filter plate is 20-60ppi) to double filter the aluminum melt. It should be preheated to above 750℃ before filtering.
[0055] After two online degassing and deslagging processes inside and outside the furnace, the hydrogen content of the aluminum melt is ≤0.10ml / 100gAl, and the slag content PoDFA is <0.1mm 2 / kg. Then the aluminum melt is left to stand for 20-30 minutes, and the temperature of the aluminum melt is controlled at 680℃-720℃. It is then poured into the crystallization wheel through a pouring nozzle for rapid cooling and solidification to form a continuous length of trapezoidal aluminum bars with a cross-sectional area of 3400mm. 2 about.
[0056] The aluminum strip enters the flat-vertical roller mill for 15 passes, and first passes through the two-roller rolling mill for 1-2 passes for rough rolling with a large reduction amount to open the aluminum strip, compress the cross-section, and increase the length of the aluminum strip. Then it undergoes 3-8 passes of extension rolling to reduce the cross-section of the aluminum strip. It undergoes 9-12 passes of pre-finished rolling again, and the shape and size of the aluminum strip are closer to the finished product. The final 3 passes of rolling make it a finished product, a round aluminum rod with a size of Φ9.5mm, and the electrical conductivity of the round aluminum rod is greater than 63% IACS.
[0057] The finished Φ9.5mm aluminum rod is drawn by an aluminum wire drawing machine. The single wire size is Φ1.6mm-Φ4.5mm. Among them, the aluminum wire of Φ3.0mm-Φ4.5mm adopts 7-drawing die. The specific die size is shown in Table 1:
[0058] Table 1 Dimensions of 7-pass wire drawing die
[0059] Aluminum rod First Course Second The Third Way The Fourth Way The Fifth Way The Sixth Way The Seventh 9.50mm 8.50mm 7.24mm 6.12mm 5.20mm 4.43mm 3.82mm 3.0mm
[0060] The finished Φ9.5mm aluminum rod is drawn into Φ1.6mm-Φ3.0mm aluminum wire using a 13-pass drawing die. The specific die dimensions are shown in Table 2:
[0061] Table 2 13-pass wire drawing die
[0062]
[0063] The drawn aluminum wire is twisted into conductors with different cross-section requirements by a frame stranding machine. The structure of the conductor is a regular twist of 1+6 or 1+6+12 or 1+6+12+18... The twisted conductor is pressed once by a roller-type pressing die with a circular hole to make the conductor surface smooth and the electric field uniformity better; after a layer of 0.5mm semi-conductive water-resistant tape is wrapped around the outside of the compressed conductor, a polyethylene insulation layer is extruded on the outside through an extrusion process. The thickness of the insulation layer is 2.5mm-3.0mm, and the overlap of the wrapped semi-conductive water-resistant tape is 30%-50%; a layer of aluminum alloy tape is wrapped around the outside of the insulation layer as the shielding layer of the cable by wrapping or longitudinal wrapping. The thickness of the aluminum alloy tape is 0.2mm, and the wrapping should be tightly wrapped with an overlap of more than 15%.
[0064] G657 bending-resistant optical fiber is used, and corrosion-resistant stainless steel strips are laser welded into seamless steel pipes. Optical fibers are placed in the seamless steel pipes, and hydrogen-absorbing fiber paste is filled in the steel pipes. The size of the stainless steel pipes is Φ1.2mm-Φ2.0mm. The stainless steel pipe containing optical fibers is used as the central pipe, and high-strength steel wires with a diameter of Φ1.2mm and a tensile strength of 2100Mpa are evenly twisted in its outer layer as a tensile layer to prepare a steel strand core. The structure of the steel strand is 1+6 or 1+6+12 or 1+6+12+18... twisted, with a stainless steel pipe containing optical fibers in the center.
[0065] Using G657 bending-resistant optical fiber, first dip-coat a layer of 0.03mm acrylic resin on the outside of the optical fiber, and form an optical fiber buffer layer through UV curing; then use a -40℃ cold-resistant flexible nylon material to extrude a tight sleeve layer on the outside of the optical fiber with a thickness of about 0.3mm to armor the optical fiber and prepare a tight sleeve optical fiber with an outer diameter of Φ0.9mm; use a braiding device to braid a tensile layer with aramid material on the outside of the Φ0.9mm tight sleeve optical fiber, and the braiding density of aramid is not less than 85% to improve the tensile performance of the optical fiber. The outer diameter of the braided layer is Φ1.2mm. Use ETFE fluoroplastic to extrude a sheath with better tensile performance, smoother and better temperature resistance on the outside of the braided layer to protect the optical fiber from the influence on the optical unit during the conductor heating process, and the final outer diameter is Φ1.8mm.
[0066] The multi-core insulated sheathed aluminum alloy conductors are twisted into cables. During the twisting process, the optical fiber units with ETFE sheaths and the filling rope materials are used to fill the twisting gaps to ensure better roundness of the appearance and make the outer diameter of the cable more uniform. Finally, the aluminum alloy wire core with optical fiber is prepared by wrapping the gaps with a wrapping tape. Among them, one core ETFE sheathed optical fiber unit is ensured to be filled in the central gap position of the aluminum alloy conductor, which is convenient for testing the temperature and current carrying capacity of the conductor, and other optical fiber units can be filled in the gaps.
[0067] Finally, the aluminum alloy core is arranged in parallel with the steel strand core, and a polyethylene sheath is extruded on its outer layer by an extruder. The middle of the two cores is connected and fixed by a sling to form a self-supporting cable. The self-supporting cable is a lightweight, high-tensile aluminum alloy optoelectronic composite cable that integrates optical fiber and power transmission wire, and has information transmission, power transmission and optical fiber sensing functions.
[0068] This embodiment uses molten aluminum to directly cast aluminum rods, avoiding the use of aluminum ingots to heat and consume too much energy, facilitating the control of the composition of the aluminum wire, and achieving low-carbon and environmentally friendly production; directly using high-purity molten aluminum and aluminum ingots, controlling some trace components within the requirements, making on-site operation more convenient and more efficient, and being able to stably produce high-conductivity aluminum alloy rods; using an appropriate amount of aluminum ingots to add to molten aluminum reduces the excessively high temperature of the molten aluminum, and also has a better effect on grain refinement during the casting process.
[0069] This embodiment adopts the process of furnace refining, and combines electromagnetic stirring to degas and deslag the aluminum melt in the furnace. The combined process of "gas + refining agent" has better degassing and deslaging effects and lower energy consumption; secondary online rotor degassing and deslaging is adopted, and H2 and oxidized impurities in the aluminum melt are adsorbed by tiny bubbles to bring out the aluminum melt, so that the degassing and deslaging effects are more thorough and the purity of the melt is improved; a two-stage foam ceramic filter plate device is used to perform double filtration of the aluminum melt, which has better filtering effects and higher purity of the aluminum melt.
[0070] This embodiment adopts a flat-vertical twin-roller rolling mill, which has a larger rolling reduction in rough rolling and a higher rolling accuracy in finishing rolling. It compacts and welds the defects such as shrinkage, looseness, voids and pores inside the aluminum strip to make the structure denser, improve the uniformity of the structure, and improve the strength and toughness of the later aluminum wire. The flat-vertical twin-roller rolling mill has lower wear on the rolls, and is easier to disassemble during roll maintenance, making the maintenance of the mill equipment more convenient and saving labor.
[0071] This embodiment configures different drawing processes according to different outer diameters of aluminum wires, and the drawing pass configuration is more scientific and reasonable, and the aluminum wire drawing process is more energy-saving and efficient; high-conductivity aluminum rods are used to draw aluminum wires, and the product has lower resistance, smaller line loss, and is low-carbon and environmentally friendly; high-strength steel wires are used, which have higher tensile strength, and optical fiber stainless steel pipes are used in the center to achieve the transmission of optical information, and at the same time, the healthy operation of the cable can be monitored, such as real-time monitoring of the damage to the line caused by wind, rain, snow and other weather. Aluminum alloy cables use optical fiber as a dual function of communication and sensing. On the one hand, it realizes the transmission of power and information, and on the other hand, it can monitor the heat generation and current carrying capacity of aluminum alloy cables in real time, evaluate the long-term operation of the line, and ensure the safety of the line.
[0072] This embodiment uses steel core stranded wire as the load-bearing wire, which improves the construction efficiency of the overhead insulated aluminum alloy cable, saves construction costs, and can be completed in one construction, saving labor and increasing construction speed.
[0073] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A self-supporting aluminum alloy cable for a wind turbine, characterized in that: It includes a steel strand core, an aluminum alloy core and an outer sheath, wherein the steel strand core is a self-supporting steel strand containing optical fiber; a single-core or two-core or more aluminum alloy core is arranged in parallel with the steel strand core, and the outer sheath is wrapped around the outside of the steel strand core and the aluminum alloy core; the gap between the aluminum alloy cores is filled with optical fiber units and filling ropes.
2. A self-supporting aluminum alloy cable for a wind turbine according to claim 1, characterized in that: The aluminum alloy wire core comprises a conductor, and a conductor shielding layer, an insulating layer and an insulating shielding layer are sequentially arranged on the outer side of the conductor.
3. A self-supporting aluminum alloy cable for a wind turbine according to claim 1 or 2, characterized in that: The steel strand core comprises a central tube, and multiple layers of steel wires are evenly twisted on the outer side of the central tube; an optical fiber is arranged in the central tube, and the central tube is filled with hydrogen absorbing fiber paste.
4. A process for preparing a self-supporting aluminum alloy cable for a wind turbine according to any one of claims 1 to 3, characterized in that: include: The aluminum alloy melt is formed by using high-purity aluminum water and aluminum ingots through batching, mixing and homogenization, degassing and deslagging, and static processing; The aluminum alloy melt is used to prepare an aluminum rod with a set diameter through continuous casting and rolling processes, and the aluminum rod is drawn to form a single wire with a set diameter range; a plurality of single wires are twisted into a conductor; The conductor is wrapped with a conductor shielding layer, an insulating layer and an insulating shielding layer in sequence, and then twisted with the optical fiber unit and the filling rope to form an aluminum alloy wire core; The aluminum alloy core and the steel strand core are arranged in parallel, and a polyethylene sheath layer is extruded on the outer layer through an extrusion process.
5. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 4, characterized in that: Pour the molten aluminum into the melting furnace and add the cold aluminum ingots for batching; The requirements for the composition of the aluminum melt after batching are as follows: Si content within 0.1%, Fe content within 0.15%, the ratio of Fe to Si about 1.3-1.8, copper content within 0.001%, Mg content within 0.01%, Zn content within 0.02%, V content within 0.02%, Ti content within 0.02%, other single component content within 0.015%, and the total content of components within 0.3%.
6. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 5, characterized in that: After the cold aluminum ingot is added, the aluminum melt in the furnace is stirred by the electromagnetic stirring at the bottom of the melting furnace; after the cold material is completely melted, the aluminum melt is refined by the aluminum liquid refining equipment in the furnace, and the refining agent is injected into the aluminum melt through the pulse gas of N2 or Ar. The pulse control time is 80-200ms, and the bubbles are broken by the graphite rotor to make the aluminum melt in the furnace and the refining agent gas sprayed by the graphite rotor evenly mixed.
7. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 4, characterized in that: After refining in the furnace, the molten metal that has been deslagging is sent to the online rotor degassing device for secondary refining and degassing. After the secondary refining and degassing, the melt is filtered and deslagging is carried out, wherein the filtering device uses a double-stage foam ceramic filter plate to perform double filtration on the aluminum melt.
8. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 7, characterized in that: After two online degassing and slag removal processes inside and outside the furnace, the aluminum melt is left to stand, cooled and solidified to form aluminum bars; the aluminum bars are first rough-rolled by a roller mill for 1-2 passes, then stretched for 3-8 passes, and then rolled before the finished product for 9-12 passes, and finally rolled into finished aluminum rods through 3 passes.
9. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 4, characterized in that: Multi-core insulated sheathed aluminum alloy conductors are twisted into cables. During the twisting process, optical fiber units with ETFE sheaths and filling rope materials are used to fill the twisted gaps. Finally, a wrapping tape is used to wrap the gaps to prepare an aluminum alloy wire core with optical fiber.
10. The process for preparing a self-supporting aluminum alloy cable for a wind turbine according to claim 9, characterized in that: Acrylic resin is dipped on the outside of the optical fiber and cured by ultraviolet light to form an optical fiber buffer layer; a flexible nylon material is used to extrude a tight jacket layer on the outside of the optical fiber to armor and protect the optical fiber, thereby preparing a tight jacket optical fiber; Aramid material is used to weave a tensile layer outside the tight-buffered optical fiber, and ETFE fluoroplastic is used to extrude a sheath outside the tensile layer.