Preparation method of iron-silicon magnetic powder core material with high magnetic conductivity

By combining organic and inorganic coating insulation processes, the problem of low permeability of iron-silicon magnetic powder core materials in the mid-to-high frequency range has been solved, realizing the preparation of iron-silicon magnetic powder core materials with high permeability and low eddy current loss, which are suitable for mid-to-high frequency electronic equipment.

CN119008160APending Publication Date: 2024-11-22BEIJING QIXING FEIXING ELECTRONICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410903238.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing iron-silicon magnetic powder core materials have low permeability and high eddy current loss in the 50Hz to 2MHz frequency band, making it difficult to meet the high permeability requirements of medium and high frequency electronic equipment.

Method used

An insulation process combining organic and inorganic coatings is employed. Iron-silicon metal magnetic powder cores are coated with phosphoric acid and resin, followed by pressing and heat treatment to form a phosphate film and resin coating, thereby improving magnetic permeability and enhancing mechanical strength.

Benefits of technology

The obtained high-permeability iron-silicon magnetic powder core material exhibits low eddy current loss and excellent paramagnetism in the 50Hz–2MHz frequency band, making it suitable for medium- and high-frequency electronic equipment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of an iron-silicon magnetic powder core material with high magnetic conductivity. The preparation method comprises the following steps: carrying out coating treatment on iron-silicon metal magnetic powder core raw powder with high saturation characteristic; then putting into a press die cavity, and performing compression molding; putting a product subjected to compression molding into a kiln, and carrying out heat treatment at a certain temperature and in a protective atmosphere; epoxy resin paint is sprayed on the product subjected to heat treatment to cover the surface of the product, so that the appearance and moisture resistance of the product are improved. The iron-silicon material metal magnetic powder core with high magnetic conductivity obtained by the preparation method disclosed by the invention effectively overcomes the problem of overlarge resistance in actual use, can realize the purpose of bearing large current, is lower in eddy current loss and better in paramagnetism when being used at 50Hz-2MHz, and is suitable for meeting the requirements of current electronic equipment on filters.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an iron silicon magnetic powder core material with high magnetic permeability, belonging to the technical field of preparation of iron silicon magnetic powder core materials. Background Art

[0002] With the development of electronic products towards miniaturization and high power, the requirements for the electromagnetic and mechanical properties of magnetic powder core materials are gradually increasing, and the demand for magnetic powder cores with high magnetic permeability and high DC bias magnetic field is becoming stronger. Photovoltaic inverters, uninterruptible power supplies, and active power filters are electronic devices with a high usage rate today, and they should also meet the requirements of carrying medium and high frequencies. At present, photovoltaic inverters, uninterruptible power supplies, and active power filters are generally made of iron silicon metal magnetic powder core materials. The magnetic powder core of iron silicon material has better power loss and excellent DC superposition characteristics, and it has a higher saturation flux density and can carry high current usage scenarios. When used in the 50Hz~2MHz frequency band, the iron silicon material magnetic powder core with lower magnetic permeability will have higher resistance, greater eddy current loss, and poor paramagnetism. There is a greater demand for magnetic powder cores with high magnetic permeability in the application scenarios of the 50Hz~2MHz frequency band. Therefore, how to prepare magnetic powder cores with higher magnetic permeability is a technical problem that needs to be solved urgently. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In order to solve the above problems in the prior art, the present invention provides a method for preparing an iron silicon magnetic powder core material with high magnetic permeability.

[0005] (II) Technical solution

[0006] In order to achieve the above object, the main technical solutions adopted by the present invention include:

[0007] A method for preparing an iron silicon magnetic powder core material with high magnetic permeability comprises the following steps:

[0008] S1. The original powder of the iron-silicon metal magnetic powder core with high saturation characteristics is coated. First, phosphoric acid is used to inorganically coat the original powder of the iron-silicon metal magnetic powder core to form a phosphide film on the surface of the powder, and then resin is added for organic coating, and finally a proper amount of lubricant is added; S2. The prepared powder is placed in the mold cavity of the press, the press is started, the tonnage of the press is adjusted, and the press is pressed into shape;

[0009] S3, placing the pressed product into a kiln for heat treatment at a certain temperature and in a protective atmosphere;

[0010] S4. Spray the heat-treated product with epoxy resin paint to cover its surface and improve its appearance and moisture resistance.

[0011] In the preparation method as described above, preferably, in step S1, the raw powder of the iron silicon metal magnetic powder core is composed of Si: 5% to 6.5%, Cr: ≤0.04%, C: ≤0.02%, O≤0.065%, and the rest is Fe, by weight percentage.

[0012] In the preparation method as described above, preferably, in step S1, the amount of phosphoric acid used is 0.6‰ to 2‰ of the weight of the powder; the resin is mark resin, and the amount of the resin added is 5‰ to 7‰ of the weight of the powder; the lubricant is E206, and the amount of the lubricant used is 1‰ to 4‰ of the weight of the powder.

[0013] Furthermore, the phosphoric acid needs to be dissolved in 15% to 20% of the weight of the powder with anhydrous ethanol before being added, and the Marc resin needs to be dissolved in 15% to 20% of the weight of the powder with acetone before being added.

[0014] In the preparation method as described above, preferably, in step S2, the press tonnage is 14T / cm 2 ~18T / cm 2 .

[0015] In the preparation method as described above, preferably, in step S3, the heat treatment is performed by increasing the temperature in a gradient manner under a nitrogen protective atmosphere.

[0016] In the preparation method as described above, preferably, in step S3, the heat treatment is performed by increasing the temperature in a gradient, first pre-baking in an oven at 100°C for 3 to 5 hours, then entering a 300°C temperature zone and burning for 10 minutes, then heating up to 100°C in the next temperature zone, and burning for 50 minutes, then keeping the temperature in a 200°C temperature zone for 30 minutes, taking out the sample, and cooling it down with room temperature.

[0017] In the preparation method as described above, preferably, in step S4, the coating is pre-baked at 150° C. for 8 hours before spraying.

[0018] In the preparation method as described above, preferably, in step S4, the spraying thickness is 0.2 mm to 0.6 mm.

[0019] (III) Beneficial effects

[0020] The beneficial effects of the present invention are:

[0021] The invention provides a method for preparing an iron silicon magnetic powder core material with high magnetic permeability. During phosphating, the ratio of phosphoric acid to solvent and powder is effectively controlled to avoid the destruction of the microscopic particle morphology of the powder and avoid affecting the actual electromagnetic performance.

[0022] The high magnetic permeability iron-silicon material metal powder core obtained by the preparation method of the present invention effectively overcomes the problem of excessive resistance in actual use, can achieve the purpose of carrying large current, and when used at 50Hz to 2MHz, has lower eddy current loss and better paramagnetism, which is suitable for the requirements for filters in current electronic equipment. DETAILED DESCRIPTION

[0023] The present invention adopts an insulation process that combines organic coating and inorganic coating. By using organic and inorganic insulating agents to coat and insulate the insulated powder, the treated powder has a higher magnetic permeability after being processed into a magnetic ring. The higher magnetic permeability has better power loss than the lower magnetic permeability, and it has a higher saturation magnetic flux density and can carry large current usage scenarios.

[0024] The preparation method provided by the present invention requires attention to the following: 1. Insulation coating: During phosphating, the ratio of phosphoric acid to solvent (anhydrous ethanol) and powder must be controlled. Specifically, the ratio of phosphoric acid to solvent and powder is 0.6% to 2% phosphoric acid by weight of the powder dissolved in 15% to 20% anhydrous ethanol by weight of the powder. The phosphoric acid reaction will make the surface morphology of the microscopic particles uneven. When too much phosphoric acid is added, the reaction will be too strong, the morphology will be destroyed, and the actual electromagnetic properties will be affected.

[0025] 2. During pressing, the weight of the powder in the mold cavity must be controlled to keep the unit pressure unchanged during each pressing process to ensure consistent performance and appearance of the product after pressing.

[0026] 3. During heat treatment, the powder needs to be heated slowly and gradually to ensure that the insulation coating effect of the powder is optimal and to obtain a product with the best performance and mechanical strength.

[0027] 4. When spraying, please note that the product needs to be pre-baked to ensure that the epoxy resin paint can fully adhere to the surface of the product, and keep the inside of the product dry after pre-baking to achieve a moisture-proof effect.

[0028] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation methods, wherein the raw materials used in the embodiments can all be commercially available products, such as Mark resin can be purchased from Shanghai Yinai Electrical Equipment Co., Ltd., and E206 can be purchased from Guangzhou Yilon Trading Co., Ltd.

[0029] Example 1

[0030] A method for preparing an iron silicon magnetic powder core material with high magnetic permeability comprises the following steps:

[0031] S1. Insulation coating: coating the raw powder of the iron-silicon metal magnetic powder core with high saturation characteristics; wherein the composition of the raw powder of the magnetic powder core is Si: 5-6.5%, Cr: ≤0.04%, C: ≤0.02%, O≤0.065%, and Fe is the remainder in weight percentage. Phosphoric acid is first used to inorganically coat the powder, and a phosphide film is formed on the surface of the powder; the phosphoric acid needs to be dissolved in anhydrous ethanol first; the amount of phosphoric acid used is 0.6‰ to 2‰ of the weight of the original powder, and the amount of anhydrous ethanol used is 15% to 20% of the weight of the original powder (for example, 1kg of powder requires 0.6g to 2g of phosphoric acid to be dissolved in 150g to 200g of alcohol). The phosphide film reduces the loss of the magnetic powder core, and then mark resin is added for organic coating, and the amount of mark resin added accounts for 5‰ to 7‰ of the weight of the powder; the mark resin is first dissolved in acetone of 15% to 20% of the weight of the powder and then mixed with the powder, and finally the lubricant E206 is added, and the amount of E206 is 1‰ to 4‰ of the weight of the powder, and all the powders are dry mixed in a mixer, and the addition of the lubricant is conducive to the pressing and molding of the powder and improves the density of the magnetic powder core;

[0032] S2. Pressing and molding: put the well-insulated powder into the press cavity, start the press, and adjust the press tonnage to 14T / cm 2 ~18T / cm 2 , press forming;

[0033] S3, high temperature sintering: the pressed and formed products are placed in a kiln for heat treatment under a nitrogen atmosphere. They are first placed in an oven at 100°C for pre-baking for about 4 hours, and then placed in a 300°C temperature zone. Each temperature zone is fired for 10 minutes, and the next temperature zone is heated by 100°C. After firing for 50 minutes, the samples are kept at 200°C for 30 minutes, and then taken out and cooled with room temperature. The products cured by temperature have stable electromagnetic properties and excellent mechanical strength, which is conducive to subsequent practical use.

[0034] S4. Spraying: After pre-baking the heat-treated product at 150°C for 8 hours, spray it with epoxy resin paint to cover its surface with a thickness of 0.2mm to 0.6mm to improve its appearance and moisture-proof ability.

[0035] Wind 10 turns with 0.51mm copper wire and test on E4980A. The magnetic permeability of the product can reach up to 91, the bias current can reach 54% at 100Oe, and the power consumption is 600mw / cm at 50kHz-1000Gs. 3 , more suitable for practical use in the range of 50Hz to 2MHz.

[0036] Specifically, based on Example 1, when the phosphoric acid used was 1.5‰ and 2.5‰ of the original iron silicon metal magnetic powder core powder, the amount of Mark resin was 6‰, and the amount of E206 was 1‰, at 17T / cm2 After pressing and sintering, the magnetic permeabilities of the sample rings were measured to be 91 and 84 respectively.

[0037] Comparative Example 1

[0038] This comparative example is based on Example 1, except that when the amount of the mac resin is 4‰, the sample cannot be pressed into shape; when the amount of E206 is less than 1‰, the sample will be roughened and cannot be formed. The mac resin and E206 used mainly protect the sample from being pressed into shape.

[0039] Comparative Example 2

[0040] This comparative example is based on Example 1, except that when the amount of phosphoric acid is 1.5‰, the amount of E206 is 2‰, and the amount of Mark resin is 6‰ and 10‰ respectively, at 17T / cm 2 After pressing and sintering, the magnetic permeability of the sample ring was measured to be 88 and 86. It can be seen that adding too much resin will reduce the magnetic permeability of the sample.

[0041] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any person skilled in the art can use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an iron silicon magnetic powder core material with high magnetic permeability, It is characterized in that It includes the following steps: S1. The original powder of the iron-silicon metal magnetic powder core with high saturation characteristics is coated. First, phosphoric acid is used to inorganically coat the original powder of the iron-silicon metal magnetic powder core to form a phosphide film on the surface of the powder, and then resin is added for organic coating, and finally a lubricant is added; S2, putting the prepared powder into the die cavity of the press, starting the press, adjusting the tonnage of the press, and pressing into shape; S3, placing the pressed product into a kiln for heat treatment at a certain temperature and in a protective atmosphere; S4. Spray the heat-treated product with epoxy resin paint to cover its surface and improve its appearance and moisture resistance.

2. The preparation method according to claim 1, It is characterized in that In step S1, the iron silicon metal magnetic powder core raw powder is composed of Si: 5% to 6.5%, Cr: ≤0.04%, C: ≤0.02%, O≤0.065%, and the rest is Fe in terms of weight percentage.

3. The preparation method according to claim 1, It is characterized in that In step S1, the amount of phosphoric acid used is 0.6‰ to 2‰ of the weight of the powder; the resin is Marc resin, and the amount of Marc resin added is 5‰ to 7‰ of the weight of the powder; the lubricant is E206, and the amount of the lubricant used is 1‰ to 4‰ of the weight of the powder.

4. The preparation method according to claim 1, It is characterized in that The phosphoric acid needs to be dissolved with 15% to 20% of the weight of the powder in anhydrous ethanol before being added, and the Marc resin needs to be dissolved with 15% to 20% of the weight of the powder in acetone before being added.

5. The preparation method according to claim 1, It is characterized in that In step S2, the press tonnage is 14T / cm 2 ~18T / cm 2 .

6. The preparation method according to claim 1, It is characterized in that In step S3, the heat treatment is carried out by increasing the temperature in a gradient, first pre-baking in an oven at 100°C for about 4 hours, then entering the 300°C temperature zone and burning for 10 minutes, and then heating up to 100°C in the next temperature zone. After burning for 50 minutes, the temperature is lowered to the 200°C temperature zone and kept for 30 minutes. After that, the sample is taken out and cooled down with room temperature.

7. The preparation method according to claim 1, It is characterized in that In step S3, the heat treatment is performed in a nitrogen protective atmosphere.

8. The preparation method according to claim 1, It is characterized in that In step S4, before spraying, pre-baking is performed at 150° C. for 8 hours.

9. The preparation method according to claim 1, It is characterized in that In step S4, in step S4, the spraying thickness is 0.2 mm to 0.6 mm.

Citation Information

Cited By

  • Iron-silicon magnetic powder core and preparation method thereof

    CN120954875A