Preparation method of neodymium-iron-boron magnet and neodymium-iron-boron magnet prepared by same

By introducing impurity remover in the airflow grinding process to remove carbon, oxygen and nitrogen from neodymium iron boron magnets, the negative impact of these impurities on magnetic properties in the existing process is solved, and the magnetic properties are improved, especially intrinsic corrections stubborn force and simplify the preparation process.

CN119008218AActive Publication Date: 2024-11-22FUJIAN CHANGTING GOLDEN DRAGON RARE EARTH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411412479.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-22
Estimated Expiration
2044-10-10

AI Technical Summary

Technical Problem

Non-metallic impurities such as carbon, oxygen and nitrogen present in the existing neodymium iron boron magnet preparation process have a negative impact on magnetic properties, especially reducing the intrinsic coercive force of the magnet, and the process is complex and difficult to simplify.

Method used

In the process of airflow grinding and powdering, impurity removers such as ammonia, chlorine, difluoromethane and chloroform are introduced to remove these impurities during high temperature sintering by forming an unstable composite, reducing carbon, oxygen and in the neodymium iron boron magnets and nitrogen content, thereby improving magnetic properties.

Benefits of technology

It effectively reduces the non-metallic impurities content in neodymium iron boron magnets, significantly improves its magnetic properties, especially its intrinsic coercive force, and simplifies the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008218A_ABST
    Figure CN119008218A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a neodymium-iron-boron magnet and the neodymium-iron-boron magnet prepared by the preparation method. Specifically, the preparation method comprises the following steps: (1) mixing and smelting neodymium-iron-boron magnet raw materials to obtain an alloy sheet; (2) performing hydrogen decrepitation treatment on the alloy sheet to obtain coarse powder; (3) performing micro-crushing treatment on the coarse powder in a jet mill to obtain micro-powder; (4) pressing the micro powder into a green body; and (5) the green body is sintered to obtain the neodymium iron boron magnet, an impurity removing agent is introduced into the jet mill in the step (3), and the impurity removing agent comprises one or more of ammonia gas, chlorine gas, difluoromethane and chloroform. The neodymium-iron-boron magnet prepared by the method has the advantages that the content of non-metal impurities (such as C, O and N) is greatly reduced, so that the magnetic performance (especially the intrinsic coercive force) is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of NdFeB magnetic materials, and in particular to a method for preparing a NdFeB magnet and the NdFeB magnet prepared by the method. Background Art

[0002] As an important type of rare earth functional material, NdFeB permanent magnet material has excellent comprehensive magnetic properties and is widely used in many fields such as the electronics industry and electric vehicles.

[0003] The magnetic properties of NdFeB magnets mainly depend on their microstructure, including grain size, grain boundary phase, and distribution of rare earth-enriched phases. One of the current research hotspots is to improve the magnetic properties of NdFeB magnets by further optimizing the structure of the NdFeB magnet material in the prior art. Specifically, according to the grain boundary diffusion technology, the coercive force of the magnet can be improved by introducing heavy rare earth elements such as dysprosium (Dy) at the grain boundary. In the grain refinement process, the number of grain boundaries can be increased by reducing the size of the grains, thereby improving the coercive force of the magnet. In addition, for example, adding elements such as cobalt (Co) and gallium (Ga) can also improve the magnetic properties of the magnet. In addition, by optimizing the sintering and heat treatment processes, for example, by precisely controlling the sintering and heat treatment processes, the microstructure of the magnet can also be optimized to improve the magnetic properties. At present, further improving the magnetic properties of NdFeB permanent magnets is still a hot research direction that technicians generally pursue.

[0004] However, it is still of great significance to develop a method for preparing NdFeB magnets with a simple process and the ability to further improve the magnetic properties (especially the intrinsic coercive force). Summary of the invention

[0005] Based on the technical problems described above, one of the objects of the present invention is to provide a method for preparing a NdFeB magnet and a NdFeB magnet prepared thereby. The method according to the present invention is simple in process and the prepared NdFeB magnet has improved magnetic properties (especially intrinsic coercive force).

[0006] Specifically, in one aspect, the present invention provides a method for preparing a neodymium iron boron magnet, the method comprising the following steps:

[0007] (1) mixing and smelting NdFeB magnet raw materials to obtain alloy sheets;

[0008] (2) subjecting the alloy flakes to hydrogen cracking treatment to obtain coarse powder;

[0009] (3) finely grinding the coarse powder in a jet mill to obtain fine powder;

[0010] (4) pressing the powder into a green compact; and

[0011] (5) sintering the green compact to obtain the NdFeB magnet, wherein:

[0012] An impurity remover is introduced into the air flow mill in the above step (3), and the impurity remover comprises one or more of ammonia, chlorine, difluoromethane and chloroform.

[0013] According to certain preferred embodiments of the present invention, the temperature in the jet mill is in the range of 10-25° C., and the pressure is in the range of 0.55-0.65 MPa.

[0014] According to certain preferred embodiments of the present invention, in the above step (3), the impurity removing agent is introduced into the inert gas passing to the jet mill.

[0015] According to certain preferred embodiments of the present invention, when the impurity removing agent is ammonia gas, chlorine gas or a mixture thereof, the content of the impurity removing agent in the inert gas is in the range of 1 ppm to 10000 ppm.

[0016] According to certain preferred embodiments of the present invention, when the impurity removing agent is ammonia gas, chlorine gas or a mixture thereof, the content of the impurity removing agent in the inert gas is in the range of 10 ppm to 100 ppm.

[0017] According to certain preferred embodiments of the present invention, when the impurity removing agent is difluoromethane, chloroform or a mixture thereof, the weight ratio of the impurity removing agent to the inert gas is in the range of 1 μg / g to 1000 μg / g.

[0018] According to certain preferred embodiments of the present invention, when the impurity removing agent is difluoromethane, chloroform or a mixture thereof, the weight ratio of the impurity removing agent to the inert gas is in the range of 10 μg / g to 100 μg / g.

[0019] According to certain preferred embodiments of the present invention, the inert gas is nitrogen or argon.

[0020] According to certain preferred embodiments of the present invention, the flow rate of the inert gas containing the impurity remover in the fluid mill is 35-45 m / s. 3 / min range.

[0021] According to certain preferred embodiments of the present invention, the D of the micropowder obtained in step (3) 50 The particle size is in the range of 3.8-4.2 μm.

[0022] According to certain preferred embodiments of the present invention, the NdFeB magnet raw material comprises the following components:

[0023] R: 28-33% by weight, wherein R is a rare earth element, and wherein R comprises Nd and Pr;

[0024] Al: ≤ 0.5 wt%;

[0025] Cu: 0.1-0.6 wt%;

[0026] Co: ≥ 0.4 wt%;

[0027] Ga: ≤ 0.3 wt%;

[0028] Ti: ≤ 0.4 wt%;

[0029] B: 0.98-1.2 wt%;

[0030] Fe: 62-69% by weight, wherein weight % is the percentage of the mass of each component to the total mass of the NdFeB magnet raw material.

[0031] In another aspect, the present invention provides a NdFeB magnet, which is prepared by the preparation method according to any one of the above items.

[0032] Compared with the preparation method of NdFeB magnets in the prior art, the preparation method of NdFeB magnets according to the present invention has the advantage that by adding an impurity remover (for example, one or more of ammonia, chlorine, difluoromethane and chloroform) during the airflow grinding process, the content of non-metallic impurities such as carbon (C), oxygen (O) and nitrogen (N) in the NdFeB magnets can be effectively reduced, which helps to reduce the negative impact of these impurities on the magnetic properties, thereby improving the magnetic properties (especially the intrinsic coercive force) of the prepared NdFeB magnets. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The figure is a process flow chart of the method for preparing a NdFeB magnet according to the present invention. DETAILED DESCRIPTION

[0034] The present invention will be described in further detail below in conjunction with the accompanying drawings and specific embodiments. It will be appreciated that other embodiments are contemplated and may be implemented without departing from the scope or spirit of the present invention. Therefore, the following detailed description is non-restrictive.

[0035] Unless otherwise indicated, all numbers used in the specification and claims to represent feature sizes, quantities and physicochemical properties should be understood as being modified by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0036] As mentioned above, it is still of great significance to develop a method for preparing NdFeB magnets with a simple process that can further improve magnetic properties (especially intrinsic coercive force). The inventors of the present invention have found in their research that impurities present in NdFeB magnets, such as carbon (C), oxygen (O) and nitrogen (N), will have a significant negative impact on the performance of the magnet. For example, in the production process of NdFeB magnets, carbon mainly comes from raw materials and process steps, such as smelting, powder making and molding. Carbon impurities can form carbides with rare earth elements in NdFeB magnets, and these carbides play a pinning role in the magnet, increase the internal stress of the magnet, and thus reduce the magnetic properties of the magnet, especially the coercive force. In addition, oxygen is usually present in the form of rare earth oxide or iron oxide in NdFeB magnets. The increase of oxygen will cause the intrinsic coercive force of the magnet to decrease, because oxygen can form oxides with rare earth elements, and the distribution of these oxides at the grain boundaries will interfere with the magnetization process of the magnet. In addition, nitrogen may exist in the form of nitrides in NdFeB magnets. The formation of nitrides consumes rare earth elements in the magnets, reduces the amount of effective magnetic materials, and leads to reduced magnetic properties of the magnets. According to the technical solution of the present invention, by adding an impurity remover (for example, one or more of ammonia, chlorine, difluoromethane and chloroform) during the airflow milling process, the content of non-metallic impurities such as carbon (C), oxygen (O) and nitrogen (N) in the NdFeB magnets can be effectively reduced, which helps to reduce the negative impact of these impurities on magnetic properties, thereby improving the magnetic properties (especially intrinsic coercive force) of the prepared NdFeB magnets.

[0037] Specifically, the present invention provides a method for preparing a neodymium iron boron magnet, the preparation method comprising the following steps:

[0038] (1) mixing and smelting NdFeB magnet raw materials to obtain alloy sheets;

[0039] (2) subjecting the alloy flakes to hydrogen cracking treatment to obtain coarse powder;

[0040] (3) finely grinding the coarse powder in a jet mill to obtain fine powder;

[0041] (4) pressing the powder into a green compact; and

[0042] (5) sintering the green compact to obtain the NdFeB magnet, wherein:

[0043] An impurity remover is introduced into the air flow mill in the above step (3), and the impurity remover comprises one or more of ammonia, chlorine, difluoromethane and chloroform.

[0044] Figure 1 The process flow chart of the preparation method of the NdFeB magnet according to the present invention is as follows:

[0045] S1: mixing and smelting NdFeB magnet raw materials to obtain alloy sheets;

[0046] S2: performing hydrogen cracking treatment on the alloy sheet to obtain coarse powder;

[0047] S3: finely grinding the coarse powder in a jet mill to obtain fine powder;

[0048] S4: pressing the micro powder into a green body; and

[0049] S5: Sintering the green compact to obtain the NdFeB magnet.

[0050] In this application, unless otherwise specified, the term "impurity remover" refers to a substance that can remove or reduce impurities such as carbon (C), oxygen (O) and nitrogen (N) present in NdFeB magnets under specific conditions (e.g., temperature and pressure). The inventors of the present invention have found in their research that by adding an impurity remover (e.g., one or more of ammonia, chlorine, difluoromethane and chloroform) during the airflow milling process, the content of non-metallic impurities such as carbon (C), oxygen (O) and nitrogen (N) in the obtained NdFeB magnet can be effectively reduced. Although the mechanism by which the impurity remover (e.g., one or more of ammonia, chlorine, difluoromethane and chloroform) removes or reduces impurities such as carbon (C), oxygen (O) and nitrogen (N) is not yet clear and without being bound by theory, it is believed that one or more of ammonia, chlorine, difluoromethane and chloroform introduced during the airflow milling process forms a relatively unstable complex with carbon species, oxygen species and nitrogen species in the coarse powder of the NdFeB magnet raw material at a specific temperature and pressure, and the complex is removed from the NdFeB system in subsequent process steps (e.g., high temperature sintering treatment, etc.).

[0051] According to the technical solution of the present invention, in step (1), NdFeB magnet raw materials are mixed and smelted to obtain alloy sheets.

[0052] There is no particular restriction on the formula of the NdFeB magnet raw material that can be used in the present invention. Preferably, the NdFeB magnet raw material comprises the following components:

[0053] R: 28-33% by weight, wherein R is a rare earth element, and wherein R comprises Nd and Pr;

[0054] Al: ≤ 0.5 wt%;

[0055] Cu: 0.1-0.6 wt%;

[0056] Co: ≥ 0.4 wt%;

[0057] Ga: ≤ 0.3 wt%;

[0058] Ti: ≤ 0.4 wt%;

[0059] B: 0.98-1.2 wt%:

[0060] Fe: 62-69% by weight, wherein weight % is the percentage of the mass of each component to the total mass of the NdFeB magnet raw material.

[0061] Specifically, the prepared NdFeB magnet raw materials are uniformly mixed, then melted at a temperature within a range of 1400-1550° C., and then alloy sheets are cast by a rapid quenching method.

[0062] According to the technical solution of the present invention, in step (2), the obtained alloy sheet is subjected to hydrogen cracking treatment to obtain coarse powder. Preferably, the hydrogen cracking treatment includes hydrogen absorption, dehydrogenation and cooling. The hydrogen absorption is carried out under the condition of hydrogen pressure of 0.09-0.29MPa. The dehydrogenation is carried out under the condition of vacuuming and heating, and the dehydrogenation temperature is 350-550°C.

[0063] According to the technical solution of the present invention, in step (3), the coarse powder is finely pulverized in a jet mill to obtain fine powder.

[0064] The airflow milling process plays an important role in the preparation of NdFeB magnets. It is mainly used to prepare alloy ingots or strip sheets into fine powder. The airflow mill used for NdFeB magnets is usually a fluidized bed airflow mill, which consists of an airflow mill, a cyclone separator, a dust collector and an induced draft fan to form a complete pulverizing system. Usually, an inert gas such as nitrogen is used as the power airflow, and the material is repeatedly collided, rubbed, and sheared under the action of high-pressure gas to be pulverized.

[0065] According to the technical solution of the present invention, preferably, the impurity removing agent (for example, one or more of ammonia, chlorine, difluoromethane and chloroform) is introduced into the inert gas leading to the jet mill.

[0066] According to the technical solution of the present invention, preferably, when the impurity remover is a gas such as ammonia, chlorine or a mixture thereof, the impurity remover is introduced at the inlet pipe of the gas compressor of the jet mill. Preferably, when the impurity remover is a liquid such as difluoromethane, chloroform or a mixture thereof, the impurity remover is introduced at the outlet pipe of the gas compressor of the jet mill.

[0067] According to the technical solution of the present invention, in order to further improve the removal effect of non-metallic impurities (e.g., C, O, and N, etc.), the temperature in the jet mill is in the range of 10-25°C, and the pressure is in the range of 0.55-0.65MPa. The inventors of the present invention have found in their research that when the above temperature and pressure ranges are not met, the effect of removing or reducing the content of non-metallic impurities (e.g., C, O, and N, etc.) from the NdFeB magnet cannot be achieved.

[0068] According to the technical solution of the present invention, when the impurity remover is ammonia, chlorine or a mixture thereof, the content of the impurity remover in the inert gas is in the range of 1ppm to 10000ppm. The inventors of the present invention have found in their research that the content of the impurity remover (e.g., ammonia, chlorine or a mixture thereof) in the inert gas has an important influence on the removal of impurities. When the content of the impurity remover (e.g., ammonia, chlorine or a mixture thereof) in the inert gas is less than 1ppm, the reduction in the content of non-metallic impurities (e.g., C, O and N, etc.) in the obtained NdFeB magnet cannot be detected and the magnetic properties of the obtained NdFeB magnet are poor; when the content of the impurity remover (e.g., ammonia, chlorine or a mixture thereof) in the inert gas is greater than 10000ppm, the presence of excessive impurity remover will cause the magnetic properties of the obtained NdFeB magnet to deteriorate. Preferably, when the impurity remover is ammonia, chlorine or a mixture thereof, in order to further improve the removal effect of non-metallic impurities (e.g., C, O and N, etc.), the content of the impurity remover (e.g., ammonia, chlorine or a mixture thereof) in the inert gas is in the range of 10 ppm to 100 ppm.

[0069] According to the technical solution of the present invention, when the impurity remover is difluoromethane, chloroform or a mixture thereof, the weight ratio of the impurity remover to the inert gas is in the range of 1 μg / g to 1000 μg / g. The inventors of the present invention have found in their research that the content of the impurity remover (e.g., difluoromethane, chloroform or a mixture thereof) in the inert gas has an important influence on the removal of impurities. When the weight ratio of the impurity remover (e.g., difluoromethane, chloroform or a mixture thereof) to the inert gas is less than 1 μg / g, the reduction in the content of non-metallic impurities (e.g., C, O and N, etc.) in the obtained NdFeB magnet cannot be detected and the magnetic properties of the obtained NdFeB magnet are poor; when the weight ratio of the impurity remover (e.g., difluoromethane, chloroform or a mixture thereof) to the inert gas is greater than 1000 μg / g, the presence of an excess of the impurity remover (e.g., difluoromethane, chloroform or a mixture thereof) will cause the magnetic properties of the obtained NdFeB magnet to deteriorate. Preferably, when the impurity remover is difluoromethane, chloroform or a mixture thereof, in order to further improve the removal effect of non-metallic impurities (e.g., C, O and N, etc.), the weight ratio of the impurity remover to the inert gas is in the range of 10 μg / g to 100 μg / g.

[0070] According to the technical solution of the present invention, preferably, the inert gas is nitrogen or argon.

[0071] According to the technical solution of the present invention, preferably, in order to further improve the removal effect of non-metallic impurities (such as C, O and N, etc.), the flow rate of the inert gas containing the impurity remover in the fluid mill is 35-45m / s. 3 / min, preferably 38-40m 3 / min range.

[0072] After the jet mill is pulverized, a lubricant, such as zinc stearate, can be optionally added to the obtained micropowder. The amount of the lubricant added can be 0.05-0.15%, such as 0.12%, of the mass of the micropowder obtained after the pulverization.

[0073] According to the technical solution of the present invention, in step (4), the powder is pressed into a green body. The pressing can be performed by conventional methods in the prior art. For example, a normal orientation pressing method can be used. For example, the molding can be performed by a magnetic field molding method. The magnetic field molding is performed, for example, at a magnetic field strength of 1.8-2.5T.

[0074] Finally, according to the technical solution of the present invention, in step (5), the green body is sintered to obtain the NdFeB magnet. The sintering process can be a conventional sintering process in the art. The sintering temperature can be 1000-1100° C. The sintering time can be 4-8 hours.

[0075] In another aspect of the present invention, a NdFeB magnet is provided. The NdFeB magnet is prepared by the preparation method described above.

[0076] The present invention is described in more detail below in conjunction with the examples. It should be noted that these descriptions and examples are intended to facilitate the understanding of the present invention, rather than to limit the present invention. The protection scope of the present invention shall be subject to the attached claims.

[0077] Example

[0078] In the present invention, unless otherwise indicated, the reagents used are commercial products and are used directly without further purification. In addition, the "%", "wt%" mentioned are "percentage by weight", and the "parts" mentioned are "parts by weight".

[0079] Example 1

[0080] First, the raw materials of NdFeB magnets are uniformly mixed according to the specified formula ratio and smelted into alloy sheets. The formula includes 30 wt% PrNd (praseodymium-neodymium alloy), 0.05 wt% Al (aluminum), 0.2 wt% Cu (copper), 0.5 wt% Co (cobalt), 0.3 wt% Ga (gallium), 0.2 wt% Ti (titanium), 0.98 wt% B (boron), and the rest is Fe (iron). The smelting temperature is 1520±5℃.

[0081] Then, the NdFeB alloy sheet is subjected to hydrogen crushing to obtain coarse powder. Hydrogen crushing is a common powder making process. By treating the alloy in a hydrogen atmosphere, its structure becomes loose, which is convenient for subsequent air flow grinding. Hydrogen crushing includes hydrogen absorption, dehydrogenation and cooling. Hydrogen absorption is carried out under the condition of hydrogen pressure of 0.098MPa. Dehydrogenation is carried out under the condition of vacuuming and heating, and the dehydrogenation temperature is 550℃.

[0082] Next, the coarse powder is refined using a jet mill. In this step, nitrogen is selected as the gas for the jet mill, and ammonia is introduced as an impurity remover at the inlet pipe of the gas compressor of the jet mill. The impurity remover, i.e., ammonia, has a content of 10 ppm in nitrogen; the temperature in the jet mill is 15-20°C, and the pressure is 0.6-0.63 MPa; the flow rate of the nitrogen containing ammonia in the jet mill is 38-40 m / s. 3 / min; the particle size D 50 It is alloy micro powder of 4.0-4.2μm.

[0083] Subsequently, the alloy powder is pressed into a green body using a conventional orientation pressing method.

[0084] Then, the green body is sintered. In the sintering process, a multi-stage degassing temperature is designed, including 150℃-300℃-550℃-800℃, and the degassing time is set to 1-3 hours to obtain the NdFeB magnet.

[0085] The sintered NdFeB blank product obtained in Example 1 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0086] The magnetic properties of the sintered NdFeB blank product obtained in Example 1 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0087] Example 2

[0088] A NdFeB magnet was prepared in a similar manner to Example 1, except that the content of the impurity removing agent, i.e., ammonia gas, in nitrogen gas was changed from 10 ppm to 25 ppm.

[0089] The sintered NdFeB blank product obtained in Example 2 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0090] The magnetic properties of the sintered NdFeB blank product obtained in Example 2 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0091] Example 3

[0092] A NdFeB magnet was prepared in a similar manner to Example 1, except that the impurity removing agent was changed from ammonia gas to chlorine gas.

[0093] The sintered NdFeB blank product obtained in Example 3 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0094] The magnetic properties of the sintered NdFeB blank product obtained in Example 3 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured.max The results are shown in Table 2 below.

[0095] Example 4

[0096] A NdFeB magnet was prepared in a similar manner to Example 1, except that the impurity removing agent was changed from ammonia to chlorine, and the content of the impurity removing agent, chlorine, in nitrogen was changed from 10 ppm to 25 ppm.

[0097] The sintered NdFeB blank product obtained in Example 4 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0098] The magnetic properties of the sintered NdFeB blank product obtained in Example 4 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0099] Example 5

[0100] A NdFeB magnet was prepared in a similar manner to Example 1, except that the impurity removing agent was changed from ammonia to dichloromethane, and the weight ratio of the impurity removing agent dichloromethane to the inert gas was 10 μg / g.

[0101] The sintered NdFeB blank product obtained in Example 5 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0102] The magnetic properties of the sintered NdFeB blank product obtained in Example 5 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0103] Example 6

[0104] A NdFeB magnet was prepared in a similar manner to Example 1, except that the impurity removing agent was changed from ammonia to dichloromethane, and the weight ratio of the impurity removing agent dichloromethane to the inert gas was 25 μg / g.

[0105] The sintered NdFeB blank product obtained in Example 6 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0106] The magnetic properties of the sintered NdFeB blank product obtained in Example 6 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0107] Comparative Example 1

[0108] NdFeB magnets were prepared in a similar manner to Example 1, except that no impurity removing agent was introduced during the jet milling process.

[0109] The sintered NdFeB blank product obtained in Comparative Example 1 was sampled at multiple points to test the total amount of non-metallic impurities, namely carbon (C), oxygen (O) and nitrogen (N), wherein each sample was tested twice and the average value was calculated. The results are shown in Table 1 below.

[0110] The magnetic properties of the sintered NdFeB blank product obtained in Comparative Example 1 (including remanence (Br), intrinsic coercivity (Hcj), magnetic energy product / coercivity (Hk / Hcj), apparent coercivity (Hcb) and maximum magnetic energy product (BH)) were measured. max The results are shown in Table 2 below.

[0111]

[0112] By comparing Examples 1-6 and Comparative Example 1 shown in Table 1 above, it can be seen that the NdFeB magnets prepared according to the method of the present invention have a significantly reduced content of non-metallic impurities (e.g., C, O, N, etc.) compared to those without using an impurity remover (e.g., one or more of ammonia, chlorine, difluoromethane, and chloroform), and thus have improved magnetic properties (especially, intrinsic coercive force).

[0113] The embodiments described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should fall within the protection scope of the present invention. The technical contents for which protection is sought in the present invention have all been recorded in the claims.

Claims

1. A method for preparing a neodymium iron boron magnet, the method comprising the following steps: (1) mixing and smelting NdFeB magnet raw materials to obtain alloy sheets; (2) subjecting the alloy flakes to hydrogen cracking treatment to obtain coarse powder; (3) finely grinding the coarse powder in a jet mill to obtain fine powder; (4) pressing the micropowder into a green compact; and (5) sintering the green compact to obtain the NdFeB magnet, wherein: An impurity remover is introduced into the air flow mill in the above step (3), and the impurity remover comprises one or more of ammonia, chlorine, difluoromethane and chloroform.

2. The method for preparing a NdFeB magnet according to claim 1, wherein the temperature in the jet mill is in the range of 10-25°C, and the pressure is in the range of 0.55-0.65 MPa.

3. The method for preparing a NdFeB magnet according to claim 1, wherein in the above step (3), the impurity remover is introduced into the inert gas leading to the jet mill.

4. The method for preparing a NdFeB magnet according to claim 3, wherein when the impurity remover is ammonia, chlorine or a mixture thereof, the content of the impurity remover in the inert gas is in the range of 1 ppm to 10000 ppm.

5. The method for preparing a NdFeB magnet according to claim 3, wherein when the impurity remover is ammonia, chlorine or a mixture thereof, the content of the impurity remover in the inert gas is in the range of 10 ppm to 100 ppm. 6 . The method for preparing a NdFeB magnet according to claim 3 , wherein when the impurity remover is difluoromethane, chloroform or a mixture thereof, a weight ratio of the impurity remover to the inert gas is in the range of 1 μg / g to 1000 μg / g. 7 . The method for preparing a NdFeB magnet according to claim 3 , wherein when the impurity remover is difluoromethane, chloroform or a mixture thereof, a weight ratio of the impurity remover to the inert gas is in the range of 10 μg / g to 100 μg / g.

8. The method for preparing a NdFeB magnet according to claim 3, wherein the inert gas is nitrogen or argon.

9. The method for preparing a NdFeB magnet according to claim 3, wherein the flow rate of the inert gas containing the impurity remover in the fluid mill is 35-45 m / s. 3 / min range.

10. The method for preparing a NdFeB magnet according to claim 1, wherein the D of the powder obtained in step (3) is 50The particle size is in the range of 3.8-4.2 μm.

11. The method for preparing a NdFeB magnet according to claim 1, wherein the NdFeB magnet raw material comprises the following components: R: 28-33% by weight, wherein R is a rare earth element, and wherein R comprises Nd and Pr; Al: ≤ 0.5 wt%; Cu: 0.1-0.6 wt%; Co: ≥ 0.4 wt%; Ga: ≤ 0.3 wt%; Ti: ≤ 0.4 wt%; B: 0.98-1.2 wt%; Fe: 62-69% by weight, wherein weight % is the percentage of the mass of each component to the total mass of the NdFeB magnet raw material.

12. A neodymium iron boron magnet, wherein the neodymium iron boron magnet is prepared by the preparation method according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Method for preparing high performance sintered neodymium-iron-boron air stream millby hydrogenation

    CN101051544A

  • Preparation method of Sm-Fe-N permanent magnet powder

    CN108777204A

  • High-coercivity neodymium iron boron magnetic material and preparation method thereof

    CN115732155A

  • Neodymium-iron-boron magnet and preparation method thereof

    CN115798917A

  • Method for manufacturing high performance neodymium-iron-boron permanent magnetic material

    WO2011134178A1