Grid annealing method of ferroelectric transistor, grid structure and ferroelectric transistor
By adopting nitrogen adsorption treatment and nanosecond laser annealing technology in ferroelectric field effect transistors, fatigue and thermal crosstalk problems caused by oxygen vacancies are solved, and the stability and durability of the ferroelectric layer are improved, suitable for small sizes High temperature annealing requirements for devices.
Patent Information
- Application Number
- CN202411099886.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
Existing ferroelectric field effect transistors (FeFETs) are prone to oxygen vacancies during high-temperature annealing, resulting in fatigue phenomena and thermal crosstalk problems, and it is difficult to compatible with the high-temperature requirements of small-sized devices.
The ferroelectric material is deposited by atomic layer deposition process and nitrogen adsorption treatment is performed on its surface. Combined with nanosecond laser annealing technology, an interface nitrogen adsorption layer is formed to inhibit the generation of oxygen vacancies, and the ferroelectric phase is activated through a low thermal budget to reduce oxygen vacancies aggregation. risk.
It effectively alleviates fatigue problems and thermal crosstalk in ferroelectric transistors, improves the stability and durability of the ferroelectric layer, and is suitable for high-temperature annealing requirements for small-sized devices.
Smart Images

Figure CN119008395A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of microelectronics, and in particular relates to a gate annealing method of a ferroelectric transistor, a gate structure, and a ferroelectric transistor. Background Art
[0002] The rapid development of big data and artificial intelligence has put forward higher demands on data storage, which has forced the development of new non-charge media memories to become a research focus in the field of microelectronics, such as resistive memory, phase change memory, and ferroelectric memory, in order to meet the needs of non-volatile storage, in-memory computing, and brain-like computing for low power consumption, high speed, and high reliability.
[0003] In related technologies, doped HfO2 has been proven to stimulate ferroelectric properties, so doped hafnium-based ferroelectric materials have been widely studied and attempted to be applied in 1T1C memory technology (Ferroelectric RAM, FeRAM) and 1T ferroelectric field-effect transistors (FeFETs) to solve the problem of the difficulty in miniaturizing classic perovskite ferroelectric materials.
[0004] However, there are still various difficulties in the current research of FeFET: the first is the fatigue problem. In order to make the doped hafnium-based oxide exhibit ferroelectricity, a metal cap layer is required to provide tensile stress to stabilize the ferroelectric orthorhombic phase (O phase) and tetragonal phase (T phase). Considering the compatibility with the complementary metal oxide semiconductor (CMOS) process, titanium nitride is usually selected as the top electrode, but the titanium element will absorb the oxygen element in the hafnium-based oxide, causing a large number of oxygen vacancies to appear near the interface between the top electrode and the ferroelectric layer. These oxygen vacancies will gather under the action of field stress to form ferroelectric reversal domains with effective built-in field pinning, causing ferroelectric fatigue. The second is the problem of thermal crosstalk. Hafnium-based ferroelectric materials need to undergo high-temperature annealing (about 500°C) to activate the ferroelectric phase. This is a relatively high thermal budget requirement for the source, drain and silicide of small-sized devices. Ferroelectric crystallization has an adverse effect on the source and drain impurity distribution and silicide, changing the device performance. At the same time, long-term high-temperature annealing will also cause the oxygen vacancies in the ferroelectric layer to accumulate, causing fatigue.
[0005] In summary, it is necessary to regulate the interfacial oxygen vacancies to alleviate the fatigue problem, and use an annealing method with a low thermal budget, short holding time and large cooling rate to regulate the oxygen vacancies in the body and alleviate the thermal crosstalk problem.
[0006] Therefore, it is of far-reaching practical significance to develop a method for activating the ferroelectric phase of hafnium-based ferroelectric materials with a low thermal budget (annealing temperature less than 500°C and annealing time less than seconds) while improving the fatigue phenomenon of ferroelectric transistors. Summary of the invention
[0007] In view of this, in order to solve at least one of the above and other technical problems in the related art, the present disclosure provides a gate annealing method for a ferroelectric transistor, comprising:
[0008] Forming an N / P well layer, a source electrode and a drain electrode on a substrate, wherein the source electrode and the drain electrode are formed at two ends of the N / P well layer;
[0009] Depositing a laser reflection layer in the source region and the drain region;
[0010] Depositing a ferroelectric material in the gate region through an atomic layer deposition process to form a ferroelectric layer, and performing a surface nitrogen enrichment treatment on the upper surface of the ferroelectric layer to form an interface nitrogen adsorption layer on the upper surface of the ferroelectric layer;
[0011] Depositing titanium nitride as a capping layer on the ferroelectric layer having the interfacial nitrogen adsorption layer to ensure the phase stability of the ferroelectric layer, and inducing the ferroelectric layer to generate a ferroelectric phase through laser annealing;
[0012] A conductive metal is deposited on the capping layer to form a gate metal stack.
[0013] According to an embodiment of the present disclosure, in the laser annealing process, the laser wavelength is 200-527nm, the laser power is 3-5W, and the laser current is 9.8-10.2A.
[0014] According to an embodiment of the present disclosure, in the nitrogen-enriched treatment, the nitrogen-enriched atmosphere is ammonia gas, the nitrogen-enriched treatment time is 1-15 min, and the flow rate of ammonia gas is 200-300 sccm.
[0015] According to an embodiment of the present disclosure, the gate annealing method includes depositing a laser reflection layer in the source region and the drain region:
[0016] Silicon nitride is deposited in the source and drain regions respectively as gate isolation, and tungsten and silicon dioxide are deposited in sequence. The silicon dioxide and tungsten in the gate region are then removed. The tungsten in the source and drain regions is used as a laser reflection layer to protect the source and drain.
[0017] According to an embodiment of the present disclosure, the conductive metal is tungsten.
[0018] According to an embodiment of the present disclosure, the aforementioned gate annealing method further includes sequentially performing photolithography and etching on the gate metal stack to obtain a gate of a target pattern.
[0019] According to an embodiment of the present disclosure, the etching process removes the laser reflection layer in the source region and the drain region.
[0020] According to an embodiment of the present disclosure, the ferroelectric material is hafnium oxide with doping elements, and the doping elements include silicon, aluminum, zirconium, yttrium, cadmium, lanthanum, and strontium.
[0021] In another aspect of the present disclosure, a gate structure of a ferroelectric transistor prepared according to the aforementioned gate annealing method is proposed, comprising a gate oxide layer, a ferroelectric layer, a cap layer and a gate metal stack. The gate oxide layer is suitable for forming an insulating structure to reduce gate leakage, enhance the control of the gate voltage on the channel carriers, and control the switch and working current of the ferroelectric transistor; the ferroelectric layer is formed on the gate oxide layer, and the ferroelectric layer has a ferroelectric phase, and through the spontaneous polarization state, according to the change of the polarization state by the gate voltage signal, the threshold voltage drift of the channel current is regulated; the cap layer is formed on the ferroelectric layer, and the cap layer is suitable for stabilizing the orthogonal phase of the ferroelectric phase crystallization in the ferroelectric layer to enhance the ferroelectric properties of the ferroelectric layer; the gate metal stack is formed on the cap layer, and the gate metal stack is suitable for receiving an external voltage.
[0022] In another aspect of the present disclosure, a ferroelectric transistor is proposed, comprising a substrate, an N / P well layer, a source, a gate and a drain. The N / P well layer is formed on the substrate, and the N / P well layer is suitable for isolating the channel carriers from the substrate to avoid the latch effect; the source is formed at one end of the N / P well layer; the gate structure is the aforementioned gate structure, formed in the middle of the N / P well layer and used as a gate, and the gate metal stack of the gate stack structure polarizes the ferroelectric layer when an external voltage is applied, so that the gate structure outputs a gate voltage to control the carrier state of the channel structure and realize the opening and closing of the ferroelectric transistor; the drain is formed at the other end of the N / P well layer.
[0023] According to the embodiments of the present disclosure, the gate annealing method proposed in the present disclosure alleviates the fatigue problem and the thermal crosstalk problem by regulating the strategy of oxygen vacancies in the ferroelectric phase and on the surface. Specifically, after the atomic layer deposition (ALD) technology is used for the ferroelectric layer, ammonia is used as a nitrogen-rich atmosphere to perform an in-situ interface nitrogen-enriched treatment on the surface of the ferroelectric layer to obtain a ferroelectric layer with an interface nitrogen adsorption layer. The interface nitrogen adsorption layer will inhibit the cap layer from absorbing oxygen from the ferroelectric layer, thereby reducing the generation of oxygen vacancies at the interface of the ferroelectric layer. Since the process of NH3 treatment inhibiting the absorption of oxygen by titanium elements and the process of high-temperature rapid thermal annealing promoting the absorption of oxygen by titanium elements are in competition, the nitrogen-enriched treatment needs to be manifested under low thermal budgets. Therefore, the present disclosure designs an annealing scheme of nanosecond short-wave laser annealing to activate the ferroelectric phase. Its extremely fast heating and cooling rate does not allow oxygen vacancies to have enough time to accumulate in the ferroelectric layer, thereby achieving the purpose of regulating oxygen vacancies in the body. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a preparation flow chart of a gate annealing method for a ferroelectric transistor in an embodiment of the present disclosure;
[0025] Figure 2 is a scanning electron microscope image of the ferroelectric phase material in Test Example 1 of the present disclosure;
[0026] Figure 3 is a scanning electron microscope image of the ferroelectric phase material in Test Example 2 of the present disclosure;
[0027] Figure 4 is a scanning electron microscope image of the ferroelectric phase material in Test Example 3 of the present disclosure;
[0028] Figure 5 The ferroelectric material in comparative example 3 of the present disclosure is subjected to 10 3 Polarization test diagram of the wake-up cycle;
[0029] Figure 6 The ferroelectric material in comparative example 3 of the present disclosure is subjected to 10 8 Polarization test diagram of fatigue cycle;
[0030] Figure 7 is a schematic cross-sectional view of the well oxygen layer in Example 1 of the present disclosure;
[0031] Figure 8 In the embodiment 1 of the present disclosure, Figure 7 A schematic cross-sectional view of forming an N / P well layer on the basis of;
[0032] Fig. 9 In the embodiment 1 of the present disclosure, Figure 8 A cross-sectional view of an isolation structure is formed on the basis of
[0033] Fig.10 In the embodiment 1 of the present disclosure, Fig. 9 A schematic cross-sectional view of forming a gate oxide layer on the basis of
[0034] Fig.11 In the embodiment 1 of the present disclosure, Fig.10 A schematic cross-sectional view of forming a dummy gate and a hard mask stack based on the present invention;
[0035] Fig.12 In the embodiment 1 of the present disclosure, Fig.11 A schematic cross-sectional view of a side wall formed on the basis of;
[0036] Fig.13 In the embodiment 1 of the present disclosure, Fig.12 A cross-sectional schematic diagram of source and drain impurity distribution is formed on the basis of
[0037] Fig.14 In the embodiment 1 of the present disclosure, Fig.13 A schematic cross-sectional view of forming source and drain silicide on the basis of;
[0038] Fig.15 In the embodiment 1 of the present disclosure, Fig.14 A schematic cross-sectional view of forming a laser reflection layer on the basis of;
[0039] Fig.16 In the embodiment 1 of the present disclosure, Fig.15 A schematic cross-sectional view of a gate position formed on the basis of FIG.
[0040] Fig.17 In the embodiment 1 of the present disclosure, Fig.16 A cross-sectional schematic diagram of nitrogen enrichment treatment based on
[0041] Fig.18 In the embodiment 1 of the present disclosure, Fig.17 A cross-sectional schematic diagram of laser annealing based on the
[0042] Fig.19 In the embodiment 1 of the present disclosure, Fig.18 A schematic cross-sectional view of a gate metal stack formed on the basis of
[0043] Fig. 20 In the embodiment 1 of the present disclosure, Fig.19 A schematic cross-sectional view of a gate lithography process based on the above;
[0044] Fig.21 In the embodiment 1 of the present disclosure, Fig. 20 Schematic diagram of a cross section of a ferroelectric transistor formed on the basis of.
[0045] In the drawings of this disclosure, the meanings of the reference numerals are:
[0046] 1-substrate; 101-ion implantation layer; 2-well oxide layer; 31-pseudo gate; 32-silicon dioxide layer; 33-silicon nitride layer; 4-sidewall; 51-source impurity region; 52-drain impurity region; 61-source silicide layer; 62-drain silicide; 7-laser reflection layer; 8-gate position; 9-ferroelectric layer; 10-cap layer; 11-gate metal stack; 12-gate; 13-spacer layer; 14-through hole interconnect metal; 15-electrode; 16-source; 17-drain. DETAILED DESCRIPTION
[0047] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0048] The endpoints and any values of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this disclosure.
[0049] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.
[0050] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification and should not be interpreted in an idealized or overly rigid manner.
[0051] In the description of the present disclosure, it is necessary to understand that the terms "longitudinal", "length", "circumferential", "front", "rear", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present disclosure and simplifying the description, and do not indicate or imply that the subsystem or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present disclosure.
[0052] Throughout the drawings, the same elements are represented by the same or similar reference numerals. Conventional structures or configurations will be omitted when they may cause confusion in the understanding of the present disclosure. The shapes, sizes, and positional relationships of the components in the drawings do not reflect the actual size, proportion, and actual positional relationship. In addition, in the present disclosure, any reference symbol between brackets should not be constructed as a limitation to the present disclosure.
[0053] Similarly, in order to simplify the present disclosure and help understand one or more of the various disclosed aspects, in the above description of the exemplary embodiments of the present disclosure, the various features of the present disclosure are sometimes grouped together into a single embodiment, figure, or description thereof. The description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" and the like means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0054] In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the fact that ordinary technicians in the field can implement it. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this disclosure.
[0055] In the process of implementing the present disclosure, it is found that to alleviate the fatigue problem of ferroelectric transistors, it is necessary to reasonably regulate the interface oxygen vacancies of the ferroelectric layer to avoid the formation of a built-in electric field pinning effective ferroelectric switching domains due to the aggregation of oxygen vacancies, resulting in ferroelectric fatigue problems. As for the thermal crosstalk problem, an annealing method with a low thermal budget, short holding time and a large cooling rate is required to activate the ferroelectric phase.
[0056] Therefore, the present invention proposes a technical solution of "NH3 nitrogen-rich passivation + low thermal budget laser annealing" to reduce the concentration of oxygen vacancy defects so as to simultaneously optimize the oxygen vacancies at the ferroelectric interface and in the ferroelectric crystal; wherein, the NH3 nitrogen-rich passivation process optimizes the oxygen vacancies at the ferroelectric layer interface, and the low thermal budget laser annealing process optimizes the oxygen vacancies in the ferroelectric layer.
[0057] Figure 1 It is a preparation flow chart of the gate annealing method of the ferroelectric transistor in the embodiment of the present disclosure.
[0058] The present disclosure provides a gate annealing method for a ferroelectric transistor, such as Figure 1 As shown, the steps S101 to S105 are included:
[0059] Step S101: forming an N / P well layer, a source electrode 16 and a drain electrode 17 on a substrate 1, wherein the source electrode 16 and the drain electrode 17 are formed at two ends of the N / P well layer;
[0060] Step S102: depositing a laser reflection layer 7 in the source region and the drain region;
[0061] Step S103: depositing ferroelectric material in the gate region by atomic layer deposition to form a ferroelectric layer 9, and performing nitrogen enrichment treatment on the upper surface of the ferroelectric layer 9 to form an interface nitrogen adsorption layer on the upper surface of the ferroelectric layer 9. Fig.17 As shown;
[0062] Step S104: depositing titanium nitride as a capping layer 10 on the ferroelectric layer 9 having the interfacial nitrogen adsorption layer, so as to ensure the phase stability of the ferroelectric layer 9, and inducing the ferroelectric layer 9 to generate a ferroelectric phase by laser annealing. Fig.18 As shown;
[0063] Step S105 : depositing a conductive metal on the capping layer 10 to form a gate metal stack 11 .
[0064] According to the embodiments of the present disclosure, the gate annealing method proposed in the present disclosure alleviates the fatigue problem and thermal crosstalk problem by regulating the strategy of oxygen vacancies in the ferroelectric phase and on the surface. Specifically, after the ferroelectric layer 9 is deposited by atomic layer deposition (ALD), ammonia is used as a nitrogen-rich atmosphere to perform an in-situ interface nitrogen-enriched treatment on the surface of the ferroelectric layer 9 to obtain a ferroelectric layer 9 with an interface nitrogen adsorption layer. The interface nitrogen adsorption layer will inhibit the cap layer from absorbing oxygen from the ferroelectric layer 9, thereby reducing the generation of oxygen vacancies at the interface of the ferroelectric layer. Since the process of NH3 treatment inhibiting the absorption of oxygen by titanium elements and the process of high-temperature rapid thermal annealing promoting the absorption of oxygen by titanium elements are in a competitive relationship, the advantage of ammonia treatment in improving fatigue can only be manifested under low thermal budgets. Therefore, the present disclosure designs an annealing scheme of nanosecond short-wave laser annealing to activate the ferroelectric phase. Its extremely fast heating and cooling rate does not allow oxygen vacancies to have enough time to accumulate in the ferroelectric layer, thereby achieving the purpose of regulating oxygen vacancies in the body. At the same time, it also meets the low thermal budget requirements of ammonia passivation treatment, and can highlight the fatigue improvement advantages of NH3 interface passivation nitrogen-enriched treatment.
[0065] In the present disclosure, “in-situ” means that after the ferroelectric layer is deposited by ALD, a nitrogen-rich passivation treatment is performed directly in the ALD chamber using an ammonia gas source of the ALD.
[0066] According to an embodiment of the present disclosure, in the laser annealing process, the laser wavelength is 200-527nm, for example, it can be 200nm, 300nm, 400nm, 500nm, 527nm, etc., and the laser power is 3-5W, for example, it can be 3W, 4W, 5W, etc., and the corresponding current range is 9.8-10.2A, preferably 10A, and the corresponding laser power is 3.8W.
[0067] According to an embodiment of the present disclosure, in the nitrogen-rich treatment, the nitrogen-rich atmosphere is ammonia, and the nitrogen-rich treatment time is 1-15 minutes, for example, it can be 1 minute, 5 minutes, 10 minutes, etc.; the flow rate of ammonia is 200-300 sccm, for example, it can be 200 sccm, 250 sccm, 300 sccm, etc.
[0068] According to the embodiments of the present disclosure, the nitrogen element in the ammonia gas can be preferentially absorbed by the titanium element in the cap layer 10, thereby preventing the titanium element from absorbing oxygen vacancies in the ferroelectric layer 9, thereby achieving regulation of oxygen vacancies in the ferroelectric layer 9. After the ferroelectric layer 9 is obtained by ALD deposition, some active attachment sites (usually some electrostatically charged dangling bonds) will appear at the interface of the ferroelectric layer 9. In-situ NH3 treatment is performed in the ALD chamber, so that NH3 molecules can be adsorbed on the active sites due to electrostatic forces, forming a nitrogen-rich interface. After the subsequent deposition of TiN, the nitrogen-rich interface will preferentially react with the Ti element, preferentially occupy the Ti element, and alleviate the Ti element from absorbing oxygen elements in the ferroelectric layer, thereby achieving regulation of oxygen vacancies on the surface of the ferroelectric layer.
[0069] According to an embodiment of the present disclosure, in step S102, the aforementioned gate annealing method deposits a laser reflection layer 7 in the source region and the drain region, including: depositing silicon nitride in the source region and the drain region respectively to serve as gate isolation, and then depositing tungsten and silicon dioxide in sequence, and then removing the silicon dioxide and tungsten in the gate region, and the tungsten in the source region and the drain region serves as the laser reflection layer 7 to protect the source 16 and the drain 17.
[0070] According to the embodiments of the present disclosure, silicon nitride can form isolation between the gate 12 and the source and drain electrodes on the one hand, and can serve as a CMP stop layer before removing the dummy gate on the other hand.
[0071] According to the embodiments of the present disclosure, metal tungsten is used as a cover layer to reflect most of the short-wave laser, achieve precise regional selective laser irradiation, and only expose and anneal the ferroelectric material in the gate area, thereby preventing the source and drain impurity distribution and silicide from being affected by the laser annealing thermal budget of ferroelectric crystallization.
[0072] According to an embodiment of the present disclosure, the conductive metal is tungsten.
[0073] According to an embodiment of the present disclosure, the gate annealing method further includes sequentially performing photolithography and etching on the gate metal stack 11 to obtain a gate 12 of a target pattern.
[0074] According to an embodiment of the present disclosure, the etching process removes the laser reflection layer in the source region and the drain region.
[0075] According to an embodiment of the present disclosure, the ferroelectric material is hafnium oxide with doping elements, and the doping elements include silicon, aluminum, zirconium, yttrium, cadmium, lanthanum, and strontium.
[0076] In another aspect of the present disclosure, a gate structure of a ferroelectric transistor prepared according to the aforementioned gate annealing method is proposed, comprising a gate oxide layer, a ferroelectric layer 9, a cap layer 10 and a gate metal stack 11. Among them, the gate oxide layer is suitable for forming an insulating structure to reduce gate leakage, enhance the control of the gate voltage on the channel carriers, and control the switch and working current of the ferroelectric transistor; the ferroelectric layer 9 is formed on the gate oxide layer, and the ferroelectric layer 9 has a ferroelectric phase, and through the spontaneous polarization state, according to the change of the polarization state by the gate voltage signal, the threshold voltage drift of the channel current is regulated; the cap layer 10 is formed on the ferroelectric layer 9, and the cap layer 10 is suitable for stabilizing the orthorhombic phase of the ferroelectric phase crystallization in the ferroelectric layer 9 to enhance the ferroelectric properties of the ferroelectric layer 9; the gate metal stack 11 is formed on the cap layer 10, and the gate metal stack 11 is suitable for realizing gate electrode interconnection.
[0077] In another aspect of the present disclosure, a ferroelectric transistor is proposed, including a substrate 1, an N / P well layer, a source 16, a gate 12 and a drain 17. The N / P well layer is formed on the substrate 1, and the N / P well layer is suitable for isolating the channel carriers from the substrate to avoid the latch effect; the source 16 is formed at one end of the N / P well layer; the structure of the gate 12 is the aforementioned gate structure, which is formed in the middle of the N / P well layer and serves as the gate 12. When an external voltage is applied to the gate metal stack 11 of the gate stack structure, the ferroelectric layer 9 is polarized, so that the gate structure outputs a gate voltage to control the carrier state of the channel structure and realize the opening and closing of the ferroelectric transistor; the drain 17 is formed at the other end of the N / P well layer.
[0078] According to the embodiments of the present disclosure, when the gate structure obtained by the gate laser annealing method proposed in the present disclosure is applied, the nitrogen element in the interface nitrogen adsorption layer of the ferroelectric transistor will be preferentially absorbed by the titanium element in the cap layer 10 during operation, thereby ensuring the stability of the oxygen element in the ferroelectric layer 9, reducing the generation of oxygen vacancies, and ensuring the operating stability of the ferroelectric transistor.
[0079] Test Case
[0080] During the implementation of the present disclosure, the feasibility of the "NH3 treatment + laser annealing" technical solution was verified on ferroelectric capacitors, and the optimal conditions were integrated into FeFET.
[0081] Figure 2-Figure 4 They are scanning electron microscope images of the ferroelectric phase materials in Comparative Examples 1, 2, and 3 in this test example.
[0082] In this test example, three groups of comparisons were performed. Among them, the treatment of comparative example 1 is to perform RTP annealing on the ferroelectric capacitor at 350°C for 60s, and its crystal structure is as follows Figure 2As shown; the treatment of comparative example 2 is to carry out nitrogen-enriched treatment in an ammonia atmosphere for 3 minutes, and then perform RTP annealing on the ferroelectric capacitor at 350°C for 60s, and its crystal structure is as shown Figure 3 As shown; the treatment of comparative example 3 is to carry out nitrogen-enriched treatment in an ammonia atmosphere for 3 minutes, and then perform 10A nanosecond laser annealing (corresponding to a laser power of 3.8W) on the ferroelectric capacitor, and its crystal structure is as shown Figure 3 shown.
[0083] From the comparison of Comparative Examples 1 and 2, it can be seen that the interface between TiN and HfZrO is smoother and the interface oxide layer is thinner after NH3 treatment for 3 minutes. From the comparison of Comparative Examples 2 and 3, it can be seen that NLA (nanosecond laser annealing) does not deteriorate the flatness of the interface between TiN and HfZrO because the heating time is very short and the thermal damage is very small; at the same time, the ferroelectric grains activated by NLA are smaller, which may correspond to smaller ferroelectric remnant polarization, making it more suitable for small-sized devices.
[0084] More specifically, the ferroelectric materials obtained by combining nanosecond laser annealing with nitrogen enrichment treatment for different times were subjected to fatigue cycle treatment.
[0085] Figure 5 , Figure 6 The ferroelectric material in comparative example 3 of the present disclosure is subjected to 10 3 wake-up cycles and 10 8 Polarization test diagram of fatigue cycles, where p is the polarization value and V is the voltage value.
[0086] like Figure 5 , 6 As shown in Figure 2, under NLA treatment, pure NH3 atmosphere can indeed effectively improve the remanent polarization (2Pr) of ferroelectric phase materials after wake-up cycle and fatigue cycle. Specifically, when no nitrogen enrichment treatment is performed, 10 3 The 2Pr after the wake-up cycle is 9.3, 10 8 After fatigue cycle, 2Pr is 5.8. After 1, 2, and 3 minutes of NH3 treatment, 10 3 After the wake-up cycle, 2Pr increased by 25.8%, 29.0% and 44.1%, respectively. 8 After fatigue cycles, 2Pr improved by 15.5%, 24.1% and 34.5%, respectively. This result shows that nanosecond laser annealing with low thermal budget can obtain good ferroelectric properties. At the same time, nitrogen-enriched treatment in NH3 atmosphere can further optimize the ferroelectric remnant polarization performance. And within a certain range, the longer the nitrogen-enriched treatment time, the better the remnant polarization optimization performance.
[0087] Example
[0088] In this embodiment, a ferroelectric transistor is completely prepared, wherein the gate is prepared according to the above-mentioned gate annealing method. Figures 7 to 21 They are schematic diagrams of the preparation process in this embodiment.
[0089] Specifically:
[0090] like Figure 7 As shown, silicon dioxide is grown on the surface of a silicon substrate 1 by thermal oxidation as a well oxygen layer 2 .
[0091] like Figure 8 As shown, the substrate 1 is then subjected to ion implantation and well-driving treatment, wherein the ion implantation layer 101 is a schematic structure after the ion implantation and well-driving treatment.
[0092] like Fig. 9 As shown, the well oxide layer 2 is completely removed, and then isolation technologies such as LOCOS or STI are used to achieve device isolation.
[0093] like Fig.10 As shown, a gate oxide layer 2 is regrown.
[0094] like Fig.11 As shown, amorphous silicon, silicon dioxide, silicon nitride, and silicon dioxide are sequentially deposited on the gate oxide layer 2 to form a dummy gate 31, a silicon dioxide layer 32, a silicon nitride layer 33, and a silicon dioxide layer 34, respectively; wherein the silicon dioxide layer 32, the silicon nitride layer 33, and the silicon dioxide layer 34 serve as an ONO hard mask stack.
[0095] like Fig.12 As shown, the ONO hard mask stacks on both sides are etched, and silicon nitride is deposited and etched on both sides of the etched ONO hard mask stacks to obtain sidewalls 4 as an isolation structure.
[0096] like Fig.13 As shown, source and drain ion implantation is performed on the surface of the substrate 1 , and annealing is performed to activate the impurity distribution of the source impurity region 51 and the drain impurity region 52 .
[0097] like Fig.14 As shown, a silicide process is performed on the source impurity region 51 and the drain impurity region 52 to form a source silicide layer 61 and a drain silicide 62 to reduce the source-drain contact resistance.
[0098] like Fig.15 As shown, SiN, W and SiO2 are deposited in sequence at the source and drain positions, and SiO2 and part of W at the gate position are polished off by chemical mechanical polishing (CMP), and the remaining W is used as a laser reflection layer 7 to avoid adverse effects on the source impurity region 51, the drain impurity region 52, the source silicide layer 61 and the drain silicide 62 during subsequent ferroelectric laser annealing. Fig.15The source electrode 16 and the drain electrode 17 are bilaterally symmetrical structures, and the positions of the source electrode and the drain electrode are only shown schematically.
[0099] like Fig.16 As shown, the dummy gate 31 is removed to expose the gate position 8.
[0100] like Fig.17 As shown, the ferroelectric material is deposited by ALD process as the ferroelectric layer 9, and the thickness of the ferroelectric layer is 7 nm. The ferroelectric layer 9 is subjected to nitrogen enrichment treatment, and the interface of the ferroelectric layer 9 is nitrogen enriched in NH3 atmosphere to form an interface nitrogen adsorption layer.
[0101] Then, a 20 nm TiN cap layer 10 is deposited by physical vapor deposition (PVD) to assist ferroelectric crystallization. Fig.18 As shown, through nanosecond laser annealing, extremely fast temperature rise and fall induces ferroelectric phase, relieves the aggregation of oxygen vacancies in the body, avoids pinning ferroelectric flip domains, and improves the durability of ferroelectric transistors. Among them, the parameters of laser annealing are Nd:YLF laser (Tolar527, 35K) with a laser wavelength of 527nm, a laser pulse duration of 200ns, a repetition rate of 500Hz, and a laser power range of 3.1-4.9W. At the same time, due to the shielding of the laser reflection layer 7, the laser is prevented from causing adverse effects on the source impurity region 51, the drain impurity region 52, the source silicide layer 61 and the drain silicide 62.
[0102] like Fig.19 As shown, a 75 nm thick conductive metal W is deposited as the gate metal stack 11.
[0103] like Fig. 20 As shown, the gate region is photolithographically processed, and then dry-etched to transfer the gate pattern, and the laser reflection layer 7 is also etched away at the same time, so as to finally form the gate 12.
[0104] like Fig.21 As shown, SiO2 is deposited as a spacer layer 13 and ON through-hole etching is performed, Ti, TiN and W are deposited in the through-hole area in sequence, and TiN is polished and deposited by CMP process for electrode etching to obtain through-hole interconnection metal 14 and electrode 15. Among them, the structure of the ferroelectric transistor is as follows Fig.21 shown.
[0105] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.
Claims
1. A gate annealing method for a ferroelectric transistor, comprising: Forming an N / P well layer, a source electrode and a drain electrode on a substrate, wherein the source electrode and the drain electrode are formed at two ends of the N / P well layer; Depositing a laser reflection layer in the source region and the drain region; Depositing a ferroelectric material in the gate region by an atomic layer deposition process to form a ferroelectric layer, and performing a surface nitrogen enrichment treatment on the upper surface of the ferroelectric layer to form an interface nitrogen adsorption layer on the upper surface of the ferroelectric layer; Depositing titanium nitride as a capping layer on the ferroelectric layer having the interfacial nitrogen adsorption layer to ensure the phase stability of the ferroelectric layer, and inducing the ferroelectric layer to generate a ferroelectric phase through laser annealing; A conductive metal is deposited on the capping layer to form a gate metal stack.
2. The gate annealing method according to claim 1, wherein: In the laser annealing process, the laser wavelength is 200-527nm, the laser power is 3-5W, and the laser current is 9.8-10.2A.
3. The gate annealing method according to claim 1, wherein: In the nitrogen-enriched treatment, the nitrogen-enriched atmosphere is ammonia gas, the nitrogen-enriched treatment time is 1-15 minutes, and the flow rate of the ammonia gas is 200-300 sccm.
4. The gate annealing method according to claim 1, wherein depositing a laser reflection layer on the source region and the drain region comprises: Silicon nitride is deposited in the source region and the drain region respectively to serve as gate isolation, and tungsten and silicon dioxide are deposited in sequence. The silicon dioxide and tungsten in the gate region are then removed. The tungsten in the source region and the drain region serves as a laser reflection layer to protect the source and the drain.
5. The gate annealing method according to claim 1, wherein: The conductive metal is tungsten. 6 . The gate annealing method according to claim 1 , further comprising sequentially performing photolithography and etching on the gate metal stack to obtain a gate of a target pattern.
7. The gate annealing method according to claim 6, wherein: The etching process removes the laser reflection layer of the source region and the drain region.
8. The gate annealing method according to claim 1, wherein: The ferroelectric material is hafnium oxide with doping elements, and the doping elements include silicon, aluminum, zirconium, yttrium, cadmium, lanthanum, and strontium.
9. A gate structure of a ferroelectric transistor prepared by any gate annealing method as claimed in any one of claims 1 to 8, comprising: The gate oxide layer is suitable for forming an insulating structure to reduce gate leakage, enhance the control of the gate voltage on the channel carriers, and control the switch and operating current of the ferroelectric transistor; A ferroelectric layer is formed on the gate oxide layer, the ferroelectric layer has a ferroelectric phase, and the threshold voltage drift of the channel current is regulated by a spontaneous polarization state and a change in the polarization state according to a gate voltage signal; A cap layer formed on the ferroelectric layer, the cap layer being suitable for stabilizing the orthorhombic phase of the ferroelectric phase crystal in the ferroelectric layer to enhance the ferroelectric properties of the ferroelectric layer; A gate metal stack is formed on the cap layer, and the gate metal stack is suitable for realizing gate electrode interconnection.
10. A ferroelectric transistor comprising: substrate; An N / P well layer is formed on the substrate and is suitable for isolating the channel carriers from the substrate to avoid a latch effect; A source electrode formed at one end of the N / P well layer; A gate, wherein the structure of the gate is the gate structure as claimed in claim 9, formed in the middle of the N / P well layer and used as a gate, and when an external voltage is applied to the gate metal stack of the gate stack structure, the ferroelectric layer is polarized, so that the gate structure outputs a gate voltage to control the carrier state of the channel structure and realize the opening and closing of the ferroelectric transistor; A drain is formed at the other end of the N / P well layer.
Citation Information
Cited By
Gate annealing method for ferroelectric transistor, gate structure, and ferroelectric transistor