Solar cell, preparation method thereof and photovoltaic module

By designing the pit structure and electrode position of the doped semiconductor layer in the solar cell, the passivation film stress problem is solved and the photoelectric conversion efficiency of the solar cell is improved.

CN119008726APending Publication Date: 2024-11-22ZHEJIANG JINKO SOLAR CO LTD +1
View PDF 0 Cites 5 Cited by

Patent Information

Application Number
CN202311738300.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The passivation film of existing solar cells has residual stress, which affects its adhesion and photoelectric conversion efficiency, resulting in low photoelectric conversion efficiency.

Method used

The doped semiconductor layer is designed to have multiple pits on one side away from the substrate to reduce stress on the passivation film, and to be located in part of the pit by the electrode to enhance the contact area between the doped semiconductor layer and the electrode and improve contact performance.

Benefits of technology

The defect rate of the passivation film is reduced, the adhesion between the passivation film and the doped semiconductor layer is enhanced, and the photoelectric conversion efficiency of the solar cell is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008726A_ABST
    Figure CN119008726A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the photovoltaic field, and provides a solar cell and a preparation method thereof, and a photovoltaic module, the solar cell comprises a substrate, and the substrate is provided with a first surface and a second surface which are oppositely arranged; the first surface is provided with a suede structure, and the suede structure comprises a convex structure; the doped semiconductor layer is located on the first surface or the second surface, a plurality of pits are formed in the side, away from the substrate, of the doped semiconductor layer, and the size of the pits is smaller than that of the protruding structures; the passive film covers the doped semiconductor layer, and the passive film is further located in part of the pits; and the electrode penetrates through the passivation film to be in electric contact with the doped semiconductor layer, and the electrode is further located in part of the pit. According to the solar cell, the preparation method thereof and the photovoltaic module provided by the embodiment of the invention, the photoelectric conversion efficiency can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the photovoltaic field, and in particular to a solar cell and a method for preparing the same, and a photovoltaic module. Background Art

[0002] At present, with the gradual depletion of fossil energy, solar cells are becoming more and more widely used as a new energy alternative. Solar cells are devices that convert sunlight into electrical energy. Solar cells use the photovoltaic principle to generate carriers, and then use electrodes to lead the carriers out, thereby facilitating the effective use of electrical energy.

[0003] Solar cells generally include a passivation film, which can saturate surface dangling bonds and reduce interface states. x It can not only saturate the surface dangling bonds and reduce the interface state, but also reduce the minority carrier concentration in the front n-type silicon through its own positive charge, thereby reducing the surface recombination rate. x The hydrogen element carried in it can diffuse into the silicon wafer during the sintering process to passivate the emitter and the internal crystal defects of the silicon wafer.

[0004] However, the passivation film of the solar cell prepared in the current preparation process has residual stress, which can directly affect the adhesion of the passivation film to the substrate (the film layer covered by the passivation film). Excessive tensile stress or compressive stress can cause the passivation film to crack or warp, thereby affecting the passivation effect of the passivation film, and the photoelectric conversion efficiency of the solar cell is correspondingly reduced. Summary of the invention

[0005] The embodiments of the present application provide a solar cell and a method for preparing the same, and a photovoltaic module, which are at least beneficial to improving the photoelectric conversion efficiency of the solar cell.

[0006] According to some embodiments of the present application, on the one hand, the embodiments of the present application provide a solar cell, including: a substrate, the substrate having a first surface and a second surface arranged opposite to each other; the first surface having a velvet structure, the velvet structure including a convex structure; a doped semiconductor layer, the doped semiconductor layer being located on the first surface or the second surface, the doped semiconductor layer having a plurality of pits on a side away from the substrate, the size of the pits being smaller than the size of the convex structure; a passivation film, the passivation film covering the doped semiconductor layer, the passivation film also being located in part of the pits; an electrode, the electrode penetrating the passivation film and electrically contacting the doped semiconductor layer, the electrode also being located in part of the pits.

[0007] In some embodiments, the doped semiconductor layer having the pit is a first portion, and a ratio of a total area of ​​the first portion to an area of ​​the doped semiconductor layer is in a range of 5% to 80%.

[0008] In some embodiments, the material of the doped semiconductor layer includes polycrystalline silicon, single crystal silicon, nanocrystalline silicon, amorphous silicon, or microcrystalline silicon.

[0009] In some embodiments, the doped semiconductor layer has a thickness ranging from 10 nm to 200 nm.

[0010] In some embodiments, the size of the pit includes a one-dimensional size of the top surface, and the one-dimensional size of the top surface ranges from 5 nm to 100 nm.

[0011] In some embodiments, the depth of the pits ranges from 5 nm to 100 nm.

[0012] In some embodiments, the doped semiconductor layer includes a plurality of silicon grains, and the pits are formed at the boundaries between the silicon grains.

[0013] In some embodiments, the silicon grains are in a shape of flakes or blocks.

[0014] In some embodiments, the doped semiconductor layer includes a first doped conductive film and a second doped conductive film, the first doped conductive film is located on the velvet structure, and the second doped conductive film is located on the second surface; at least one of the first doped conductive film and the second doped conductive film has the pit.

[0015] In some embodiments, the doped semiconductor layer includes a first doped conductive film and a second doped conductive film, and the first doped conductive film and the second doped conductive film are alternately arranged on the second surface; at least one of the first doped conductive film and the second doped conductive film has the pit.

[0016] In some embodiments, the first doped conductive film is doped with one of an N-type doping element or a P-type doping element, and the second doped conductive film is doped with the other of the N-type doping element or the P-type doping element.

[0017] In some embodiments, a material of the first doped conductive film is different from a material of the second doped conductive film, and the second doped conductive film and the substrate have doping elements of the same conductivity type.

[0018] In some embodiments, a first dielectric layer is provided between the second doped conductive film and the second surface, and a second dielectric layer is provided between the first doped conductive film and the substrate.

[0019] In some embodiments, a material of at least one of the first dielectric layer or the second dielectric layer includes silicon oxide, amorphous silicon, microcrystalline silicon, nanocrystalline silicon, or silicon carbide.

[0020] In some embodiments, a thickness of the first doped conductive film is less than or equal to a thickness of the second doped conductive film.

[0021] According to some embodiments of the present application, on the other hand, the embodiments of the present application further provide a method for preparing a solar cell, comprising: providing a substrate, the substrate having a first surface and a second surface arranged opposite to each other; the first surface having a velvet structure, the velvet structure comprising a convex structure; forming a doped semiconductor layer, the doped semiconductor layer being located on the first surface or the second surface, the doped semiconductor layer having a plurality of pits on a side away from the substrate, the size of the pits being smaller than the size of the convex structure; forming a passivation film, the passivation film covering the doped semiconductor layer, the passivation film also being located in the pits; forming an electrode, the electrode penetrating the passivation film and being in electrical contact with the doped semiconductor layer, the electrode being located in the pits.

[0022] In some embodiments, the process steps for forming the doped semiconductor layer include: forming a semiconductor film on the surface of the substrate; performing doping treatment and activation treatment on the semiconductor film so that the semiconductor film is doped with N-type doping elements or P-type doping elements, and the surface of the semiconductor film has pits; the semiconductor film after the doping treatment and activation treatment is used as a doped semiconductor layer.

[0023] In some embodiments, the process steps of the doping treatment include: providing a doping source gas; and performing in-situ doping and diffusion treatment on the semiconductor film.

[0024] In some embodiments, the process parameters of the activation treatment include: a gas flow rate of 500 sccm to 5000 sccm; and a reaction temperature of 800° C. to 1000° C.

[0025] According to some embodiments of the present application, another aspect of the embodiments of the present application further provides a photovoltaic assembly, comprising: a cell string, which is formed by connecting a plurality of solar cells as described in the above embodiments or solar cells prepared by the method for preparing a solar cell as described in any one of the above embodiments through connecting components; a packaging layer for covering the surface of the cell string; and a cover plate for covering the surface of the packaging layer facing away from the cell string.

[0026] The technical solution provided by the embodiment of the present application has at least the following advantages:

[0027] In the solar cell provided in the embodiment of the present application, the doped semiconductor layer has a pit on the side away from the substrate, and the pit can increase the roughness of the doped semiconductor layer, thereby reducing the stress of the passivation film deposited on the surface of the doped semiconductor layer, and avoiding the problem of the passivation film bursting due to excessive stress. The pit can enhance the internal reflection of the incident light, thereby reducing the optical loss of the battery. If the electrode is located in part of the pit, the pit design can enhance the contact area between the electrode slurry and the doped semiconductor layer, thereby improving the contact performance between the doped semiconductor layer and the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] One or more embodiments are exemplarily illustrated by the figures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the figures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present application or the technical solutions in the traditional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 A schematic diagram of the structure of a solar cell;

[0030] Figure 2 It is a scanning electron microscope image of a doped semiconductor film in a solar cell and an optical microscope image of a passivation film;

[0031] Figure 3 A schematic structural diagram of a first solar cell provided in one embodiment of the present application;

[0032] Figure 4 for Figure 3 Schematic diagram of the first cross-sectional structure along the A1-A2 section;

[0033] Figure 5 for Figure 3 Schematic diagram of the second cross-sectional structure along the A1-A2 section;

[0034] Figure 6 for Figure 3 Schematic diagram of the third cross-sectional structure along the A1-A2 section;

[0035] Figure 7 A scanning electron microscope image of a doped semiconductor layer and an optical microscope image of a passivation film in a solar cell provided in one embodiment of the present application;

[0036] Figure 8 A partial structural diagram of a doped semiconductor layer in a solar cell provided in one embodiment of the present application;

[0037] Fig. 9 A schematic diagram of the structure of a second solar cell provided in one embodiment of the present application;

[0038] Fig.10 for Fig. 9 Schematic diagram of the first cross-sectional structure along the A1-A2 section;

[0039] Fig.11 for Fig. 9 Schematic diagram of the second cross-sectional structure along the A1-A2 section;

[0040] Fig.12 for Fig. 9 Schematic diagram of the third cross-sectional structure along the A1-A2 section;

[0041] Fig.13 A schematic structural diagram of a third solar cell provided in an embodiment of the present application;

[0042] Fig.14 for Fig.13 Schematic diagram of the first cross-sectional structure along the A1-A2 section;

[0043] Fig.15 for Fig.13 Schematic diagram of the second cross-sectional structure along the A1-A2 section;

[0044] Fig.16 A schematic structural diagram of a fourth solar cell provided in an embodiment of the present application;

[0045] Fig.17 for Fig.16 A schematic diagram of a cross-sectional structure along the A1-A2 section;

[0046] Fig.18 for Fig.16 An electron microscope image of the electrode area and the non-electrode area of ​​the corresponding solar cell;

[0047] Fig.19 for Fig.16 Another electron microscope image of the corresponding electrode area and non-electrode area in the solar cell;

[0048] Fig. 20 for Fig.16 A schematic diagram of a local structure of the third surface structure in the corresponding solar cell;

[0049] Fig.21 A schematic structural diagram of a fifth solar cell provided in an embodiment of the present application;

[0050] Fig. 22 for Fig.21 A schematic diagram of a cross-sectional structure along the B1-B2 section;

[0051] Fig.23 A schematic diagram of the structure of a photovoltaic module provided in another embodiment of the present application;

[0052] Fig.24 for Fig.23 Schematic diagram of the cross-sectional structure along the M1-M2 section. DETAILED DESCRIPTION

[0053] As can be seen from the background art, the photoelectric conversion efficiency of current solar cell structures is poor.

[0054] Analysis has found that one of the reasons for the poor photoelectric conversion efficiency of current solar cells is that Figure 1 is a schematic diagram of the structure of a solar cell, refer to Figure 1 The solar cell includes: an emitter 103 , a passivation layer 111 and a secondary grid 114 located on the front side 11 of the substrate 100 , and a dielectric layer 104 , a doped semiconductor film 121 , a passivation film 122 and an electrode 124 located on the back side 12 of the substrate. Figure 2 a is the surface morphology of the doped semiconductor film 121. Figure 2 a It can be seen that the surface of the doped semiconductor film 121 is relatively flat. The pyramid structure formed by the texturing process is left with a relatively low base after polishing, and the top of the pyramid has been etched away. Figure 2 b is the surface morphology of the passivation film 122. Figure 2 In b, it can be seen that the passivation film covers the doped semiconductor film and conforms to the tower base morphology on the back of the substrate in the surface morphology. Figure 2 It can be seen from b that the passivation film has a stress point 1220, and the stress of the passivation film 122 itself is relatively large. In the subsequent process steps, the passivation film 122 may burst on the surface or the passivation film 122 may be separated from the doped semiconductor film 121, and even lead to hydrogen passivation failure, abnormal appearance and other problems, thereby affecting the yield and photoelectric conversion efficiency of the solar cell.

[0055] One of the reasons why the passivation film has high stress is: 1. The difference in thermal expansion coefficients between the passivation film and the doped semiconductor film is large, that is, the deformation degree of the passivation film and the deformation degree of the doped semiconductor film cannot be offset, so that the deformation degree of the passivation film itself is large, and then compressive stress or tensile stress occurs. When the compressive stress or tensile stress exceeds the elastic limit of the passivation film itself, the passivation film may burst. 2. According to the thin film growth theory, the surface of the doped semiconductor film is in a relatively flat state. The passivation film first changes from the crystal nucleus to the island stage, and then develops into the network stage until the channel is filled and becomes a continuous film. In this process, the size of the grains used to form the passivation film is small, and the corresponding grain boundary area between the grains is also increased, and the stress is also increased accordingly.

[0056] The embodiment of the present application provides a solar cell, wherein the doped semiconductor layer has a pit on one side away from the substrate, and the pit can buffer the deformation difference caused by the difference in thermal expansion coefficient between the doped semiconductor layer and the passivation film, thereby buffering the stress of the passivation film, thereby reducing the defective rate of the passivation film. If the doped semiconductor layer has a pit, the grains constituting the passivation film will migrate relatively during the nucleation process, and gather and grow in the pit or near the pit, and the difficulty of developing in a network after forming an island shape increases, and it continues to agglomerate, forming a coarser grain agglomeration, thereby reducing the grain boundary area between the grains forming the passivation film, thereby reducing the stress. If the doped semiconductor layer has a pit, the roughness of the doped semiconductor layer increases accordingly, increasing the specific surface area of ​​the doped semiconductor layer, increasing the surface energy of the substrate surface, and improving the nucleation density of the passivation film on the heterogeneous doped semiconductor layer, while enhancing the adhesion between the passivation film and the doped semiconductor layer. Among them, "heterogeneous" means that the material of the passivation film is different from the material of the doped semiconductor layer, and has different characteristics such as energy band width, affinity energy and conduction band order.

[0057] In addition, the doped semiconductor layer has pits, and the pits are smaller than the size of the protruding structures, so the doped semiconductor layer itself will not have large defects or generate holes, so that the passivation film and the doped semiconductor layer are in close contact, thereby improving the adhesion and bonding strength between the doped semiconductor layer and the passivation film.

[0058] The pits can enhance the internal reflection of incident light, thereby reducing the optical loss of the battery. If the electrode is located in part of the pits, the pit design can enhance the contact area between the electrode slurry and the doped semiconductor layer, thereby improving the contact performance between the doped semiconductor layer and the electrode.

[0059] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0060] Figure 3 A schematic diagram of the structure of a solar cell provided in one embodiment of the present application; Figure 4 for Figure 3 Schematic diagram of the first cross-sectional structure along the A1-A2 section; Figure 5 for Figure 3 Schematic diagram of the second cross-sectional structure along the A1-A2 section; Figure 6 for Figure 3 Schematic diagram of the third cross-sectional structure along the A1-A2 section; Figure 7A scanning electron microscope image of a doped semiconductor layer and an optical microscope image of a passivation film in a solar cell provided in one embodiment of the present application; Figure 8 A partial structural diagram of a doped semiconductor layer in a solar cell provided in one embodiment of the present application.

[0061] refer to Figure 4 According to some embodiments of the present application, on the one hand, the embodiments of the present application provide a solar cell, including: a substrate 200, the substrate 200 having a first surface 21 and a second surface 22 arranged opposite to each other; the first surface 21 having a velvet structure 23, the velvet structure 23 including a protruding structure 201; a doped semiconductor layer 221, the doped semiconductor layer 221 is located on the second surface 22, and the doped semiconductor layer 221 has a plurality of pits 2210 on a side away from the substrate 200, and the size of the pits 2210 is smaller than the size of the protruding structure 201; a passivation film 222, the passivation film 222 covers the doped semiconductor layer 221, and the passivation film 222 is also located in part of the pits 2210; an electrode 224, the electrode 224 penetrates the passivation film 222 and is in electrical contact with the doped semiconductor layer 221, and the electrode 224 is also located in part of the pits 2210.

[0062] In some embodiments, the material of the substrate 200 may be an elemental semiconductor material. Specifically, the elemental semiconductor material is composed of a single element, such as silicon or germanium. The elemental semiconductor material may be in a single crystalline state, a polycrystalline state, an amorphous state, or a microcrystalline state (a state having both a single crystalline state and an amorphous state is referred to as a microcrystalline state), for example, silicon may be at least one of single crystalline silicon, polycrystalline silicon, amorphous silicon, or microcrystalline silicon.

[0063] In some embodiments, the material of the substrate 200 may also be a compound semiconductor material. Common compound semiconductor materials include but are not limited to silicon germanium, silicon carbide, gallium arsenide, indium gallium, perovskite, cadmium telluride, copper indium selenide, etc. The substrate 100 may also be a sapphire substrate, a silicon on insulator substrate, or a germanium on insulator substrate.

[0064] In some embodiments, the substrate 200 may be an N-type semiconductor substrate or a P-type semiconductor substrate. The N-type semiconductor substrate is doped with an N-type doping element, which may be any one of the V-group elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As). The P-type semiconductor substrate is doped with a P-type element, which may be any one of the III-group elements such as boron (B), aluminum (Al), gallium (Ga), or indium (In).

[0065] In some embodiments, the first surface 21 of the substrate 200 can be the front side and the second surface 22 can be the back side, or the first surface of the substrate can be the back side and the second surface can be the front side. The solar cell is a single-sided cell, the front side can be used as the light-receiving surface for receiving incident light, and the back side can be used as the backlight side. In some embodiments, the solar cell is a bifacial cell, that is, the first surface and the second surface of the substrate can both be used as the light-receiving surface, and can both be used to receive incident light. Among them, the backlight side can also receive incident light, but the efficiency of receiving incident light is weaker than the efficiency of receiving incident light by the light-receiving surface.

[0066] Figure 4-Figure 6 In the solar cell shown, the first surface of the substrate is the front surface, and the second surface of the substrate is the back surface. Figure 4-Figure 6 The solution of the solar cell shown is improved on the back side of the solar cell, and the doped semiconductor layer is located on the back side of the substrate, thereby improving the passivation performance of the back side of the solar cell. Figure 4-Figure 6 In the solar cell shown, the side of the substrate facing upward is used as the light-receiving side, and the side of the substrate facing downward is used as the backlight side.

[0067] refer to Figure 4 The solar cell further comprises: a first doped layer 203, the first doped layer 203 is located on the first surface 21 of the substrate 200, and a doped semiconductor layer 221 is located on the second surface 22 of the substrate 200. The solar cell comprises a passivation layer 211 and a secondary grid 214, the secondary grid 214 penetrates the thickness of the passivation layer 211 and is in electrical contact with the first doped layer 203.

[0068] In some embodiments, the first doping layer 203 and the substrate 200 are the same original substrate prepared by a doping process, the doping element in the first doping layer is one of an N-type doping element and a P-type doping element, and the doping element of the doped semiconductor layer 221 is the other of the N-type doping element and the P-type doping element.

[0069] In some embodiments, the substrate is an N-type substrate, the first doped layer is doped with P-type doping elements, and the doped semiconductor layer 221 is doped with N-type doping elements, then a PN junction is formed between the substrate and the first doped layer, the doping element concentration of the doped semiconductor layer 221 is greater than the doping element concentration of the substrate, and a high-low junction is formed between the substrate and the doped semiconductor layer 221.

[0070] In some embodiments, the material of the doped semiconductor layer 221 is the same as that of the substrate 200 , and the material of the doped semiconductor layer 221 may be crystalline silicon. Thus, there is no interface threshold difference between the doped semiconductor layer 221 and the substrate 20 , and the bonding force between the doped semiconductor layer 221 and the substrate is better.

[0071] In some embodiments, the substrate is an N-type substrate, the doped semiconductor layer 221 is doped with P-type doping elements, and the first doped layer 203 is doped with N-type doping elements, then a PN junction is formed between the substrate 200 and the doped semiconductor layer 221, the doping element concentration of the first doping layer 203 is greater than the doping element concentration of the substrate, and a high-low junction is formed between the substrate and the first doping layer.

[0072] refer to Figure 5 A tunnel dielectric layer 204 is provided between the doped semiconductor layer 221 and the second surface 22 , and the doped semiconductor layer 221 may be a doped polysilicon layer.

[0073] In some embodiments, a passivation contact structure is formed between the tunneling dielectric layer 204 and the doped polysilicon layer. The doped polysilicon layer can form an energy band bending on the surface of the substrate 200. The tunneling dielectric layer 204 causes an asymmetric shift in the energy band on the surface of the substrate 200, so that the potential barrier to the majority carriers (also called majority carriers) among the carriers is lower than the potential barrier to the minority carriers (also called minority carriers) among the carriers. Therefore, the majority carriers can more easily perform quantum tunneling through the tunneling dielectric layer 204, while the minority carriers find it difficult to pass through the tunneling dielectric layer 204, so as to realize the selective transmission of carriers.

[0074] In addition, the tunnel dielectric layer 204 has a chemical passivation effect. Specifically, due to the presence of interface state defects at the interface between the substrate 200 and the tunnel dielectric layer 204, the interface state density on the front side of the substrate 200 is relatively large. The increase in the interface state density promotes the recombination of photogenerated carriers, increases the fill factor, short-circuit current and open-circuit voltage of the solar cell, and improves the photoelectric conversion efficiency of the solar cell. The tunnel dielectric layer 204 is arranged on the first surface 21 of the substrate 200, so that the tunnel dielectric layer 204 has a chemical passivation effect on the surface of the substrate 200, specifically: by saturating the dangling bonds of the substrate 200, reducing the defect state density of the substrate 200, and reducing the recombination center of the substrate 200 to reduce the carrier recombination rate.

[0075] In some embodiments, the thickness of the tunneling dielectric layer 204 is 0.5 nm to 5 nm. The thickness of the tunneling dielectric layer 204 ranges from 0.5 nm to 1.3 nm, 1.3 nm to 2.6 nm, 2.6 nm to 4.1 nm, or 4.1 nm to 5 nm. When the thickness of the tunneling dielectric layer 204 is within any of the above ranges, the thickness of the tunneling dielectric layer 204 is thinner, and majority carriers can easily perform quantum tunneling through the tunneling dielectric layer 204, while minority carriers have difficulty passing through the tunneling dielectric layer 204, so as to achieve selective transmission of carriers.

[0076] The doped polysilicon layer has a field passivation effect. Specifically, an electrostatic field pointing to the inside of the substrate 200 is formed on the surface of the substrate 200, so that minority carriers escape from the interface, thereby reducing the minority carrier concentration, so that the carrier recombination rate at the interface of the substrate 200 is reduced, thereby increasing the open circuit voltage, short circuit current and fill factor of the solar cell, and improving the photoelectric conversion efficiency of the solar cell.

[0077] The doped polysilicon layer may be doped with the same type of doping elements as the substrate 200 . For example, the doping element type of the substrate 200 is N-type.

[0078] In some embodiments, the material of the tunnel dielectric layer 204 includes silicon oxide, amorphous silicon, microcrystalline silicon, nanocrystalline silicon, or silicon carbide.

[0079] refer to Figure 6 An intrinsic dielectric layer 205 and a doped amorphous silicon layer 206 are provided between the doped semiconductor layer 221 and the second surface 22. The doped semiconductor layer 221 is a transparent conductive layer, and the material of the transparent conductive layer can be at least one of indium tin oxide (or tin-doped indium oxide, Indium Tin Oxide abbreviated as ITO), aluminum-doped zinc oxide (AZO), cerium-doped indium oxide, and tungsten-doped indium oxide.

[0080] It should be noted that the doping element in the transparent conductive layer is not a P-type doping element or an N-type doping element, and the transparent conductive layer is an n-type semiconductor or a P-type semiconductor formed by a metal oxide doped with a metal.

[0081] In some embodiments, a heterojunction structure is formed between the intrinsic dielectric layer 205 and the substrate 200 . The intrinsic dielectric layer 205 can have a good passivation effect on the surface of the substrate 200 , which can greatly avoid the recombination of carriers and achieve a higher minority carrier lifetime and open circuit voltage.

[0082] In some embodiments, the material of the intrinsic dielectric layer 205 includes intrinsic amorphous silicon, intrinsic microcrystalline silicon, intrinsic silicon oxide, intrinsic nanocrystalline silicon or intrinsic silicon carbide. The thickness of the intrinsic dielectric layer 205 can be selected in a range of greater than or equal to 2 microns and less than or equal to 10 microns, preferably 5 microns. In some cases, due to the influence of the diffusion or doping process conditions of other film layers prepared subsequently, the intrinsic dielectric layer 205 may also include a small amount of doping elements, but the intrinsic dielectric layer with a small amount of doping elements is still regarded as an intrinsic dielectric layer.

[0083] In some embodiments, the thickness of the doped amorphous silicon layer 206 ranges from 4 to 30 nm. The thickness of the doped amorphous silicon layer 206 can range from 4 nm to 7.2 nm, 7.2 nm to 13 nm, 13 nm to 16.1 nm, 16.1 nm to 21 nm, 21 nm to 25 nm, or 25 nm to 30 nm.

[0084] In some embodiments, the material of the doped semiconductor layer 221 includes polycrystalline silicon, single crystal silicon, nanocrystalline silicon, amorphous silicon, or microcrystalline silicon.

[0085] In some embodiments, the thickness of the doped semiconductor layer 221 ranges from 10 nm to 200 nm, and the thickness of the doped semiconductor layer 221 ranges from 10 nm to 25 nm, 25 nm to 53 nm, 53 nm to 100 nm, 100 nm to 121 nm, 121 nm to 161 nm, or 161 nm to 200 nm. When the thickness of the doped semiconductor layer 221 is within any of the above ranges, the thickness of the doped semiconductor layer 221 is moderate, and the surface of the substrate 200 or the surface of part of the film layer can be covered, part of the morphology of the substrate 200 can be covered, and the roughness of the substrate 200 can be modified. In this way, the doped semiconductor layer 221 can have a certain passivation effect, thereby reducing the surface defects of the substrate 200. When the thickness of the doped semiconductor layer 221 is within the above range, the adhesion and bonding force between the doped semiconductor layer 221 and the passivation film 222 can also be improved to improve the film quality of the passivation film 222.

[0086] In some embodiments, when the thickness of the doped semiconductor layer 221 is within the above range, the thickness of the doped semiconductor layer 221 is relatively thin, the morphology of pits 2210 may exist between the silicon grains 2213 constituting the doped semiconductor layer 221, and the size and number of the pits 2210 may be controlled by adjusting the thickness of the doped semiconductor layer 221.

[0087] In some embodiments, Figure 7b is an optical microscope image of the surface of the passivation film 222. It can be seen from the 7b object that there are no stress points on the surface of the passivation film 222, which can explain that: the doped semiconductor layer 221 has a pit 2210 on the side away from the substrate 200, and the pit 2210 can buffer the deformation difference caused by the difference in thermal expansion coefficient between the doped semiconductor layer 221 and the passivation film 222, and then buffer the stress of the passivation film 222, so as to reduce the defect rate of the passivation film 222. If the doped semiconductor layer 221 has the pit 2210, the grains constituting the passivation film 222 will migrate relatively during the nucleation process, and gather and grow in the pit 2210 or near the pit 2210, and the difficulty of developing into an island-like and then a network-like shape increases, and they continue to agglomerate, forming a coarser grain agglomeration, thereby reducing the grain boundary area between the grains forming the passivation film 222, thereby reducing the stress. The doped semiconductor layer 221 has pits 2210, so the roughness of the doped semiconductor layer 221 increases accordingly, increasing the specific surface area of ​​the doped semiconductor layer 221, increasing the surface energy of the substrate 200, and improving the nucleation density of the passivation film 222 on the heterogeneous doped semiconductor layer 221, while enhancing the adhesion between the passivation film 222 and the doped semiconductor layer 221.

[0088] In addition, the doped semiconductor layer 221 has a pit 2210, and the pit 2210 is smaller than the size of the protruding structure 201, so the doped semiconductor layer 221 itself will not have large defects or generate holes, so that the passivation film 222 and the doped semiconductor layer 221 are in close contact, thereby improving the adhesion and bonding force between the doped semiconductor layer 221 and the passivation film 222.

[0089] The pit 2210 can enhance the internal reflection of the incident light, thereby reducing the optical loss of the battery. The electrode 224 is located in part of the pit 2210, and the pit 2210 design can enhance the contact area between the electrode slurry and the doped semiconductor layer 221, thereby improving the contact performance between the doped semiconductor layer 221 and the electrode 224.

[0090] In some embodiments, reference Figure 7a, the doped semiconductor layer 221 with the pits 2210 is the first part, and the ratio of the total area of ​​the first part to the area of ​​the doped semiconductor layer 221 is in the range of 5% to 80%. The ratio range can be 5% to 20%, 20% to 36%, 36% to 50%, 50% to 68%, 68% to 71% or 71% to 80%. If the ratio of the pits 2210 is within any of the above ranges or any values ​​within the range, the doped semiconductor layer 221 itself will not have many defects while ensuring that the doped semiconductor layer 221 has more pits 2210 to reduce the stress of the passivation film 222 and improve the contact performance between the doped semiconductor layer 221 and the electrode. In addition, if the ratio of the pits 2210 is within the above range, the void problem caused by the inability of the passivation film 222 to fill all the pits 2210 can be effectively avoided.

[0091] In some embodiments, reference Figure 7 a. The size of the pit 2210 includes a top surface one-dimensional size d, which ranges from 5nm to 100nm. The top surface one-dimensional size d can be 5nm to 18nm, 18nm to 32nm, 32nm to 50nm, 50nm to 73nm, 73nm to 86nm, or 86nm to 100nm.

[0092] In some embodiments, the depth of the pit 2210 ranges from 5 nm to 100 nm. The depth of the pit 2210 may be from 5 nm to 21 nm, from 21 nm to 44 nm, from 44 nm to 58 nm, from 58 nm to 69 nm, from 69 nm to 84 nm, or from 84 nm to 100 nm.

[0093] The value of the one-dimensional size d of the top surface is within any of the above ranges and the depth of the pit 2210 satisfies any one of the above ranges. By controlling the size of the pit 2210, it is possible to ensure that the pit 2210 is used to reduce the stress of the passivation film 222 while the film performance of the doped semiconductor layer 221 itself is better.

[0094] It should be noted that the pit 2210 does not penetrate the thickness of the doped semiconductor layer 221 , and the passivation film 222 can fill the pit 2210 or conformally cover the pit 2210 with a thickness less than the depth of the pit 2210 .

[0095] The one-dimensional size d of the top surface of the pit 2210 refers to the diameter of the top surface pattern, the distance between the two sides of the top surface pattern, or the distance between the two diagonal corners of the top surface pattern. The depth of the pit 2210 is the vertical distance between the bottom and the top of the pit 2210.

[0096] Continue to refer Figure 7a. The doped semiconductor layer 221 includes a plurality of silicon grains 2213 .

[0097] It is worth noting that in the process of forming the doped semiconductor layer 221, silicon atoms are arranged in a diamond lattice to form a plurality of crystal nuclei, which grow into crystal grains with different crystal plane orientations, and these crystal grains are combined to crystallize into the doped semiconductor layer. The silicon crystal grains 2213 refer to the crystal grains with different crystal plane orientations constituting the doped semiconductor layer 221.

[0098] In some embodiments, the grain size of the silicon grains 2213 ranges from 100 nm to 900 nm. The grain size of the silicon grains 2213 may be 100 nm to 250 nm, 250 nm to 360 nm, 360 nm to 490 nm, 490 nm to 5840 nm, 584 nm to 610 nm, 610 nm to 790 nm, or 790 nm to 900 nm. When the grain size of the silicon grains 2213 is within any of the above ranges, the grain boundaries between the silicon grains 2213 and the silicon grains 2213 are small, and the carriers can pass through the doped semiconductor layer 221 more easily, thereby increasing the carrier migration rate, which is beneficial to improving the battery efficiency.

[0099] Among them, the scale of grain size is called grain size. Commonly used methods of expression include the number of grains per unit volume (ZV), the number of grains per unit area (ZS) or the average linear length (or diameter) of the grains. The average linear length of the grains refers to the linear length of the extension surface of the extension direction of the grains. The grain size in the embodiments of the present application can be the average linear length of the grains.

[0100] In some embodiments, the shape of silicon grains 2213 includes flakes or blocks. Figure 7 The microscopic morphology of the silicon grain 2213 shown in a is flaky.

[0101] It should be noted that the shape of the silicon grain 2213 is observed by a test method with a magnification such as an electrical microscope or an optical microscope. The electrical microscope may include a conventional test method such as a scanning electron microscope (SEM) or an atomic force microscope (AFM). Figure 7 a is a microscopic morphology of silicon grains shown by a scanning electron microscope, from which it can be seen that the silicon grains are in the form of sheets extending in two dimensions.

[0102] In some embodiments, pits 2210 are provided at the junctions between silicon grains 2213 and silicon grains 2213. Thus, pits 2210 are located at the junctions between silicon grains, i.e., grain boundaries 2214. Compared with conventional solutions, the space between grain boundaries 2214 and grain boundaries 2214 is increased, and doping elements in doped semiconductor layer 221 can migrate through the space between grain boundaries and finally be collected by electrodes.

[0103] In some embodiments, the passivation film 222 may be a single-layer structure or a stacked-layer structure, and the material of the passivation film 222 may be one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride oxide, titanium oxide, hafnium oxide, or aluminum oxide. Figure 7 The passivation film 222 shown in b is an optical microscope image of the silicon nitride surface.

[0104] In some embodiments, the passivation layer 211 may be a single-layer structure or a stacked-layer structure, and the material of the passivation layer 211 may be one or more of silicon oxide, silicon nitride, silicon oxynitride, silicon carbonitride oxide, titanium oxide, hafnium oxide or aluminum oxide.

[0105] In some embodiments, the passivation film 222 and the passivation layer 211 are made of the same material, and the passivation film 222 and the passivation layer 211 can be prepared in the same process step.

[0106] In some embodiments, the spacing between the electrodes 224 along the first direction X ranges from 0.5 mm to 2 mm. The spacing between the electrodes 224 along the first direction X ranges from 0.5 mm to 0.8 mm, 0.8 mm to 1.15 mm, 1.15 mm to 1.28 mm, 1.28 mm to 1.46 mm, 1.46 mm to 1.68 mm, 1.68 mm to 1.84 mm, or 1.84 mm to 2 mm.

[0107] In some embodiments, the width of the electrode 224 along the first direction X ranges from 5um to 50um. The width of the electrode 224 along the first direction X ranges from 5um to 9um, 9um to 14um, 14um to 23um, 23um to 34um, 34um to 42um, 42um to 45um, 45um to 48um or 48um to 50um.

[0108] In some embodiments, the electrode 224 can be sintered by a burn-through paste. The method for forming the electrode 224 includes: printing a metal paste on a portion of the surface of the passivation film 222 using a screen printing process. The metal paste may include at least one of silver, aluminum, copper, tin, gold, lead or nickel. Then, the metal paste is subjected to a sintering process, and the metal paste contains a material with a highly corrosive component such as glass powder. In this way, during the sintering process, the corrosive component will corrode the passivation film 222, so that the metal paste penetrates into the passivation film 222 and is in electrical contact with the doped semiconductor layer.

[0109] In some embodiments, the orthographic projection of the secondary grid 214 on the second surface 22 overlaps with the orthographic projection of the electrode 224 on the second surface 22, the electrode 224 overlaps with the secondary grid 214 in a direction perpendicular to the second surface 22 of the substrate 200, and the spacing between the secondary grids 214 and the secondary grids 214 along the first direction X ranges from 0.5 mm to 2 mm. The width of the secondary grid 214 along the first direction X ranges from 5 um to 50 um.

[0110] In some embodiments, the auxiliary grid 214 can be sintered by a burn-through paste. The method for forming the auxiliary grid 214 includes: printing a metal paste on a surface of a portion of the passivation layer 211 using a screen printing process. The metal paste may include at least one of silver, aluminum, copper, tin, gold, lead or nickel. Then, the metal paste is subjected to a sintering process, and the metal paste contains a material with a highly corrosive component such as glass powder. In this way, during the sintering process, the corrosive component will corrode the passivation layer, so that the metal paste penetrates into the passivation layer 211 and is in electrical contact with the first doping layer 203.

[0111] In some embodiments, the material of the auxiliary gate 214 and the electrode 224 is the same, and the auxiliary gate 214 and the electrode 224 can be manufactured in the same process step.

[0112] In some embodiments, the first surface 21 is a surface with a concave-convex structure, which increases the internal reflection of incident light and improves the utilization rate of light by the solar cell, thereby improving the photoelectric conversion efficiency of the cell.

[0113] In some embodiments, the velvet structure 23 includes a plurality of protruding structures 101 , and the shapes of the protruding structures may include a pyramid shape, a parabola shape, or an ellipsoidal spherical shape.

[0114] Accordingly, Figure 3 to Figure 7 In the solar cell shown, the first surface is the front side, the second surface is the back side, and the doped semiconductor layer is located on the second surface. An embodiment of the present application also provides a solar cell, in which the first surface of the solar cell is the front side, the second surface is the back side, and the doped semiconductor layer is located on the first surface. The technical features that are the same or corresponding to the above embodiments will not be described in detail here.

[0115] Fig. 9 A schematic diagram of the structure of a second solar cell provided in one embodiment of the present application; Fig.10 for Fig. 9 Schematic diagram of the first cross-sectional structure along the A1-A2 section; Fig.11 for Fig. 9 Schematic diagram of the second cross-sectional structure along the A1-A2 section; Fig.12 for Fig. 9 Schematic diagram of the third cross-sectional structure along the A1-A2 section.

[0116] refer to Fig.10 The solar cell includes: a substrate 300, the substrate 300 has a first surface 31 and a second surface 32 that are opposite to each other; the first surface 31 has a velvet structure 33, and the velvet structure 33 includes a protruding structure 301; a doped semiconductor layer 321, the doped semiconductor layer 321 is located on the first surface 31, and the side of the doped semiconductor layer 321 away from the substrate 300 has a plurality of pits 3210, and the size of the pits 3210 is smaller than the size of the protruding structure 301; a passivation film 322, the passivation film 322 covers the doped semiconductor layer 321, and the passivation film 322 is also located in part of the pits 3210; an electrode 324, the electrode 324 penetrates the passivation film 322 and is in electrical contact with the doped semiconductor layer 321, and the electrode 324 is also located in part of the pits 3210.

[0117] In some embodiments, the doped semiconductor layer 321 covers the textured structure 33. The solar cell further includes: a passivation layer 311, which is located on the second surface 32 of the substrate; and a secondary grid 314, which penetrates the passivation layer 311 and is in electrical contact with the surface of the substrate 300.

[0118] In some embodiments, the material of the doped semiconductor layer 311 is the same as that of the substrate 300 , and the material of the doped semiconductor layer 311 may be crystalline silicon.

[0119] In some embodiments, the substrate is an N-type substrate, the doped semiconductor layer is doped with a P-type doping element, and the first doped layer is doped with an N-type doping element, and a PN junction is formed between the substrate and the doped semiconductor layer.

[0120] refer to Fig.11, a tunnel dielectric layer 304 is provided between the substrate 300 and the doped semiconductor layer 321, one of the N-type doping element or the P-type doping element is doped in the doped semiconductor layer 321, and the other of the N-type doping element or the P-type doping element is doped in the substrate 300. In this way, a PN junction is constructed between the doped semiconductor layer 321 and the substrate, and new hole-electron pairs are formed by the sun irradiating the PN junction. Under the action of the built-in electric field of the PN junction, the photogenerated holes flow to the p-region, and the photogenerated electrons flow to the n-region, and current is generated after the circuit is connected. The doped semiconductor layer 321 can be a doped polysilicon layer. A passivation contact structure is formed between the tunnel dielectric layer 304 and the doped polysilicon layer.

[0121] The description of the doped semiconductor layer 321 and the tunnel dielectric layer 304 can be found in Figure 5 The tunnel dielectric layer 204 and the doped semiconductor layer 221 are formed in the tunnel dielectric layer 204 and the doped semiconductor layer 221.

[0122] refer to Fig.12 An intrinsic dielectric layer 305 and a doped amorphous silicon layer 306 are provided between the doped semiconductor layer 321 and the first surface 31. The doped semiconductor layer 321 is a transparent conductive layer. The material of the transparent conductive layer can be at least one of indium tin oxide (or tin-doped indium oxide, Indium Tin Oxide abbreviated as ITO), aluminum-doped zinc oxide (AZO), cerium-doped indium oxide, and tungsten-doped indium oxide.

[0123] The relevant descriptions of the doped semiconductor layer 321, the intrinsic dielectric layer 305 and the doped amorphous silicon layer 306 can be referred to in Figure 6 The doped semiconductor layer 221, the intrinsic dielectric layer 205 and the doped amorphous silicon layer 206 are included in the embodiment of the present invention.

[0124] In some embodiments, the doped amorphous silicon layer and the substrate are doped with doping elements of different conductivity types, and a PN junction is formed between the doped amorphous silicon layer and the substrate. An intrinsic dielectric layer is inserted between the PN junction as a buffer layer, and the intrinsic dielectric layer has a good passivation effect on the surface of the substrate 300, which can greatly avoid the recombination of carriers and achieve a higher minority carrier lifetime and open circuit voltage.

[0125] For the above Figure 10-12 The substrate 300, the passivation layer 311, the auxiliary gate 314, the tunnel dielectric layer 304, the intrinsic dielectric layer 305, the intrinsic amorphous silicon layer 306, the electrode 324, the velvet structure 33, the doped semiconductor layer 321, the passivation film 322 and the pit 3210 can be referred to in Figure 3-Figure 6 The description of the substrate 200, the passivation layer 211, the auxiliary gate 214, the tunnel dielectric layer 204, the intrinsic dielectric layer 205, the intrinsic amorphous silicon layer 206, the electrode 224, the velvet structure 23, the doped semiconductor layer 221, the passivation film 222 and the pit 2210 are not repeated here.

[0126] Correspondingly, an embodiment of the present application also provides a solar cell, the doped semiconductor layer includes a first doped conductive film and a second doped conductive film, the first doped conductive film is located on the velvet structure, and the second doped conductive film is located on the second surface; at least one of the first doped conductive film and the second doped conductive film has pits, and the technical features that are the same or corresponding to the above-mentioned embodiments will not be described in detail here.

[0127] Fig.13 A schematic structural diagram of a third solar cell provided in an embodiment of the present application; Fig.14 for Fig.13 Schematic diagram of the first cross-sectional structure along the A1-A2 section; Fig.15 for Fig.13 Schematic diagram of the second cross-sectional structure along the A1-A2 section.

[0128] refer to Fig.14 The solar cell includes: a substrate 400, the substrate 400 has a first surface 41 and a second surface 42 that are opposite to each other; the first surface 41 has a velvet structure 43, and the velvet structure 43 includes a protruding structure 401; a doped semiconductor layer, the doped semiconductor layer is located on the first surface 41 and the second surface 42, and the doped semiconductor layer has a plurality of pits 4210 on a side away from the substrate 400, and the size of the pits 4210 is smaller than the size of the protruding structure 401; a passivation film 422, the passivation film 422 covers the doped semiconductor layer, and the passivation film 422 is also located in part of the pits 4210; an electrode, the electrode penetrates the passivation film 422 and is in electrical contact with the doped semiconductor layer, and the electrode is also located in part of the pits 4210.

[0129] refer to Fig.14 The doped semiconductor layer includes a first doped conductive film 4211 and a second doped conductive film 4212 . The first doped conductive film 4211 is located on the velvet structure 43 , and the second doped conductive film 4212 is located on the second surface 42 . At least one of the first doped conductive film 4211 and the second doped conductive film 4212 has a pit 4210 .

[0130] In some embodiments, the first doped conductive film 4211 is doped with one of an N-type doping element or a P-type doping element, and the second doped conductive film 4212 is doped with the other of the N-type doping element or the P-type doping element.

[0131] In some embodiments, a first dielectric layer 4041 is disposed between the second doped conductive film 4212 and the second surface 42 , and a second dielectric layer 4042 is disposed between the first doped conductive film 4211 and the substrate 200 .

[0132] In some embodiments, the material of at least one of the first dielectric layer 4041 or the second dielectric layer 4042 includes silicon oxide, amorphous silicon, microcrystalline silicon, nanocrystalline silicon, or silicon carbide.

[0133] In some embodiments, the first dielectric layer 4041 and the second dielectric layer 4042 may be tunnel dielectric layers. The first dielectric layer 4041 may refer to Fig.11 The tunnel dielectric layer 304 and the second dielectric layer 4042 can refer to Figure 5 Similarly, the first doped conductive film 4211 can refer to Fig.11 The doped semiconductor layer 321 in the second doped conductive film 4212 can refer to Figure 5 The doped semiconductor layer 221 in the embodiment of the present invention.

[0134] In some embodiments, the electrode includes a first electrode 4241 and a second electrode 4242, wherein the first electrode 4241 can refer to Fig.11 The electrode 324 in the second electrode 4242 can refer to Figure 5 The first passivation film 4221 can refer to Fig.11 The passivation film 322 in the figure and the second passivation film 4222 can refer to Figure 5 The passivation film 222 in the.

[0135] In some embodiments, the thickness of the first doped conductive film 4211 is less than or equal to the thickness of the second doped conductive film 4212. In this way, the average thickness of the first doped conductive film 4211 located on the front side is small, which can reduce the parasitic absorption of the first doped conductive film 4211 on the incident light irradiated to the front side; the average thickness of the second doped conductive film 4212 located on the back side is large, which can reduce the risk of the second electrode 4242 burning through the second doped conductive film 4212 due to the second doped conductive film 4212 being too thin, thereby reducing the risk of the P-type doping element diffusing into the substrate, thereby avoiding the problem of the P-type doping element of the second doped conductive film 4212 accumulating at the interface of the substrate to form a "dead layer", improving the transmission efficiency of carriers, and reducing the generation of carrier recombination centers.

[0136] In some embodiments, the material of the first doped conductive film 4211 is different from the material of the second doped conductive film 4212. For example, the first doped conductive film 4211 is a doped polysilicon layer, and the second doped conductive film 4212 is a transparent conductive layer. For another example, the first doped conductive film 4211 is a film layer of the same material as the substrate, and the second doped conductive film 4212 is a doped polysilicon layer or a transparent conductive layer.

[0137] refer to Fig.15The first doped conductive film 4211 is a doped polysilicon layer, the second doped conductive film 4212 is a transparent conductive layer, a tunneling dielectric layer 404 is provided between the first doped conductive film 4211 and the substrate, and an intrinsic dielectric layer 405 and a doped amorphous silicon layer 406 are provided between the second doped conductive film 4212 and the substrate 400.

[0138] In some embodiments, the second doped conductive film 4212 and the substrate have doping elements of the same conductive type, and the first doped conductive film 4211 and the substrate have doping elements of different conductive types. For example, the substrate is an N-type substrate, the second doped conductive film 4212 is doped with N-type doping elements, and the first doped conductive film 4211 is doped with P-type doping elements, that is, a PN junction is formed between the first doped conductive film 4211 and the substrate.

[0139] In some embodiments, the first doped conductive film 4211 and the substrate have doping elements of the same conductive type, and the second doped conductive film 4212 and the substrate have doping elements of a different conductive type. For example, the substrate is an N-type substrate, the first doped conductive film 4211 is doped with N-type doping elements, and the second doped conductive film 4212 is doped with P-type doping elements, that is, a PN junction is formed between the second doped conductive film 4212 and the substrate.

[0140] For the above Fig.15 The substrate 400, the tunnel dielectric layer 404, the intrinsic dielectric layer 405, the intrinsic amorphous silicon layer 406, the velvet structure 43, the first doped conductive film 4211, the second doped conductive film 4212, the first passivation film 4221, the second passivation film 4222 and the pit 4210 may correspond to the reference Figure 3-Figure 12 The description of the substrate 200, the passivation layer 211, the tunneling dielectric layer 204, the intrinsic dielectric layer 205, the intrinsic amorphous silicon layer 206, the velvet structure 23, the doped semiconductor layer 221, the doped semiconductor layer 321, the passivation film 222, the passivation film 322 and the pit 2210 are not repeated here.

[0141] Correspondingly, an embodiment of the present application also provides a solar cell, which includes an electrode area and a non-electrode area, and the doped conductive layer is located on the surface of the substrate corresponding to the electrode area. The technical features are the same or corresponding to the above embodiments and will not be repeated here.

[0142] Fig.16 A schematic structural diagram of a fourth solar cell provided in an embodiment of the present application; Fig.17 for Fig.16 A schematic diagram of a cross-sectional structure along the A1-A2 section; Fig.18 for Fig.16 An electron microscope image of the electrode area and the non-electrode area of ​​the corresponding solar cell; Fig.19 for Fig.16 Another electron microscope image of the corresponding electrode area and non-electrode area in the solar cell; Fig. 20 for Fig.16 Schematic diagram of the local structure of the third surface structure in the corresponding solar cell.

[0143] refer to Fig.17 The solar cell includes: a substrate 500, the substrate 500 has a first surface 51 and a second surface 52 that are opposite to each other; the first surface 51 has a velvet structure 53, and the velvet structure 53 includes a protruding structure 501; a doped semiconductor layer, the doped semiconductor layer is located on a portion of the first surface 51 and the second surface 52, and the doped semiconductor layer has a plurality of pits 5210 on a side away from the substrate 500, and the size of the pits 5210 is smaller than the size of the protruding structure 501; a passivation film, the passivation film covers the doped semiconductor layer, and the passivation film is also located in a portion of the pits 5210; an electrode, the electrode penetrates the passivation film and is in electrical contact with the doped semiconductor layer, and the electrode is also located in a portion of the pits 5210.

[0144] refer to Fig.16 The solar cell includes an electrode region 1 and a non-electrode region 2 which are alternately arranged, the doped semiconductor layer is located in the electrode region, and the passivation film is located in the electrode region 1 and the non-electrode region 2.

[0145] In some embodiments, the doped semiconductor layer includes a first doped conductive film 5211 located on the first surface and a second doped conductive film 5212 located on the second surface, a first dielectric layer 5041 is provided between the first doped conductive film 5211 and the substrate 500, and a second dielectric layer 5042 is provided between the second doped conductive film 5212 and the substrate. The passivation film includes a first passivation film 5221 covering the first doped conductive film 5211 and a portion of the surface of the substrate 500 and a second passivation film 5222 covering the second doped conductive film 5212, and the electrode includes a first electrode 5241 and a second electrode 5242, the first electrode 5241 is in electrical contact with the first doped conductive film 5211, and the second electrode 5242 is in electrical contact with the second doped conductive film 5212.

[0146] In some embodiments, electrode region 1 refers to the region in substrate 500 directly facing the electrode in the thickness direction of substrate 500, or can be understood as the region where the orthogonal projection of first electrode 5241 on substrate 500 is located or the region where the orthogonal projection of second electrode 5242 on substrate 500 is located. Conversely, the region in substrate 500 that is not directly facing the first electrode 5241 and the second electrode 5242 is non-electrode region 2. The area of ​​electrode region 1 is greater than or equal to the orthogonal projection of the first electrode 5241 on substrate 500 or the orthogonal projection of the second electrode 5242 on substrate 500, thereby ensuring that the region contacted by the first electrode 5241 or the second electrode 5242 is electrode region 1.

[0147] In some embodiments, the width of the electrode region is 1 to 5 times the width of the electrode. Excessive width of the electrode region may affect the integrity and uniformity of the film in the non-electrode region 1, reduce the internal reflection of light, and thus be detrimental to improving the carrier surface recombination rate and the photoelectric conversion efficiency of the solar cell. The mid-perpendicular line of the electrode region may overlap with the central axis of the secondary grid or deviate from the left and right by ±5%.

[0148] In some embodiments, reference Fig.17 The first surface 11 facing the electrode region 1 has a first surface structure 55 , and the first dielectric layer and the first doped conductive film cover the first surface structure 55 . The first surface 11 facing the non-electrode region 2 has a second surface structure 54 , and the first passivation film also covers the second surface structure 54 .

[0149] In some embodiments, the minimum distance between the first surface structure 55 and the second surface 52 is a first distance, the minimum distance between the second surface structure 54 and the second surface 52 is a second distance, and the first distance is smaller than the second distance.

[0150] The minimum distance between the first surface structure and the second surface refers to the distance between the bottom surface of the first surface structure and the second surface. The minimum distance between the second surface structure and the second surface refers to the distance between the bottom surface of the second surface structure and the second surface.

[0151] In some embodiments, the difference between the first distance and the second distance ranges from 0.5 to 10 um. The difference between the first distance and the second distance may be 0.5 to 2 um, 2 to 3.8 um, 3.8 to 6.9 um, 6.9 to 7.6 um, 7.6 to 8.3 um, or 8.3 to 10 um.

[0152] In some embodiments, reference Fig.17 The first surface structure 55 includes a plurality of first protruding structures 551 arranged at intervals. In practical applications, there is no restriction on the arrangement of the plurality of first protruding structures 551. Since the first dielectric layer and the first doped conductive film are relatively thin, the first dielectric layer and the first doped conductive film can reflect the morphology of the first protruding structures 551.

[0153] In some embodiments, reference Fig.17 The second surface structure 54 includes a plurality of second protruding structures 541 . In practical applications, there is no limitation on the arrangement of the plurality of second protruding structures 541 .

[0154] In some embodiments, at least one of the first surface structure 55 or the second surface structure 54 includes a platform protrusion structure or a pyramid velvet structure.

[0155] In some embodiments, reference Fig.18 or Fig.19 The surface of the substrate 500 also has a third surface structure 56 , and the third surface structure 56 is located at the junction of the non-electrode area 2 and the electrode area 1 .

[0156] refer to Fig.18 The third surface structure 56 has a plurality of third convex structures 562 arranged in an interlaced manner, and in addition to the discrete third convex structures 562, the third surface structure 56 also has a micro-convex structure 563, so that the incident light incident at different angles to the junction of the electrode area and the non-electrode area increases the probability of being absorbed by the substrate 500 through the third convex structure 562 and / or the micro-convex structure 563 after at least one reflection, and increases the probability of being reflected to the non-electrode area 2 through the third convex structure 562 and / or the micro-convex structure 563 after at least one reflection, and then absorbed by the non-electrode area 2, thereby facilitating the first surface 51 to have a higher absorption rate of the incident light. By improving the serious problem of carrier recombination in the electrode area 1 and increasing the absorption rate of the first surface 51 to the incident light, the photoelectric conversion efficiency of the solar cell is improved.

[0157] In some embodiments, the third surface structure 56 includes a prism structure, a pyramid structure, or a tetrahedron structure.

[0158] In some embodiments, reference Fig.18 or Fig.19 The micro-convex structure 563 includes at least one of a prism structure inclined toward the electrode region 1, a second pyramid structure, or a triangular plate structure.

[0159] It should be noted that Fig.18 as well as Fig.19 In the example, the micro-convex structure 563 includes a prism structure inclined toward the electrode region 1, a second pyramid structure, or a triangular plate structure. In practical applications, for the third surface structure 56 in the same area, the micro-convex structure 563 may include only one of the second pyramid structure, the triangular plate structure, or the prism structure inclined toward the electrode region 1, or any two of the three. In addition, in addition to being one of the prism structure inclined toward the electrode region 1, the second pyramid structure, or the triangular plate structure, the micro-convex structure 563 may also be an irregular granular structure.

[0160] The specific features of the prism structure are described in detail below.

[0161] In some embodiments, reference Fig.19, the prism structure is located on the side of the third protruding structure 562. The arrangement of the prism structure on the side of the third protruding structure 562 includes the following two situations: in some cases, one prism structure is located on the side of one third protruding structure 562; in other cases, multiple prism structures are attached to the same side of one third protruding structure 562, and each prism structure is in contact with and connected to the side.

[0162] In some other embodiments, continue to refer to Fig.19 , part of the prism structure is located on a part of the transition region 102 close to the electrode region 1. For example, the prism structure is located between the third protruding structure 562 and the electrode region 1.

[0163] In some other embodiments, the plurality of prism structures are arranged in sequence in a direction away from the side of the third protrusion structure 562. For example, only the prism structure closest to the side of the third protrusion structure 562 among the plurality of prism structures is in contact with the side of the third protrusion structure 562.

[0164] It should be noted that the multiple prismatic structures at the same intersection are at least at least one of the three prismatic structures in the above-mentioned embodiments, that is, the multiple prismatic structures at the same intersection can respectively have the characteristics of the prismatic structures in the three embodiments above-mentioned, or have the characteristics of the prismatic structures in any two of the above-mentioned embodiments, or have the characteristics of the prismatic structures in any one of the above-mentioned embodiments.

[0165] The specific features of the second pyramid structure are described in detail below.

[0166] In some embodiments, the bottom of the second pyramid structure is in contact with the bottom of the third protruding structure 562. In some cases, the bottom of the same third protruding structure 562 may be surrounded by multiple second pyramid structures, and the bottom of each second pyramid structure is in contact with the bottom of the third protruding structure 562.

[0167] In some other embodiments, at least one second pyramid structure is located between two adjacent third protruding structures 562. In other words, the bottom of the second pyramid structure will not be in contact with or connected to the bottom of the third protruding structure 562.

[0168] It should be noted that the second pyramid structure at the same junction is at least at least one of the second pyramid structures in the above two embodiments, that is, the multiple second pyramid structures at the same junction can respectively have the characteristics of the second pyramid structures in the above two embodiments, or have the characteristics of the second pyramid structure in any one of the above embodiments.

[0169] The specific features of the triangular plate structure are described in detail below.

[0170] In some cases, a triangular plate-like structure is located on a side of a third protruding structure 562; in other cases, a plurality of triangular plate-like structures are attached to the same side of a third protruding structure 562, and each triangular plate-like structure is in contact with and connected to the side.

[0171] In other embodiments, the plurality of triangular plate structures are arranged in sequence in a direction away from the side of the third protruding structure 562. For example, only the triangular plate structure closest to the side of the third protruding structure 562 among the plurality of triangular plate structures is in contact with the side of the third protruding structure 562.

[0172] It should be noted that the triangular plate-like structure at the same intersection is at least at least one of the triangular plate-like structures in the above two embodiments, that is, the multiple triangular plate-like structures at the same intersection can respectively have the characteristics of the triangular plate-like structures in the above two embodiments, or have the characteristics of the triangular plate-like structures in any one of the above embodiments.

[0173] In some embodiments, the third protruding structure 562 is located on a portion of the interface close to the non-electrode region 2. In other words, a portion of the interface close to the non-electrode region 2 has a more typical third protruding structure 562.

[0174] It should be noted that the third surface structure 56 at the junction is described above through various embodiments, that is, the structure of the third surface structure 56 is diverse. In some cases, not only does the same junction have a third convex structure 562 but also a plurality of micro-convex structures 563, but also the specific features of the plurality of micro-convex structures 563 at different junctions may be different, for example, one of two adjacent junctions has a prism structure inclined toward the electrode region 1 and a second pyramid structure, and the other has a second pyramid structure and a triangular plate structure.

[0175] refer to Fig. 20 The third protruding structure 562 includes a first side surface 5621 and a second side surface 5622 . The first side surface 5621 faces the electrode region 1 , and the dielectric layer 504 covers the first side surface 5621 . The second side surface 5622 faces the non-electrode region 2 . The radial length of the first side surface 5621 is smaller than the radial length of the second side surface 5622 .

[0176] In some embodiments, for the above Fig.17 The substrate 500, the first dielectric layer 5041, the second dielectric layer 5042, the texture structure 53, the first doped conductive film 5211, the second doped conductive film 5212, the first passivation film 5221, the second passivation film 5222, the first electrode 5241, the second electrode 5242 and the pit 5210 may correspond to the reference Fig.15The description of the substrate 400, the first dielectric layer 4041, the second dielectric layer 4042, the velvet structure 43, the first doped conductive film 4211, the second doped conductive film 4212, the first passivation film 4221, the second passivation film 4222, the first electrode 4241, the second electrode 4242 and the pit 4210 are not repeated here.

[0177] Correspondingly, an embodiment of the present application also provides a solar cell, the doped semiconductor layer includes a first doped conductive film and a second doped conductive film, the first doped conductive film and the second doped conductive film are alternately arranged on the second surface, and the technical features are the same or corresponding to the above embodiments, which will not be described in detail here.

[0178] Fig.21 A schematic structural diagram of a fifth solar cell provided in an embodiment of the present application; Fig. 22 for Fig.21 Schematic diagram of a cross-sectional structure along the B1-B2 section.

[0179] refer to Fig. 22 The solar cell includes: a substrate 600, the substrate 600 has a first surface 61 and a second surface 62 that are arranged opposite to each other; the first surface 61 has a velvet structure 63, and the velvet structure 63 includes a protruding structure 601; a doped semiconductor layer, the doped semiconductor layer is located on the second surface 62, and the doped semiconductor layer has a plurality of pits 6210 on a side away from the substrate 600, and the size of the pits 6210 is smaller than the size of the protruding structure 601; a passivation film 622, the passivation film 622 covers the doped semiconductor layer, and the passivation film 622 is also located in part of the pits 6210; an electrode, the electrode penetrates the passivation film 622 and is in electrical contact with the doped semiconductor layer, and the electrode is also located in part of the pits 6210.

[0180] In some embodiments, the doped semiconductor layer includes a first doped conductive film 6211 and a second doped conductive film 6212, and the first doped conductive film 6211 and the second doped conductive film 6212 are alternately arranged on the second surface; at least one of the first doped conductive film 6211 and the second doped conductive film 6212 has a pit.

[0181] In some embodiments, the substrate 100 has P regions and N regions that are spaced and alternately disposed.

[0182] In some embodiments, the first surface of the substrate has a front surface field (FSF), and the conductivity type of the doped ions is the same as the conductivity type of the doped ions of the substrate. The field passivation effect is used to reduce the surface minority carrier concentration, thereby reducing the surface recombination rate. At the same time, the series resistance can also be reduced and the electron transmission capacity can be improved.

[0183] In some embodiments, there is a non-electrode region 2 between the P region and the N region, and a passivation layer is located in the non-electrode region 2, wherein a groove 106 is formed between the P region and the N region to achieve automatic isolation between regions of different conductive types, thereby eliminating leakage caused by the tunnel junction formed by the heavily doped P region and N region on the back of the IBC battery, which affects the battery efficiency.

[0184] In some embodiments, the solar cell includes: a stacked first dielectric layer 6041 and a first doped conductive film 6211, the first dielectric layer 6041 is located on the back side, the first doped conductive film 6211 is located on the surface of the first dielectric layer 6041, and the first doped conductive film 6211 is doped with N-type doping elements; the first dielectric layer 6041 and the first doped conductive film 6211 are located on the surface of the substrate 600 in the N region.

[0185] In some embodiments, the solar cell includes: a stacked second dielectric layer 4042 and a second doped conductive film 4212122, the second dielectric layer 6042 is located on the back side, the second doped conductive film 6212 is located on the surface of the second dielectric layer 6042, and the second doped conductive film 6212 is doped with P-type doping elements; the second dielectric layer 6042 and the second doped conductive film 6212 are located on the substrate surface of the P region.

[0186] for Fig. 22 In the solar cell shown, in some embodiments, the first doped conductive film 6211 and the substrate are doped with doping elements of different conductivity types, a PN junction is formed between the first doped conductive film 6211 and the substrate, and the first doped conductive film 6211 serves as an emitter. In some embodiments, the second doped conductive film 6212 and the substrate are doped with doping elements of different conductivity types, a PN junction is formed between the second doped conductive film 6212 and the substrate, and the second doped conductive film 6212 serves as an emitter.

[0187] Accordingly, according to some embodiments of the present application, embodiment 1 of the present application also provides a method for preparing a solar cell, which can be used to prepare the solar cell provided by the above embodiments. The technical features that are the same as or corresponding to the above embodiments will not be repeated here.

[0188] Among them, Figure 5 The method for preparing a solar cell is shown as an example.

[0189] The preparation method comprises: providing a substrate, wherein the substrate comprises a first surface and a second surface which are arranged opposite to each other; the first surface comprises a velvet structure, and the velvet structure comprises a convex structure.

[0190] Specifically, it includes: providing an original substrate, and performing polishing treatment on two opposite sides of the original substrate, wherein the polishing treatment is used to reduce surface defects of the substrate.

[0191] In some embodiments, the original substrate includes electrode regions and non-electrode regions that are spaced apart.

[0192] The preparation method includes: performing a texturing treatment on one side of the original substrate so that a velvet structure is formed on one side of the original substrate, and then performing a diffusion treatment on one side of the velvet structure, wherein the portion of the original substrate that has been diffused serves as the first doping layer, and the remaining original substrate serves as the substrate, the side having the velvet structure and in contact with the first doping layer serves as the first surface, and the other side serves as the second surface. The texturing treatment includes: chemical etching, for example, a mixed solution of potassium hydroxide and hydrogen peroxide solution can be used to clean the substrate, and specifically, a velvet structure having an expected morphology can be formed by controlling the concentration ratio of potassium hydroxide and hydrogen peroxide solution. In some embodiments, the velvet structure can also be formed by laser etching, mechanical method, or plasma etching. In laser etching, the laser process parameters are controlled to obtain a velvet structure having an expected morphology.

[0193] In some embodiments, both sides of the original substrate are subjected to a velvet treatment, and then one side is subjected to a diffusion treatment, and the portion of the original substrate after the diffusion treatment serves as the first doping layer; the other side is subjected to a polishing treatment, and the remaining original substrate serves as the substrate, the side having a velvet structure and in contact with the first doping layer serves as the first surface, and the side subjected to the polishing treatment serves as the second surface.

[0194] The preparation method comprises: forming a tunnel dielectric layer on the second surface of the substrate.

[0195] In some embodiments, the tunnel dielectric layer is formed using a low pressure atomic layer deposition thin film growth technique.

[0196] The preparation method comprises: forming a doped semiconductor layer, the doped semiconductor layer covers the tunnel dielectric layer, the doped semiconductor layer has a plurality of pits on a side away from the substrate, and the size of the pits is smaller than the size of the protruding structure.

[0197] In some embodiments, the process steps for forming a doped semiconductor layer include: forming a semiconductor film on the surface of a substrate; performing doping treatment and activation treatment on the semiconductor film so that the semiconductor film is doped with N-type doping elements or P-type doping elements, and the surface of the semiconductor film has pits; and the semiconductor film after the doping treatment and activation treatment is used as a doped semiconductor layer.

[0198] In some embodiments, the process steps of forming a semiconductor film include: providing a first source gas, the first source gas is used to prepare the semiconductor film, and controlling the flow rate of the first source gas to be 100 sccm to 1000 sccm and the reaction temperature to be 500-650°C.

[0199] In some embodiments, the process steps of the doping treatment include: providing a doping source gas; and performing in-situ doping and diffusion treatment on the semiconductor film.

[0200] In some embodiments, process parameters of the activation treatment include: a gas flow rate of 500 sccm to 5000 sccm; and a reaction temperature of 800° C. to 1000° C.

[0201] Taking the formation of a doped polysilicon layer as an example, the process steps for forming the doped polysilicon layer include: using low pressure chemical vapor deposition (LPCVD) technology to form an amorphous silicon film on the surface of the tunnel dielectric layer, wherein the flow rate of the source gas silane used to form the amorphous silicon is controlled within 100 sccm to 1000 sccm and the reaction temperature is within 500-650°C.

[0202] Then, a doping source gas is provided to dope the amorphous silicon film, wherein the doping source gas may be POCL 3 During the doping process, the process parameters of the doping process are controlled to change the lattice arrangement between the doping elements and the amorphous silicon film, which is a pretreatment for the subsequent activation process.

[0203] The doping process and the formation of the semiconductor film can be performed in the same step, that is, in-situ doping is performed to form a doped amorphous silicon film.

[0204] Finally, an activation treatment is performed to transform the doped amorphous silicon film into a poly-Si (n+) structural state, and the surface of the transformed doped polysilicon layer has a pit structure.

[0205] The preparation method includes: forming a passivation film, the passivation film covers the doped semiconductor layer, and the passivation film is also located in the pit; forming an electrode, the electrode penetrates the passivation film and is in electrical contact with the doped semiconductor layer, and the electrode is located in the pit.

[0206] In some embodiments, a passivation layer may be formed on the surface of the first doping layer while the passivation film is formed. A secondary gate may be formed while the electrode is formed.

[0207] In some embodiments, during the process of forming an electrode, the doped semiconductor layer includes a plurality of silicon grains. When the silicon particles contact the conductive electrode, a Schottky contact or an Ohmic contact will be formed between the two. Under the action of a relatively low external negative voltage, electrons will overcome the interface barrier and be injected into the particle surface to attract positively charged protons, thereby inducing proton insertion into the lattice to form a polaron state, making the particle surface exhibit metal-like conductive properties. The resistance between the protonated particle layer and the unprotonated particle layer is greatly reduced, so that the particle surface protonation reaction can occur one particle at a time from bottom to top along the particle accumulation layer. The doped conductive layer has pits. By increasing the surface roughness of the doped conductive layer, the contact area between the conductive electrode and the nanoparticles can be increased, which is conducive to the occurrence of surface protonation. Particle surface protonation provides a direct electron transmission channel between particles, which is an effective way to electrically connect particles, thereby improving the carrier transmission efficiency, and also reducing the resistance between particles, greatly improving the electrode photocurrent.

[0208] Fig.23 A schematic diagram of the structure of a photovoltaic module provided in another embodiment of the present application; Fig.24 for Fig.23 Schematic diagram of the cross-sectional structure along the M1-M2 section.

[0209] Accordingly, according to some embodiments of the present application, some further embodiments of the present application provide a photovoltaic assembly, which may include the solar cell of the above embodiment, and the parts that are the same as the above embodiment will not be repeated in detail here.

[0210] refer to Fig.24 The photovoltaic module includes: a battery string, which is formed by connecting a plurality of solar cells 70 as in the above-mentioned embodiment or a solar cell 70 prepared by the method for preparing a solar cell in any one of the above-mentioned embodiments through a connecting component 709; an encapsulation layer 77 for covering the surface of the battery string; and a cover plate 78 for covering the surface of the encapsulation layer 77 away from the battery string.

[0211] Specifically, in some embodiments, a plurality of battery strings may be electrically connected via a connecting component 709 , and the connecting component 709 is welded to a main grid 708 on a battery cell.

[0212] In some embodiments, no intervals are set between the battery cells, that is, the battery cells overlap each other.

[0213] In some embodiments, the connection component 709 is welded to the secondary grid on the battery cell, and the secondary grid includes the secondary grid 714 and the electrode 724 .

[0214] In some embodiments, the encapsulation layer 77 includes a first encapsulation layer and a second encapsulation layer, the first encapsulation layer covers one of the front side or the back side of the solar cell, and the second encapsulation layer covers the other of the front side or the back side of the solar cell. Specifically, at least one of the first encapsulation layer or the second encapsulation layer can be an organic encapsulation film such as polyvinyl butyral (PVB) film, ethylene-vinyl acetate copolymer (EVA) film, polyethylene octene co-elastomer (POE) film or polyethylene terephthalate (PET) film.

[0215] It is worth noting that there is a boundary line between the first encapsulation layer and the second encapsulation layer before the lamination process. After the lamination process, the photovoltaic module is formed and there is no longer the concept of the first encapsulation layer and the second encapsulation layer, that is, the first encapsulation layer and the second encapsulation layer have formed an integral encapsulation layer 77.

[0216] In some embodiments, the cover plate 78 may be a glass cover plate, a plastic cover plate or the like with a light-transmitting function. Specifically, the surface of the cover plate 78 facing the encapsulation layer 77 may be a concave-convex surface, thereby increasing the utilization rate of the incident light. The cover plate 48 includes a first cover plate and a second cover plate, the first cover plate is opposite to the first encapsulation layer, and the second cover plate is opposite to the second encapsulation layer; or the first cover plate is opposite to one side of the solar cell, and the second cover plate is opposite to the other side of the solar cell.

[0217] Although the present application discloses the preferred embodiments as above, it is not intended to limit the claims. Any person skilled in the art can make several possible changes and modifications without departing from the concept of the present application. Therefore, the protection scope of the present application shall be based on the scope defined by the claims of the present application. In addition, the embodiments of the present application specification and the drawings shown are only examples and are not the full scope of the protection of the claims of the present application.

[0218] Those skilled in the art will appreciate that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present application, and therefore the scope of protection of the present application shall be subject to the scope defined in the claims.

Claims

1. A solar cell, characterized in that: include: A substrate having a first surface and a second surface that are oppositely disposed; The first surface has a suede structure, and the suede structure includes a convex structure; A doped semiconductor layer, the doped semiconductor layer is located on the first surface or the second surface, the doped semiconductor layer has a plurality of pits on a side away from the substrate, and the size of the pits is smaller than the size of the protruding structure; a passivation film, the passivation film covering the doped semiconductor layer, and the passivation film also being located in a portion of the pit; An electrode penetrates the passivation film and is in electrical contact with the doped semiconductor layer, and the electrode is also located in a portion of the pit.

2. The solar cell according to claim 1, characterized in that The doped semiconductor layer having the pit is a first portion, and a ratio of a total area of ​​the first portion to an area of ​​the doped semiconductor layer is in a range of 5% to 80%.

3. The solar cell according to claim 1, characterized in that The material of the doped semiconductor layer includes polycrystalline silicon, single crystal silicon, nanocrystalline silicon, amorphous silicon or microcrystalline silicon.

4. The solar cell according to claim 1, characterized in that The thickness of the doped semiconductor layer is in the range of 10 nm to 200 nm.

5. The solar cell according to claim 4, characterized in that: The size of the pit includes a one-dimensional size of the top surface, and the one-dimensional size of the top surface ranges from 5 nm to 100 nm.

6. The solar cell according to claim 4, characterized in that: The depth of the pits ranges from 5 nm to 100 nm.

7. The solar cell according to claim 1, characterized in that The doped semiconductor layer includes a plurality of silicon grains, and the pits are formed at the junctions between the silicon grains.

8. The solar cell according to claim 7, characterized in that: The silicon grains may be in a flake or block shape.

9. The solar cell according to claim 1, characterized in that: The doped semiconductor layer includes a first doped conductive film and a second doped conductive film, wherein the first doped conductive film is located on the velvet structure, and the second doped conductive film is located on the second surface; at least one of the first doped conductive film and the second doped conductive film has the pit.

10. The solar cell according to claim 1, characterized in that: The doped semiconductor layer includes a first doped conductive film and a second doped conductive film, and the first doped conductive film and the second doped conductive film are alternately arranged on the second surface; at least one of the first doped conductive film and the second doped conductive film has the pit.

11. The solar cell according to claim 9 or 10, characterized in that: The first doped conductive film is doped with one of an N-type doping element or a P-type doping element, and the second doped conductive film is doped with the other of the N-type doping element or the P-type doping element.

12. The solar cell according to claim 11, characterized in that: The material of the first doped conductive film is different from that of the second doped conductive film, and the second doped conductive film and the substrate have doping elements of the same conductivity type.

13. The solar cell according to claim 11, characterized in that: A first dielectric layer is provided between the second doped conductive film and the second surface, and a second dielectric layer is provided between the first doped conductive film and the substrate.

14. The solar cell according to claim 13, characterized in that: The material of at least one of the first dielectric layer or the second dielectric layer includes silicon oxide, amorphous silicon, microcrystalline silicon, nanocrystalline silicon or silicon carbide.

15. The solar cell according to claim 9, characterized in that: The thickness of the first doped conductive film is less than or equal to the thickness of the second doped conductive film.

16. A method for preparing a solar cell, characterized in that: include: Providing a substrate, wherein the substrate has a first surface and a second surface that are oppositely disposed; The first surface has a suede structure, and the suede structure includes a convex structure; forming a doped semiconductor layer, wherein the doped semiconductor layer is located on the first surface or the second surface, and a side of the doped semiconductor layer away from the substrate has a plurality of pits, and the size of the pits is smaller than the size of the protruding structure; forming a passivation film, wherein the passivation film covers the doped semiconductor layer and is also located in the pit; An electrode is formed, wherein the electrode penetrates the passivation film and is in electrical contact with the doped semiconductor layer, and the electrode is located in the pit.

17. The method for preparing a solar cell according to claim 16, characterized in that: The process steps of forming the doped semiconductor layer include: forming a semiconductor film on the surface of the substrate; The semiconductor film is doped and activated so that N-type doping elements or P-type doping elements are doped in the semiconductor film and the surface of the semiconductor film has pits; the semiconductor film after the doping and activation treatment serves as a doped semiconductor layer.

18. The method for preparing a solar cell according to claim 17, characterized in that: The process steps of the doping treatment include: providing doping source gas; and performing in-situ doping and diffusion treatment on the semiconductor film.

19. The method for preparing a solar cell according to claim 17, characterized in that: The process parameters of the activation treatment include: a gas flow rate of 500 sccm to 5000 sccm; and a reaction temperature of 800° C. to 1000° C.

20. A photovoltaic module, characterized in that: include: A battery string, formed by connecting a plurality of solar cells according to any one of claims 1 to 16 or a plurality of solar cells prepared by the method for preparing a solar cell according to any one of claims 17 to 19 through connecting components; An encapsulation layer, used to cover the surface of the battery string; The cover plate is used to cover the surface of the packaging layer facing away from the battery string.

Citation Information

Cited By

  • TOPCon battery film layer structure and preparation method thereof

    CN119562662A

  • A topcon cell film layer structure and a preparation method thereof

    CN119562662B

  • Solar cell, cell module and photovoltaic system

    CN120475819A

  • Solar cell and preparation method and equipment thereof, laminated cell and photovoltaic module

    CN122373538A

  • Solar cell and manufacturing method thereof

    EP4694630A3