Flexible thin-film solar cell and preparation method and application thereof

By introducing a multi-junction cascade structure and AlxGa1-xAs/AlyGa1-yAs DBR reflective layer into flexible thin-film solar cells, the problem of low photoelectric conversion efficiency of flexible thin-film solar cells is solved, and an increase of efficiency of more than 30% is achieved.

CN119008754APending Publication Date: 2024-11-22GUSU LAB OF MATERIALS
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411097807.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing flexible thin-film solar cells have the problem of low photoelectric conversion efficiency.

Method used

Using a multi-junction cascade structure and AlxGa1-xAs/AlyGa1-yAs DBR reflective layer, the reflectivity of the full spectrum of the sunlight is improved and the photoelectric conversion efficiency is improved.

Benefits of technology

The photoelectric conversion efficiency of flexible solar cells is achieved exceeding 30%, and the full spectrum of solar light reflection is realized through the adjustment of Al components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008754A_ABST
    Figure CN119008754A_ABST
Patent Text Reader

Abstract

The invention provides a flexible thin-film solar cell and a preparation method and application thereof. An epitaxial structure of the flexible thin-film solar cell comprises a GaAs substrate, a buffer layer, a corrosion barrier layer, a first contact layer, a window layer, an emission layer, a base layer, a back field layer, a DBR reflecting layer and a second contact layer which are sequentially stacked. The DBR reflecting layer comprises at least one group of Al < x > Ga < 1-x > As / Al < y > Ga < 1-y > As combined layers which are arranged in a laminated manner, and x and y are different in value. According to the flexible thin-film solar cell, by arranging the Al < x > Ga < 1-x > As / Al < y > Ga < 1-y > As DBR structure, the reflectivity of the full spectrum of sunlight can be improved, the performance of the flexible solar cell is enhanced, and the photoelectric conversion efficiency of the thin-film solar cell can exceed 30%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of solar cells and relates to a flexible thin-film solar cell and a preparation method and application thereof. Background Art

[0002] As one of the most effective clean energy sources, the weight-to-power ratio of solar cells has always been one of the concerns of photovoltaic panels, whether in space or on the ground. Flexible solar cells have also been an ideal target energy demand. In the current material system, III-V compound semiconductor solar cells have an absolute leading advantage in conversion efficiency. They also have the advantages of good high temperature resistance and strong radiation resistance. They are recognized as a new generation of high-performance and long-life space power sources.

[0003] At present, traditional III-V solar cells are epitaxially grown on InP, GaAs or Ge substrates. The rigid substrate accounts for more than 90% of the total mass of the solar cell, and the solar cell device is hard and fragile. Flexible III-V solar cells have excellent characteristics such as light weight, good bending performance and good specific power, which has opened up a new track for high-efficiency solar cells. If ultra-thin flexible materials are used instead of rigid materials as supporting substrates, III-V solar cells can be prepared into flexible devices.

[0004] For example, CN 113948598A discloses a flexible thin-film solar cell and a method for preparing the same, comprising: n-Al x Ga 1-x As single crystal; n-Al x Ga 1-x The upper and lower surfaces of the As single crystal are doped to form p + -Al x Ga 1-x As layer and n + -Al x Ga 1-x As layer, p + -Al x Ga 1-x The anti-reflection film, transparent conductive film and front electrode are formed on the As layer in sequence. + -Al x Ga 1-x An anti-reflection film, a transparent conductive film and a back electrode are sequentially formed on the As layer, and the front electrode and the back electrode are coated with polyester materials respectively. However, flexible thin-film solar cells have the problem of low photoelectric conversion efficiency.

[0005] Based on the above research, it is necessary to provide a flexible thin-film solar cell with a simple preparation method and high photoelectric conversion efficiency. Summary of the invention

[0006] The purpose of the present invention is to provide a flexible thin film solar cell and a preparation method and application thereof. The flexible thin film solar cell uses a semiconductor GaAs thin film material, is connected through a multi-junction cascade, and is provided with an Al x Ga 1-x As / Al y Ga 1-y The As DBR structure can improve the reflectivity of the full spectrum of sunlight, enhance the performance of the flexible solar cell, and enable the photoelectric conversion efficiency of the thin-film solar cell to exceed 30%.

[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0008] In a first aspect, the present invention provides a flexible thin-film solar cell, wherein the epitaxial structure of the flexible thin-film solar cell comprises a GaAs substrate, a buffer layer, a corrosion barrier layer, a first contact layer, a window layer, an emission layer, a base layer, a back field layer, a DBR reflective layer, and a second contact layer stacked in sequence;

[0009] The DBR reflective layer includes at least one set of stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where the values ​​of x and y are different.

[0010] A1 of the present invention x Ga 1-x As / Al y Ga 1-y As combination layer refers to the stacked Al x Ga 1-x As layer and Al y Ga 1-y As layer, this is a group of combined layers arranged in a stacked manner.

[0011] The present invention provides a DBR reflective layer in the epitaxial structure of a flexible thin-film solar cell, wherein the DBR reflective layer is Al x Ga 1-x As / Al y Ga 1-y As combination layer, and Al x Ga 1-x As and Al y Ga 1-yThe different Al component contents in As can realize reflection of low-energy photons, improve the reflectivity of most photons, and further improve the conversion efficiency of the flexible solar film. Even the reflection of the full spectrum of sunlight can be realized by adjusting the Al component. At the same time, the present invention provides a flexible thin-film solar cell. In order to match the flexible thin-film solar cell, the position of the DBR reflective layer of the present invention is set between the back field layer and the second contact layer, rather than the traditional setting close to the GaAs substrate side.

[0012] Preferably, the thickness of the DBR reflective layer is 1-2 μm, for example, 1 μm, 1.5 μm or 2 μm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0013] The thickness of the DBR reflective layer of the present invention will affect the reflectivity. If the thickness is too thin, it cannot function effectively. If it is too thick, it will be difficult to prepare and will also affect the stacking regularity of the reflective layer and the battery performance.

[0014] Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, the thickness of each layer is the same and is 1 / 4 of the central reflection wavelength of the DBR reflection layer.

[0015] Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, the carrier concentration of each layer is 1E 18 cm -3 ~1E 19 cm -3 , for example, it can be 1E 18 cm -3 , 2E 18 cm -3 , 5E 18 cm -3 ,8E 18 cm -3 or 1E 19 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the DBR reflective layer comprises n groups of stacked Al x Ga 1-x As / Al y Ga 1-yAs combined layer, wherein 10≤n≤30, for example, it can be 10, 15, 20, 25 or 30, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] The present invention preferably includes 10 to 30 groups of Al x Ga 1-x As / Al y Ga 1-y As combination layer, thereby promoting the realization of full spectrum reflection of the sun. If you want to improve the reflectivity of DBR, you need to increase the number of logarithmic growth layers. However, this will lead to an increase in the thickness of DBR, which will bring about greater series resistance, light absorption and thermal effects, but the growth process of thicker DBR is relatively difficult.

[0018] Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, x is 0.8 to 0.9, such as 0.8, 0.85 or 0.9, and y is 0.1 to 0.2, such as 0.1, 0.15 or 0.2, and the values ​​of x and y are different.

[0019] Preferably, the thickness of the GaAs substrate is 150-350 μm, for example, 150 μm, 200 μm, 250 μm, 300 μm or 350 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the buffer layer comprises a GaAs buffer layer.

[0021] Preferably, the GaAs buffer layer has a thickness of 300-400 nm, for example, 300 nm, 350 nm or 400 nm, and a carrier concentration of 1E 18 cm -3 ~3E 18 cm -3 , for example, it can be 1E 18 cm -3 , 2E 18 cm -3 or 3E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the corrosion barrier layer comprises an N-GaInP corrosion barrier layer.

[0023] Preferably, the thickness of the N-GaInP corrosion barrier layer is 200-400 nm, for example, 200 nm, 300 nm or 400 nm, and the carrier concentration is 2E 18 cm -3 ~1E 19 cm -3 , for example, it can be 2E 18 cm -3 , 5E 18 cm -3 or 1E 19 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the thickness of the N-GaInP corrosion barrier layer is 300 nm, and the Si doping concentration is 2E 18 cm -3 ~1E 19 cm -3 .

[0025] Preferably, the first contact layer comprises an N-GaAs contact layer.

[0026] Preferably, the thickness of the N-GaAs contact layer is 300-400 nm, for example, 300 nm, 350 nm or 400 nm, and the carrier concentration (Si doping concentration) is 5E 18 cm -3 ~9E 18 cm -3 , for example, it could be 5E 18 cm -3 , 6E 18 cm -3 , 7E 18 cm -3 ,8E 18 cm -3 or 9E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, the window layer comprises an N-InAlP window layer.

[0028] Preferably, the thickness of the N-InAlP window layer is 20-30 nm, for example, 20 nm, 25 nm or 30 nm, and the carrier concentration (Si doping concentration) is 1E 18 cm -3 ~3E 18 cm -3 , for example, it can be 1E 18 cm -3, 2E 18 cm -3 or 3E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the emission layer includes an N-GaAs emission region.

[0030] Preferably, the thickness of the N-GaAs emitter region is 50-100 nm, for example, 50 nm, 70 nm, 90 nm or 100 nm, and the carrier concentration (Si doping concentration) is 1E 18 cm -3 ~3E 18 cm -3 , for example, it can be 1E 18 cm -3 , 2E 18 cm -3 or 3E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the base layer comprises a P-GaAs base layer.

[0032] Preferably, the thickness of the P-GaAs base layer is 3-4 μm, for example, 3 μm, 4.5 μm or 4 μm, and the carrier concentration (C doping concentration) is 1E 17 cm -3 ~3E 17 cm -3 , for example, it can be 1E 17 cm -3 , 2E 17 cm -3 or 3E 17 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the back field layer comprises a P-AlGaAs back field layer.

[0034] Preferably, the thickness of the P-AlGaAs back field layer is 100-200 nm, for example, 100 nm, 150 nm or 200 nm, and the carrier concentration (C doping concentration) is 5E 17 cm -3 ~1E 18 cm -3 , for example, it could be 5E 17 cm -3 ,8E 17 cm-3 or 1E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the second contact layer comprises a GaAs contact layer.

[0036] Preferably, the thickness of the GaAs contact layer is 400-500 nm, for example, 400 nm, 450 nm or 500 nm, and the carrier concentration (C doping concentration) is 5E 18 cm -3 ~9E 18 cm -3 , for example, it could be 5E 18 cm -3 , 7E 18 cm -3 or 9E 18 cm -3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0037] In a second aspect, the present invention provides a method for preparing a flexible thin-film solar cell as described in the first aspect, the preparation method comprising the following steps:

[0038] The epitaxial structure is bonded to a flexible substrate, and then the GaAs substrate is peeled off to obtain the flexible thin-film solar cell.

[0039] The GaAs substrate in the epitaxial structure of the present invention is a rigid substrate. After the rigid GaAs substrate is stripped off by a wet method, a high-efficiency flexible solar cell can be obtained.

[0040] The epitaxial structure of the present invention is firstly evaporated with a P electrode and then electroplated with copper. Copper has good ductility and conductivity, and can be used as a support layer of the flexible solar cell and also as an extension of the back electrode. The next step is temporary bonding. The flexible substrate can be Si, glass or a flexible GaAs substrate. Then the original GaAs substrate is wet-etched to obtain an efficient flexible solar cell device.

[0041] Preferably, the epitaxial structure is prepared by MOCVD method.

[0042] Preferably, the method for preparing the epitaxial structure comprises the following steps:

[0043] (1) growing a buffer layer on a surface of a GaAs substrate at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0044] (2) continuing to grow a corrosion barrier layer on the surface of the buffer layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0045] (3) continuing to grow a first contact layer on the surface of the corrosion barrier layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0046] (4) continuing to grow a window layer on the surface of the first contact layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0047] (5) continuing to grow an emission layer on the surface of the window layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0048] (6) Continue to grow a base layer on the surface of the emission layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0049] (7) Continue to grow a back field layer on the surface of the base layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0050] (8) growing a DBR reflective layer on the surface of the back field layer at 600-700° C., for example, 600° C., 650° C. or 700° C.;

[0051] (9) Continue to grow a second contact layer on the surface of the DBR reflective layer at 600-700°C, for example, 600°C, 650°C or 700°C.

[0052] In a third aspect, the present invention provides an application of the flexible thin-film solar cell as described in the first aspect, wherein the application includes use in the automotive field or the aerospace field.

[0053] Compared with the prior art, the present invention has the following beneficial effects:

[0054] The present invention provides a DBR reflective layer in the epitaxial structure of a flexible thin-film solar cell, wherein the DBR reflective layer is Al x Ga 1-x As / Al y Ga 1-y As combination layer, and Al x Ga 1-x As and Al y Ga 1-yThe Al component content in As is different to reflect low-energy photons, thereby improving the reflectivity of most photons, so that the conversion efficiency of the flexible solar film is further improved, and even the reflection of the full spectrum of sunlight can be achieved by adjusting the Al component; at the same time, the rigid GaAs substrate is peeled off and the obtained film is flip-chip bonded on the flexible substrate to obtain a high-efficiency flexible solar cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] Figure 1 A schematic diagram of the epitaxial structure described in Example 1 of the present invention;

[0056] Among them, 1-GaAs substrate, 2-GaAs buffer layer, 3-N-GaInP corrosion barrier layer, 4-N-GaAs contact layer, 5-N-InAlP window layer, 6-N-GaAs emission layer, 7-P-GaAs base layer, 8-P-AlGaAs back field layer, 9-DBR reflection layer, 10-GaAs contact layer. DETAILED DESCRIPTION

[0057] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0058] Example 1

[0059] This embodiment provides a flexible thin-film solar cell, wherein the epitaxial structure of the flexible thin-film solar cell is as follows: Figure 1 As shown, it includes a GaAs substrate 1, a GaAs buffer layer 2, an N-GaInP corrosion barrier layer 3, an N-GaAs contact layer 4, an N-InAlP window layer 5, an N-GaAs emitter layer 6, a P-GaAs base layer 7, a P-AlGaAs back field layer 8, a DBR reflective layer 9 and a GaAs contact layer 10 stacked in sequence;

[0060] The DBR reflective layer 9 includes 20 stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where x is 0.9, y is 0.1, the thickness of each layer is the same and is 1 / 4 of the central reflection wavelength of the DBR reflection layer 9, and the carrier concentration of each layer is 3E 18 cm -3 , the thickness of the DBR reflective layer 9 is 2 μm;

[0061] The thickness of the GaAs substrate 1 is 250 μm, the thickness of the GaAs buffer layer 2 is 350 nm, and the carrier concentration is 2E 18 cm -3The thickness of the N-GaInP corrosion barrier layer 3 is 300 nm, and the carrier concentration is 2E 18 cm -3 The thickness of the N-GaAs contact layer 4 is 350nm, and the carrier concentration is 9E 18 cm -3 The thickness of the N-InAlP window layer 5 is 20 nm, and the carrier concentration is 2E 18 cm -3 The thickness of the N-GaAs emitter region 6 is 80 nm, and the carrier concentration is 2E 18 cm -3 The thickness of the P-GaAs base layer 7 is 3 μm, and the carrier concentration is 1E 17 cm -3 The thickness of the P-AlGaAs back field layer 8 is 150 nm, and the carrier concentration is 6E 17 cm -3 The thickness of the GaAs contact layer 10 is 500 nm, and the carrier concentration is 5E 18 cm -3 ;

[0062] The method for preparing the flexible thin-film solar cell comprises the following steps:

[0063] (1) growing an epitaxial structure by MOCVD, specifically growing a GaAs buffer layer 2 on a surface of a GaAs substrate 1 at 680° C.;

[0064] (2) Continue to grow an N-GaInP corrosion barrier layer 3 on the surface of the GaAs buffer layer 2 at 650° C.;

[0065] (3) Continue to grow an N-GaAs contact layer 4 on the surface of the N-GaInP corrosion barrier layer 3 at 650° C.;

[0066] (4) Continue to grow an N-InAlP window layer 5 on the surface of the N-GaAs contact layer 4 at 650° C.;

[0067] (5) Continue to grow an N-GaAs emission layer 6 on the surface of the N-InAlP window layer 5 at 650° C.;

[0068] (6) Continue to grow a P-GaAs base layer 7 on the surface of the N-GaAs emitter layer 6 at 650° C.;

[0069] (7) Continue to grow a P-AlGaAs back field layer 8 on the surface of the P-GaAs base layer 7 at 650° C.;

[0070] (8) Continue to grow a DBR reflective layer 9 on the surface of the P-AlGaAs back field layer 8 at 650° C.;

[0071] (9) Continue to grow a GaAs contact layer 10 on the surface of the DBR reflective layer 9 at 650° C.;

[0072] (10) P-type electrode evaporation, copper film electroplating, temporary substrate bonding, and etching of the original GaAs substrate are performed on the reverse epitaxial layer to obtain an effective flexible solar cell.

[0073] Example 2

[0074] This embodiment provides a flexible thin-film solar cell, wherein the epitaxial structure of the flexible thin-film solar cell comprises a GaAs substrate, a GaAs buffer layer, an N-GaInP corrosion barrier layer, an N-GaAs contact layer, an N-InAlP window layer, an N-GaAs emission layer, a P-GaAs base layer, a P-AlGaAs back field layer, a DBR reflective layer and an InGaAs contact layer stacked in sequence;

[0075] The DBR reflective layer includes 30 groups of stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where x is 0.9, y is 0.1, the thickness of each layer is the same and is 1 / 4 of the central reflection wavelength of the DBR reflection layer, and the carrier concentration of each layer is 1E 19 cm -3 , the thickness of the DBR reflective layer is 1 μm;

[0076] The thickness of the GaAs substrate is 350 μm, the thickness of the GaAs buffer layer is 300 nm, and the carrier concentration is 1E 18 cm -3 cm -3 The thickness of the N-GaInP corrosion barrier layer is 400nm, and the carrier concentration is 1E 19 cm -3 The thickness of the N-GaAs contact layer is 300nm and the carrier concentration is 5E 18 cm -3 The thickness of the N-InAlP window layer is 30 nm, and the carrier concentration is 1E 18 cm -3 The thickness of the N-GaAs emitter region is 100 nm, and the carrier concentration is 1E 18 cm -3 The thickness of the P-GaAs base layer is 4 μm, and the carrier concentration is 1E 17 cm -3 The thickness of the P-AlGaAs back field layer is 200 nm, and the carrier concentration is 5E 17 cm-3 The thickness of the InGaAs contact layer is 500nm and the carrier concentration is 9E 18 cm -3 ;

[0077] The method for preparing the flexible thin-film solar cell comprises the following steps:

[0078] (1) growing an epitaxial structure by MOCVD, specifically growing a GaAs buffer layer on a GaAs substrate at 700°C;

[0079] (2) Continue to grow an N-GaInP corrosion barrier layer on the surface of the GaAs buffer layer at 600°C;

[0080] (3) Continue to grow an N-GaAs contact layer on the surface of the N-GaInP corrosion barrier layer at 600°C;

[0081] (4) Continue to grow an N-InAlP window layer on the surface of the N-GaAs contact layer at 700°C;

[0082] (5) Continue to grow an N-GaAs emission layer on the surface of the N-InAlP window layer at 600°C;

[0083] (6) Continue to grow a P-GaAs base layer on the surface of the N-GaAs emitter layer at 700° C.;

[0084] (7) Continue to grow a P-AlGaAs back field layer on the surface of the P-GaAs base layer at 700° C.;

[0085] (8) Continue to grow a DBR reflective layer on the surface of the P-AlGaAs back field layer at 600°C;

[0086] (9) Continue to grow a GaAs contact layer on the surface of the DBR reflective layer at 600°C;

[0087] (10) P-type electrode evaporation, copper film electroplating, temporary substrate bonding, and etching of the original GaAs substrate are performed on the reverse epitaxial layer to obtain an effective flexible solar cell.

[0088] Example 3

[0089] This embodiment provides a flexible thin-film solar cell, wherein the epitaxial structure of the flexible thin-film solar cell comprises a GaAs substrate, a GaAs buffer layer, an N-GaInP corrosion barrier layer, an N-GaAs contact layer, an N-InAlP window layer, an N-GaAs emission layer, a P-GaAs base layer, a P-AlGaAs back field layer, a DBR reflective layer and an InGaAs contact layer stacked in sequence;

[0090] The DBR reflective layer includes 10 stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where x is 0.9, y is 0.1, the thickness of each layer is the same and is 1 / 4 of the central reflection wavelength of the DBR reflection layer, and the carrier concentration of each layer is 1E 18 cm -3 , the thickness of the DBR reflective layer is 3 μm;

[0091] The thickness of the GaAs substrate is 150 μm, the thickness of the GaAs buffer layer is 400 nm, and the carrier concentration is 3E 18 cm -3 The thickness of the N-GaInP corrosion barrier layer is 200nm, and the carrier concentration is 2E 18 cm -3 The thickness of the N-GaAs contact layer is 400nm and the carrier concentration is 9E 18 cm -3 The thickness of the N-InAlP window layer is 20 nm, and the carrier concentration is 3E 18 cm -3 The thickness of the N-GaAs emitter region is 50 nm, and the carrier concentration is 3E 18 cm -3 The thickness of the P-GaAs base layer is 3 μm and the carrier concentration is 3E 17 cm -3 The thickness of the P-AlGaAs back field layer is 100 nm, and the carrier concentration is 1E 18 cm -3 The thickness of the InGaAs contact layer is 400 nm and the carrier concentration is 5E 18 cm -3 ;

[0092] The method for preparing the flexible thin-film solar cell comprises the following steps:

[0093] (1) growing an epitaxial structure by MOCVD, specifically growing a GaAs buffer layer on a GaAs substrate at 600°C;

[0094] (2) Continue to grow an N-GaInP corrosion barrier layer on the surface of the GaAs buffer layer at 700°C;

[0095] (3) Continue to grow an N-GaAs contact layer on the surface of the N-GaInP corrosion barrier layer at 700°C;

[0096] (4) Continue to grow an N-InAlP window layer on the surface of the N-GaAs contact layer at 600°C;

[0097] (5) Continue to grow an N-GaAs emission layer on the surface of the N-InAlP window layer at 700°C;

[0098] (6) Continue to grow a P-GaAs base layer on the surface of the N-GaAs emitter layer at 600° C.;

[0099] (7) Continue to grow a P-AlGaAs back field layer on the surface of the P-GaAs base layer at 600° C.;

[0100] (8) Continue to grow a DBR reflective layer on the surface of the P-AlGaAs back field layer at 700° C.;

[0101] (9) Continue to grow a GaAs contact layer on the surface of the DBR reflective layer at 700°C.

[0102] (10) P-type electrode evaporation, copper film electroplating, temporary substrate bonding, and etching of the original GaAs substrate are performed on the reverse epitaxial layer to obtain an effective flexible solar cell.

[0103] Example 4

[0104] This embodiment provides a flexible thin-film solar cell. The flexible thin-film solar cell is the same as that of Embodiment 1 except that the thickness of the DBR reflective layer is 0.5 μm.

[0105] Example 5

[0106] This embodiment provides a flexible thin-film solar cell. The flexible thin-film solar cell is the same as that of Embodiment 1 except that the thickness of the DBR reflective layer is 3 μm.

[0107] Example 6

[0108] This embodiment provides a flexible thin film solar cell. In addition to the DBR reflective layer, the flexible thin film solar cell includes five stacked Al x Ga 1-x As / Al y Ga 1-y Except for the As combination layer, the rest is the same as that in Example 1.

[0109] Example 7

[0110] This embodiment provides a flexible thin film solar cell. In addition to the DBR reflective layer, the flexible thin film solar cell includes 35 stacked Al x Ga 1-x As / Aly Ga 1-y Except for the As combination layer, the rest is the same as that in Example 1.

[0111] Comparative Example 1

[0112] This comparative example provides a flexible thin-film solar cell, which is the same as Example 1 except that it does not contain a DBR reflective layer.

[0113] The flexible thin-film solar cells obtained in the above embodiments and comparative examples were tested for photoelectric conversion efficiency under the irradiation condition of AM1.5.

[0114] The test results are shown in Table 1:

[0115] Table 1

[0116] Photoelectric conversion efficiency (%) Example 1 30 Example 2 25.1 Example 3 27.8 Example 4 21.9 Example 5 24.7 Example 6 20.7 Example 7 22.1 Comparative Example 1 18.9

[0117] From Table 1 we can see that:

[0118] It can be seen from Example 1 and Comparative Example 1 that the flexible thin-film solar cell containing a DBR structure of the present invention can promote the reflection of the full spectrum of sunlight, thereby improving the photoelectric conversion efficiency; it can be seen from Example 1 and Examples 4-5 that the thickness of the DBR reflective layer of the present invention is within a reasonable range, which can further improve the photoelectric conversion efficiency of the flexible thin-film solar cell; it can be seen from Example 1 and Examples 6-7 that the growth period of the DBR reflective layer of the present invention, i.e., Al x Ga 1-x As / Al y Ga 1-y The number of As combination layers will affect the reflection efficiency and thus the photoelectric conversion efficiency of flexible thin-film solar cells.

[0119] In summary, the present invention provides a flexible thin-film solar cell and a preparation method and application thereof. The flexible thin-film solar cell uses a semiconductor GaAs thin film material, is cascaded through multiple junctions, and is configured with Al x Ga 1-x As / Al y Ga 1-y The As DBR structure can improve the reflectivity of the full spectrum of sunlight, enhance the performance of the flexible solar cell, and enable the photoelectric conversion efficiency of the thin-film solar cell to exceed 30%.

[0120] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A flexible thin-film solar cell, characterized in that: The epitaxial structure of the flexible thin-film solar cell comprises a GaAs substrate, a buffer layer, a corrosion barrier layer, a first contact layer, a window layer, an emission layer, a base layer, a back field layer, a DBR reflective layer and a second contact layer which are stacked in sequence; The DBR reflective layer includes at least one set of stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where x and y have different values.

2. The flexible thin-film solar cell according to claim 1, characterized in that: The thickness of the DBR reflective layer is 1-2 μm; Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, the thickness of each layer is the same; Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, the carrier concentration of each layer is 1E 18 cm -3 ~1E 19 cm -3 .

3. The flexible thin-film solar cell according to claim 1 or 2, characterized in that: The DBR reflective layer includes n groups of stacked Al x Ga 1-x As / Al y Ga 1-y As combination layer, where 10≤n≤30; Preferably, the Al x Ga 1-x As / Al y Ga 1-y In the As combination layer, x is 0.8-0.9, y is 0.1-0.2, and the values ​​of x and y are different.

4. The flexible thin-film solar cell according to any one of claims 1 to 3, characterized in that: The thickness of the GaAs substrate is 150-350 μm; Preferably, the buffer layer comprises a GaAs buffer layer; Preferably, the GaAs buffer layer has a thickness of 300-400 nm and a carrier concentration of 1E 18 cm -3 ~3E 18 -3 cm.

5. The flexible thin-film solar cell according to any one of claims 1 to 4, characterized in that: The corrosion barrier layer comprises an N-GaInP corrosion barrier layer; Preferably, the thickness of the N-GaInP corrosion barrier layer is 200-400 nm, and the carrier concentration is 2E 18 cm -3 ~1E 19 cm -3 ; Preferably, the first contact layer comprises an N-GaAs contact layer; Preferably, the thickness of the N-GaAs contact layer is 300-400 nm, and the carrier concentration is 5E 18 cm -3 ~9E 18 cm -3 ; Preferably, the window layer comprises an N-InAlP window layer; Preferably, the thickness of the N-InAlP window layer is 20-30 nm, and the carrier concentration is 1E 18 cm -3 ~3E 18 cm -3 .

6. The flexible thin-film solar cell according to any one of claims 1 to 5, characterized in that: The emission layer includes an N-GaAs emission region; Preferably, the thickness of the N-GaAs emitter region is 50-100 nm, and the carrier concentration is 1E 18 cm -3 ~3E 18 cm -3 ; Preferably, the base layer comprises a P-GaAs base layer; Preferably, the thickness of the P-GaAs base layer is 3-4 μm, and the carrier concentration is 1E 17 cm -3 ~3E 17 cm -3 .

7. The flexible thin-film solar cell according to any one of claims 1 to 6, characterized in that: The back field layer comprises a P-AlGaAs back field layer; Preferably, the thickness of the P-AlGaAs back field layer is 100-200 nm, and the carrier concentration is 5E 17 cm -3 ~1E 18 cm -3 ; Preferably, the second contact layer comprises a GaAs contact layer; Preferably, the thickness of the GaAs contact layer is 400-500 nm, and the carrier concentration is 5E 18 cm -3 ~9E 18 cm -3 .

8. A method for preparing a flexible thin-film solar cell according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The epitaxial structure is bonded to a flexible substrate, and then the GaAs substrate is peeled off to obtain the flexible thin-film solar cell.

9. The preparation method according to claim 8, characterized in that: The epitaxial structure is prepared by MOCVD method.

10. An application of the flexible thin-film solar cell according to any one of claims 1 to 7, characterized in that: The applications include use in the automotive sector or in the aerospace sector.

Citation Information

Patent Citations

  • Flexible thin-film solar cell and preparation method thereof

    CN113948598A