Red Micro LED chip and preparation method thereof

By forming polygonal star holes on the seed layer to release stress, the problem of insufficient In content in the InGaN quantum well is solved, the luminous efficiency and yield of the red Micro LED chip are improved, and an efficient production process is achieved.

CN119008794AActive Publication Date: 2024-11-22COSLIGHT YUANXIN (HANGZHOU) OPTOELECTRONICS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411098048.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-22
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

When preparing red LEDs, the In atoms in the epitaxially grown red light InGaN quantum well are large in volume and difficult to dopate, resulting in insufficient In content and the In content requirement of more than 35% cannot be achieved.

Method used

By forming a first opening of multiple polygonal star shapes on the seed layer, gradually reducing cross-sectional area and sharp bottom design, stress is released, and epitaxial growth is performed thereon, forming a red light emitting element layer, increasing the In atom Doping rate.

Benefits of technology

The high In content in InGaN quantum well is achieved, the luminescence efficiency and yield of the red Micro LED chip is improved, the production efficiency and controllability are ensured, and it is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008794A_ABST
    Figure CN119008794A_ABST
Patent Text Reader

Abstract

The invention discloses a red Micro LED chip and a preparation method thereof, and relates to the technical field of semiconductors, the red Micro LED chip comprises a substrate layer, a seed layer and a red light-emitting element layer, a plurality of first holes are formed in the seed layer, the cross section of each first hole is in a polygonal star shape, the cross section area of each first hole is gradually reduced from top to bottom, and the first holes are formed in the seed layer. The first opening is provided with a sharp bottom; a plurality of second openings which are in one-to-one correspondence with the first openings in position are formed in the red light-emitting element layer, and the first openings are arranged in multiple rows and multiple columns. The method has the advantages of being controllable in yield and high in production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a red Micro LED chip and a preparation method thereof. Background Art

[0002] When preparing red LEDs, epitaxial growth of red light InGaN quantum wells is a difficult point. The main reason is that In atoms are large in size, and when there is a large stress in the material system, it is difficult for In atoms to be doped into the quantum well. In related technologies, a maximum In content of 30% can be achieved. However, red LEDs require an In content of more than 35% to be realized.

[0003] Therefore, how to increase the In content in the InGaN quantum well has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention provides a red Micro LED chip and a preparation method thereof, which have the advantages of controllable yield and high production efficiency.

[0005] In order to achieve the above-mentioned purpose, as a first aspect of the present invention, a red Micro LED chip is provided, including a substrate layer, a seed layer and a red light-emitting element layer, wherein a plurality of first openings are formed on the seed layer, and the cross-section of the first openings is configured as a polygonal star, and the cross-sectional area of ​​the first openings gradually decreases from top to bottom, and the first openings have a pointed bottom; a plurality of second openings corresponding to the positions of the first openings are formed on the red light-emitting element layer, and the plurality of first openings are arranged in multiple rows and columns.

[0006] Optionally, the cross-section of the first opening is configured as a hexagonal star.

[0007] Optionally, the sidewall of the first opening is covered with a material for forming the red light emitting element layer.

[0008] Optionally, the first opening is filled with a dielectric material.

[0009] Optionally, the depth of the first opening is 200-1000 nm.

[0010] Optionally, the red light emitting element layer includes a superlattice layer, an n-type semiconductor layer, a barrier layer, a quantum well layer and a p-type semiconductor layer which are stacked in sequence, and the superlattice layer is formed on the seed layer.

[0011] As a second aspect of the present invention, a method for preparing a red Micro LED chip is provided, wherein the preparation method comprises:

[0012] providing a substrate layer;

[0013] forming a seed layer on the substrate layer;

[0014] forming a mask layer on the seed layer;

[0015] Patterning the mask layer to obtain a mask pattern having a plurality of circular openings;

[0016] Using the mask pattern as a mask, etching the seed layer to form a plurality of first openings on the seed layer, wherein the cross section of the first opening is a polygonal star shape, and the cross-sectional area of ​​the first opening gradually decreases from the top to the bottom, and the first opening has a pointed bottom, and the plurality of first openings are arranged in a plurality of rows and columns;

[0017] Epitaxial growth is performed on a side of the seed layer away from the substrate layer to obtain a red light emitting element layer.

[0018] Optionally, after the step of forming a plurality of first openings on the seed layer, the step further includes:

[0019] forming a dielectric material layer on a side of the seed layer away from the substrate layer;

[0020] The dielectric material outside the first opening is removed.

[0021] Optionally, the material of the dielectric material layer is selected from SiO2, SiN X , one or more of SiCN, SiOCN, and SiOC.

[0022] Optionally, the material of the mask layer is selected from one or more of SiO2, SiNX, SiCN, SiOCN, and SiOC.

[0023] Optionally, the etching the seed layer using the mask pattern as a mask includes:

[0024] Using the mask pattern as a mask, etching the seed layer with an etching solution; or

[0025] The seed layer is plasma etched using the mask pattern as a mask.

[0026] Optionally, the preparation method further comprises:

[0027] The prepared red light-emitting element layer is cut to obtain a Micro LED array.

[0028] In the present application, when preparing the Micro LED chip, a first opening for releasing stress is formed on the seed layer through an etching process. The size and density of the first opening are controllable, which is suitable for mass production of chips, and the yield of the manufactured chips is controllable. In addition, the first opening adopts a more regular array layout, so that the interface stress distribution is more uniform, and the accuracy and repeatability of each step of the process can be ensured during the manufacturing process, thereby improving production efficiency.

[0029] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. In addition, there are multiple features, elements, and components that appear in each of the following texts and drawings, and different symbols or numbers are marked for convenience, but they all represent components with the same or similar structures or functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The present invention will be further described below in conjunction with the accompanying drawings:

[0031] Figure 1 This is a schematic structural diagram of an implementation mode of a red Micro LED chip provided by the present invention;

[0032] Figure 2 A schematic diagram showing the shape of the first opening;

[0033] Figure 3 This is a schematic structural diagram of another implementation of the red Micro LED chip provided by the present invention;

[0034] Figure 4 A flow chart of an embodiment of the preparation method provided by the present invention;

[0035] Figure 5 A schematic diagram showing a mask pattern.

[0036] Among them, 1. substrate layer; 2. seed layer; 21. first opening; 3. red light emitting element layer; 31. second opening; 4. dielectric material; 5. mask layer. DETAILED DESCRIPTION

[0037] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0038] References in this specification to "one embodiment" or "an example" or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment of the present patent disclosure. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0039] V-type defects are a type of bulk defect that is common in GaN materials. They are mainly caused by factors such as lattice mismatch. Especially in the preparation process of LED epitaxial structure, due to the low growth temperature, the growth between layers is destroyed, and V-type defects are easily formed in the quantum well area. After the formation of this V-type defect, when the light-emitting element layer is formed, it can make it easier for In atoms to be incorporated into the quantum well, thereby generating red light.

[0040] However, the current technology uses a completely uncontrollable method to form V-shaped defects, resulting in uncontrollable size and density of the V-shaped defects. Therefore, it cannot be applied to large-scale mass production, and the yield of the Micro LED chips produced is uncontrollable.

[0041] In view of this, as a first aspect of the present invention, Figure 1 , Figure 2 and Figure 3 As shown, a red MicroLED chip is provided, including a substrate layer 1, a seed layer 2 and a red light-emitting element layer 3. A plurality of first openings 21 are formed on the seed layer 2. The cross-section of the first opening 21 is a polygonal star. From the top to the bottom, the cross-sectional area of ​​the first opening 21 gradually decreases, and the first opening 21 has a pointed bottom. A plurality of second openings 31 corresponding to the positions of the first openings 21 are formed on the red light-emitting element layer 3. In addition, the plurality of first openings 21 are arranged in multiple rows and columns.

[0042] In the embodiment of the present invention, the red light emitting element layer 3 is formed on the seed layer 2 by epitaxial growth.

[0043] Before the step of epitaxial growth, a plurality of first openings 21 with a polygonal star-shaped cross-section are formed on the seed layer 2, and each corner is a V-shaped defect to release the stress accumulated in the material system. The stress in the area where the first opening 21 is not formed on the seed layer 2 has been released, so that more In can be doped. Specifically, after the stress generated at the interface is released by the first opening 21 and the second opening 31, In atoms are more easily doped into the quantum well and grow InGaN materials with a high In content, thereby making the red Micro LED chip emit the required wavelength and efficiency of red light, emitting red light (wavelength of 620-625nm).

[0044] Because the first opening 21 is in the shape of a polygonal star, its formation process is easier to control. That is, when preparing the red Micro LED chip provided in the embodiment of the present invention, the number, position and density of V-shaped defects in the seed layer 2 are controlled by forming the first opening 21 in the shape of a polygonal star, so that the epitaxial growth process can be better controlled, the stress caused by the epitaxial growth can be reduced, the doping rate of In can be increased, and finally the yield of manufacturing red Micro LED chips can be improved.

[0045] The cross-section of the first opening 21 is designed to be a polygonal star. The polygonal star structure means that the edge of the first opening 21 has multiple vertices and edges, and the second opening 31 formed by epitaxial growth is also constructed to have multiple vertices and edges. This structure helps to disperse the stress to multiple points instead of concentrating it at a single location, further reducing stress concentration, thereby improving the quality and luminous efficiency of the red Micro LED chip.

[0046] A plurality of first openings 21 form a first opening 21 array, and a plurality of second openings 31 form a second opening 31 array, further enhancing the stress release effect. The first openings 21 in the present application also adopt a relatively regular array layout, so that the stress distribution is more uniform, and the accuracy and repeatability of each step of the process can be ensured during the manufacturing process, thereby improving the manufacturing efficiency and making it easier to mass produce red Micro LED chips.

[0047] In the embodiment of the present invention, there is no particular limitation on the specific shape of the first opening 21 , as long as the cross section thereof has a plurality of acute angles to form a V-shaped defect for relieving stress.

[0048] In the embodiment of the present invention, the first opening 21 can be formed on the seed layer 2 by an etching process. By controlling the process parameters during the etching process, different etching ratios can be achieved in different directions to form the first opening 21 on the seed layer 2.

[0049] Optionally, the material of the seed layer 2 may be a metal material or a semiconductor material, on which a hole with a hexagonal star cross section is easily formed. Therefore, as an optional embodiment, the cross section of the first opening 21 is a hexagonal star. It should be noted that the shape of the first opening 21 mainly depends on the material of the seed layer 2 and the determination of appropriate etching process conditions, and combined with real-time monitoring and feedback adjustment mechanism, a regular opening shape is prepared on the seed layer 2.

[0050] In the embodiment of the present invention, there is no special limitation on the type of material in the first opening 21. As an optional implementation, the sidewall of the first opening 21 is covered with a material for forming the red light emitting element layer 3. That is, after the first opening 21 is formed, the red light emitting element layer 3 is directly formed by an epitaxial growth process, thereby reducing the process difficulty and improving the efficiency of preparing the red light Micro LED.

[0051] like Figure 3 As shown, the material of the red light-emitting element layer will grow on the side wall of the first opening 21 and the top surface of the seed layer 2. However, during the epitaxial growth process, the growth rate of the side wall of the first opening 21 is much lower than the growth rate of the top surface of the seed layer 2. Therefore, the thickness of the red light-emitting element layer 3 grown on the side wall of the first opening 21 is much lower than the thickness of the red light-emitting element layer 3 grown on the top surface of the seed layer 2. The red light-emitting element layer 3 grown on the side wall of the first opening 21 can inject more holes into the quantum well, change the light-emitting angle, and reduce the influence of the total reflection angle on the light output, thereby improving the light-emitting efficiency and light-emitting intensity.

[0052] Of course, the embodiment of the present invention is not limited to this, and the material for forming the red light emitting element layer 3 may not be arranged in the first opening. Figure 1 As shown, the dielectric material 4 may be filled in the first opening 21 first.

[0053] In this embodiment, the first opening 21 is filled with a dielectric material 4, that is, the interior of the first opening 21 is occupied by the dielectric material 4. Therefore, the red light-emitting element layer 3 will not be able to grow in the first opening 21, but will grow on the plane (top surface) of the seed layer 2 not covered by the dielectric material 4. The resulting red Micro LED chip reduces leakage channels, improves electric field distribution, and improves device reliability.

[0054] How to fill the dielectric material 4 in the first opening 21 will be described below, and will not be described in detail here.

[0055] In the embodiment of the present invention, there is no special limitation on the depth of the first opening 21. Optionally, the depth of the first opening is between 200 nm and 10000 nm.

[0056] When the depth of the first opening 21 is less than 200nm, the hole injection path is limited, making it difficult for holes to be effectively transferred from the electrode to the light-emitting layer, thereby affecting the luminous efficiency and brightness of the chip. In addition, the shallower first opening 21 is not convenient for releasing the interface stress. When the depth of the first opening 21 is greater than 1000nm, the leakage path inside the chip is increased, making it easier for the current to pass through an unexpected path, resulting in leakage. The leakage phenomenon will directly affect the luminous efficiency and energy consumption of the chip, and may even damage the chip in severe cases.

[0057] In the embodiment of the present invention, the specific structure and material of the red light emitting element layer are not particularly limited. As an optional implementation, the red light emitting element layer includes a superlattice layer, an n-type semiconductor layer, a barrier layer, a quantum well layer and a p-type semiconductor layer stacked in sequence, and the superlattice layer is formed on the seed layer.

[0058] In the embodiment of the present invention, the substrate may be a sapphire substrate, a silicon carbide substrate, a silicon substrate, or the like.

[0059] In this embodiment, the superlattice layer is generally composed of thin layers of two or more different materials grown alternately, and the thickness of the thin layer is generally nanometer scale. This structure can introduce periodic potential barriers and potential wells to improve the injection efficiency and transmission characteristics of carriers. The n-type semiconductor layer is an electron-rich layer, which is mainly formed by donor impurity doping. In the LED, the n-type semiconductor layer serves as an electron injection layer, responsible for injecting electrons from the external circuit into the light-emitting area. This layer generally has a high electron mobility and a low resistivity to ensure that electrons can be efficiently transmitted to the quantum well layer. The barrier layer is generally located between the n-type semiconductor layer and the quantum well layer, or between the quantum well layers (if there are multiple quantum wells), and its main function is to limit the recombination of carriers (electrons and holes) in the quantum well layer, thereby improving the radiative recombination efficiency and reducing non-radiative recombination losses. The barrier layer has a higher band gap energy and can form a barrier to carriers, making it easier for them to recombine and emit light in the quantum well layer. The quantum well layer is the core light-emitting region, which is formed by a thinner semiconductor layer (usually a low band gap material) sandwiched between wider barrier layers. Due to the quantum size effect, the carriers (electrons and holes) in the quantum well layer are confined in a two-dimensional space, increasing the probability that they collide with each other and recombine to emit light. By adjusting the thickness, material and composition of the quantum well layer, the emission wavelength and spectral characteristics of the LED can be precisely controlled. The p-type semiconductor layer is a hole-rich layer, which is mainly formed by acceptor impurity doping. In the LED, the p-type semiconductor layer acts as a hole injection layer, responsible for injecting holes from the external circuit into the light-emitting area. Similar to the n-type semiconductor layer, the p-type semiconductor layer also needs to have a high hole mobility and a low resistivity to ensure that the holes can be efficiently transferred to the quantum well layer and recombine with electrons to emit light.

[0060] This embodiment of the present invention also provides a method for preparing a red Micro LED chip, such as Figure 4 As shown, the preparation method comprises:

[0061] In step S1, a substrate layer is provided;

[0062] In step S2, a seed layer is formed on the substrate layer;

[0063] In step S3, a mask layer is formed on the seed layer;

[0064] In step S4, the mask layer is patterned to obtain a mask pattern having a plurality of circular openings, and the seed layer is etched using the mask pattern as a mask to form a plurality of first openings on the seed layer, wherein the cross section of the first opening is a polygonal star shape;

[0065] In step S5, epitaxial growth is performed on a side of the seed layer away from the substrate layer to obtain a red light emitting element layer.

[0066] The preparation method can prepare the Micro LED chip provided by the first aspect of the present invention. As described above, because the first opening is a polygonal star, its formation process is easier to control, that is, when preparing the red Micro LED chip provided by the embodiment of the present invention, the number, position and density of V-shaped defects in the seed layer are controlled by forming the first polygonal star opening, so that the epitaxial growth process can be better controlled, and the doping rate of In can be increased, and finally the yield of manufacturing red Micro LED chips can be improved.

[0067] In the embodiment of the present invention, the substrate may be a sapphire substrate, a silicon substrate, a silicon carbide substrate, or the like.

[0068] In the embodiment of the present invention, the material of the seed layer is not particularly limited. The material of the seed layer can be a metal material such as copper, titanium, or a semiconductor material such as zinc oxide. The seed layer is the basis of epitaxial growth, and is usually a thin film prepared on the surface of the substrate layer by physical vapor deposition, chemical vapor deposition or other methods. The seed layer provides a starting point and guide for the subsequent growth of new crystal materials.

[0069] As an optional implementation, the material of the mask layer is SiO2. In other embodiments, the material of the mask layer may also be selected from SiN X , SiCN, SiOCN, SiOC or one or more thereof. The mask layer is used to isolate and protect a specific area in the seed layer. A corresponding process is selected according to the type of mask layer selected to form the mask layer on the seed layer.

[0070] In step S140, the mask layer may be patterned by a photolithography process to obtain a mask pattern having a plurality of circular openings. Specifically, an exposure machine may be selected to project the pattern to be produced onto the mask layer, or the desired pattern may be directly engraved on the mask layer by laser irradiation, and then a plurality of circular openings may be formed on the mask layer by an etching process. It should be noted that after the patterning is completed, the circular openings should penetrate the mask layer along the thickness direction of the mask layer, but the etching depth should also be controlled to avoid etching the seed layer.

[0071] like Figure 5As shown, the seed layer 2 is etched with the mask pattern as a mask, and a plurality of first openings 21 are formed on the seed layer 2 by precisely controlling the etching process parameters. Specifically, in this embodiment, the cross section of the first opening 21 is a hexagonal star, and in other embodiments, the cross section of the first opening 21 may also be other polygonal stars. In this embodiment, KOH is selected to perform wet etching on the seed layer 2. In other embodiments, one or more solutions of NaOH, NH3OH, DHF, BOE, HCl, and HNO3 may also be selected for wet etching. The area of ​​the seed layer 2 covered by the mask layer 5 will not be etched, but the area on the seed layer 2 corresponding to the circular opening of the mask layer 5 will still be in contact with the etching solution, so after wet etching, a plurality of first openings 21 with regular shapes corresponding to the circular opening positions of the mask layer 5 are formed on the seed layer 2.

[0072] Epitaxial growth is performed on the side of the seed layer 2 away from the substrate layer 1 to obtain a red light-emitting element layer 3. Epitaxial growth is to grow a single crystal film on the seed layer 2 (single crystal substrate), that is, the red light-emitting element layer 3 in this embodiment. The red light-emitting element layer 3 grows according to the crystal phase extension of the seed layer 2, and its crystal structure is an extension of the crystal structure of the seed layer 2. By selecting a substrate with a specific crystal direction and orientation, the epitaxial layer can be guided to grow in a specific direction. The crystal quality, thickness and uniformity of the seed layer 2 have an important influence on epitaxial growth. The seed layer 2 with good crystal quality can guide the new crystal material to grow in a specific direction to obtain high-quality crystals. In addition, growth parameters such as temperature, pressure, and atmosphere need to be precisely controlled to ensure that the growth rate and morphology of the crystal meet the requirements. For example, too high a temperature may lead to an increase in crystal defects, while too low a temperature may lead to a too slow growth rate. During the crystal growth process, measures need to be taken to reduce the introduction of impurities and defects. These impurities and defects may have an adverse effect on the electrical, optical and magnetic properties of the crystal.

[0073] In this embodiment, the substrate is a silicon substrate, and in other embodiments, the substrate may also be a sapphire substrate or a silicon carbide substrate.

[0074] After the step of forming a plurality of first openings on the seed layer, the method may further include: covering a dielectric material 4 on a side of the seed layer 2 away from the substrate layer 1 ; and removing the dielectric material 4 outside the first openings 21 .

[0075] In this embodiment, the dielectric material 4 is covered on the side of the seed layer 2 away from the substrate layer 1, and the dielectric material 4 in the non-opening area is removed by chemical mechanical polishing and other processes, and finally only the first opening 21 is filled with the dielectric material 4. Since the area covered with the dielectric material 4 cannot be subjected to the epitaxial growth process, the red light-emitting element layer 3 will not grow in the first opening 21.

[0076] In other embodiments, the seed layer 2 may not be covered with the dielectric material 4 , and in this case, the red light emitting element layer 3 may also be grown in the first opening 21 .

[0077] Specifically, the dielectric material 4 in this embodiment is made of SiO2. In other embodiments, the dielectric material 4 may also be selected from SiN X , one or more of SiCN, SiOCN, and SiOC.

[0078] The preparation method further includes cutting the prepared light-emitting element layer to obtain a Micro LED array. Using laser cutting and mechanical cutting methods to separate micro display chips can reduce production costs.

[0079] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A red Micro LED chip, comprising a substrate layer (1), a seed layer (2) and a red light-emitting element layer (3), characterized in that: A plurality of first openings (21) are formed on the seed layer (2), the cross-section of the first openings (21) is a polygonal star, and the cross-sectional area of ​​the first openings (21) gradually decreases from top to bottom, and the first openings (21) have a pointed bottom; a plurality of second openings (32) corresponding one-to-one to the positions of the first openings (21) are formed on the red light-emitting element layer (3), and the plurality of first openings (21) are arranged in a plurality of rows and columns.

2. The chip according to claim 1, characterized in that: The cross section of the first opening (21) is configured as a hexagonal star.

3. The chip according to claim 1, characterized in that: The side wall of the first opening (21) is covered with a material used to form the red light-emitting element layer (3).

4. The chip according to claim 1, characterized in that: The first opening (21) is filled with a dielectric material (4).

5. The chip according to any one of claims 1 to 4, characterized in that: The depth of the first opening (21) is 200-1000 nm.

6. The chip according to any one of claims 1 to 4, characterized in that: The red light emitting element layer includes a superlattice layer, an n-type semiconductor layer, a barrier layer, a quantum well layer and a p-type semiconductor layer which are stacked in sequence, and the superlattice layer is formed on the seed layer.

7. A method for preparing a red Micro LED chip, characterized in that: The preparation method comprises: providing a substrate layer; forming a seed layer on the substrate layer; forming a mask layer on the seed layer; Patterning the mask layer to obtain a mask pattern having a plurality of circular openings; Using the mask pattern as a mask, etching the seed layer to form a plurality of first openings on the seed layer, wherein the cross section of the first opening is a polygonal star shape, and the cross-sectional area of ​​the first opening gradually decreases from the top to the bottom, and the first opening has a pointed bottom, and the plurality of first openings are arranged in a plurality of rows and columns; Epitaxial growth is performed on a side of the seed layer away from the substrate layer to obtain a red light emitting element layer.

8. The preparation method according to claim 7, characterized in that: After the step of forming a plurality of first openings on the seed layer, the method further comprises: forming a dielectric material layer on a side of the seed layer away from the substrate layer; The dielectric material outside the first opening is removed.

9. The preparation method according to claim 8, characterized in that: The material of the dielectric material layer is selected from SiO2, SiN X , one or more of SiCN, SiOCN, and SiOC.

10. The preparation method according to any one of claims 7 to 9, characterized in that: The material of the mask layer is selected from one or more of SiO2, SiNX, SiCN, SiOCN, and SiOC.

11. The preparation method according to any one of claims 7 to 9, characterized in that: The step of etching the seed layer using the mask pattern as a mask comprises: Using the mask pattern as a mask, etching the seed layer with an etching solution; or The seed layer is plasma etched using the mask pattern as a mask.

12. The preparation method according to any one of claims 7 to 9, characterized in that: The preparation method further comprises: The prepared red light-emitting element layer is cut to obtain a Micro LED array.

Citation Information

Patent Citations

  • Composite substrate with isolating layer and manufacturing method of composite substrate

    CN103280425A

  • Composite substrate with isolation layer and manufacturing method thereof

    CN103413776A

  • Gallium nitride epitaxial structure

    CN216624314U

  • Method of manufacturing nitride semiconductor, nitride semiconductor device, method of manufacturing the same semiconductor light emitting device and its manufacturing method

    JP2002009004A

  • Semiconductor light emitting device, manufacturing method of the same and light emitting apparataus