Light emitting diode for improving electric leakage and preparation method thereof
By annealing the epitaxial layer under a nitrogen-free atmosphere, the leakage problem caused by water vapor corrosion of the light emitting diode is solved, the flatness of the groove side wall is improved, and the service life of the equipment is extended.
Patent Information
- Application Number
- CN202411023668.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-22
AI Technical Summary
During the working process, the passivation layer in the groove area is poorly dense, and it is prone to burst due to thermal expansion and contraction, causing water vapor to enter and corrode the active layer, resulting in leakage failure.
The epitaxial layer is annealed in an atmosphere without nitrogen and ammonia, which promotes the breaking and decomposition of the side walls of the grooves, improves the flatness of the side walls, and thus reduces the possibility of water vapor corrosion.
By increasing the flatness of the groove side walls, preventing water vapor from invading the active layer, significantly improving the leakage problem of the light-emitting diodes and extending their service life.
Smart Images

Figure CN119008800A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of optoelectronic manufacturing technology, and in particular to a light emitting diode with improved leakage current and a preparation method thereof. Background Art
[0002] Light Emitting Diode (LED) is an extremely influential new product in the optoelectronics industry. It has the characteristics of small size, long service life, rich colors and low energy consumption. It is widely used in lighting, display screens, signal lights, backlight sources, toys and other fields.
[0003] In the related art, a light emitting diode generally includes: an epitaxial layer, an electrode and a passivation layer, wherein the epitaxial layer includes an n-type layer, an active layer and a p-type layer stacked in sequence. The surface of the p-type layer has a groove exposing the n-type layer, the passivation layer is located on the surface of the p-type layer and in the groove, and the electrode is located on the surface of the passivation layer and is connected to the p-type layer and the n-type layer respectively through the through holes on the passivation layer.
[0004] Since the groove has a stepped corner area, the passivation layer stacked in the corner area has poor compactness. During the operation of the light-emitting diode, the passivation layer in the corner area is prone to cracking due to repeated thermal expansion and contraction, which in turn causes water vapor to enter and corrode the active layer, causing the light-emitting diode to leak and fail. Summary of the invention
[0005] The embodiments of the present disclosure provide a light-emitting diode with improved leakage current and a method for manufacturing the same, which can improve the problem of water vapor intruding into the active layer causing leakage current failure of the light-emitting diode. The technical solution is as follows:
[0006] On the one hand, an embodiment of the present disclosure provides a method for preparing a light-emitting diode, the preparation method comprising: forming an epitaxial layer, the epitaxial layer comprising a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, the second semiconductor layer having a groove exposing the first semiconductor layer; annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia.
[0007] Optionally, annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia includes: controlling the annealing temperature to be greater than or equal to 700°C, controlling the annealing pressure to be less than or equal to 500 torr, and controlling the atmosphere in the reaction chamber to include at least one of oxygen, hydrogen and inert gas to anneal the epitaxial layer.
[0008] Optionally, when the epitaxial layer is annealed in an atmosphere free of nitrogen and ammonia, the annealing time is controlled to be greater than or equal to 1 min.
[0009] Optionally, after annealing the epitaxial layer in an atmosphere without nitrogen and ammonia, the method further includes: annealing the epitaxial layer again in an atmosphere of ammonia and nitrogen.
[0010] Optionally, annealing the epitaxial layer again in an atmosphere of ammonia and nitrogen includes: controlling the annealing temperature to be 750° C. to 950° C., controlling the annealing pressure to be greater than 200 torr, and annealing the epitaxial layer.
[0011] Optionally, when the epitaxial layer is annealed again, the volume ratio of nitrogen and ammonia in the reaction chamber is controlled to be 0 to 5.
[0012] Optionally, when the epitaxial layer is annealed again in the atmosphere of ammonia and nitrogen, the annealing time is controlled to be greater than or equal to 3 minutes.
[0013] Optionally, after annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia, the method further includes: forming a passivation layer on the surface of the second semiconductor layer and in the groove, and forming through holes on the surface of the passivation layer to expose the second semiconductor layer and the first semiconductor layer respectively.
[0014] Optionally, forming the epitaxial layer includes: etching on the surface of the substrate to form a patterned structure, the patterned structure including at least one of a protrusion and a groove; and sequentially forming the first semiconductor layer, the active layer and the second semiconductor layer on the surface of the substrate.
[0015] On the other hand, an embodiment of the present disclosure also provides a light-emitting diode, which includes an epitaxial layer, the epitaxial layer includes a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, the second semiconductor layer has a groove exposing the first semiconductor layer; the roughness Ra of the groove wall is less than 0.05nm.
[0016] The beneficial effects brought by the technical solution provided by the embodiments of the present disclosure include at least:
[0017] The method for preparing a light-emitting diode provided by the embodiment of the present disclosure, after forming an epitaxial layer with a groove, annealing the epitaxial layer in an atmosphere without nitrogen and ammonia. Due to the etching of the epitaxial layer, there will be many cut atomic bonds on the side wall of the groove, so that the side wall of the groove has more randomly distributed broken bonds. When water vapor invades the passivation layer and enters the side wall of the groove, the randomly distributed broken bonds are more easily corroded by water vapor. Since the epitaxial layer is annealed in an atmosphere without nitrogen and ammonia, the broken bonds on the side wall of the groove can be decomposed, so that the randomly distributed broken bonds on the side wall of the groove are flatter, so as to improve the flatness of the side wall of the groove. The flatter side wall of the groove does not have more randomly distributed broken bonds on the surface. Therefore, even if water vapor invades the groove, it is not easy for water vapor to corrode the side wall of the groove, thereby improving the problem of water vapor invading the active layer and causing leakage failure of the light-emitting diode. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the technical solutions in the embodiments of the present disclosure, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0019] Figure 1 is a flow chart of a method for preparing a light emitting diode provided by an embodiment of the present disclosure;
[0020] Figure 2 is a flow chart of another method for preparing a light emitting diode provided by an embodiment of the present disclosure;
[0021] Figure 3 It is a structural schematic diagram of a light emitting diode provided in an embodiment of the present disclosure.
[0022] The descriptions of the marks in the figure are as follows:
[0023] 10. Substrate;
[0024] 20. epitaxial layer; 21. first semiconductor layer;
[0025] 22, active layer; 221, quantum barrier layer; 222, quantum well layer;
[0026] 23. A second semiconductor layer;
[0027] 30. Groove;
[0028] 40. Passivation layer;
[0029] 50. Electrode. DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present disclosure more clear, the embodiments of the present disclosure will be further described in detail below with reference to the accompanying drawings.
[0031] Figure 1 FIG. 1 is a flow chart of a method for preparing a light emitting diode provided by an embodiment of the present disclosure. Figure 1 As shown, the preparation method comprises:
[0032] Step 101: forming an epitaxial layer.
[0033] The epitaxial layer includes a first semiconductor layer, an active layer and a second semiconductor layer stacked in sequence, and the second semiconductor layer has a groove exposing the first semiconductor layer.
[0034] Step 102: Annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia.
[0035] The method for preparing a light-emitting diode provided by the embodiment of the present disclosure, after forming an epitaxial layer with a groove, annealing the epitaxial layer in an atmosphere without nitrogen and ammonia. Due to the etching of the epitaxial layer, there will be many cut atomic bonds on the side wall of the groove, so that the side wall of the groove has more randomly distributed broken bonds. When water vapor invades the passivation layer and enters the side wall of the groove, the randomly distributed broken bonds are more easily corroded by water vapor. Since the epitaxial layer is annealed in an atmosphere without nitrogen and ammonia, the broken bonds on the side wall of the groove can be decomposed, so that the randomly distributed broken bonds on the side wall of the groove are flatter, so as to improve the flatness of the side wall of the groove. The flatter side wall of the groove does not have more randomly distributed broken bonds on the surface. Therefore, even if water vapor invades the groove, it is not easy for water vapor to corrode the side wall of the groove, thereby improving the problem of water vapor invading the active layer and causing leakage failure of the light-emitting diode.
[0036] Figure 2 FIG. 1 is a flow chart of another method for preparing a light emitting diode provided by an embodiment of the present disclosure. Figure 2 As shown, the preparation method comprises:
[0037] Step 201: forming an epitaxial layer on a substrate.
[0038] The epitaxial layer includes a first semiconductor layer, an active layer and a second semiconductor layer stacked in sequence, and the second semiconductor layer has a groove exposing the first semiconductor layer.
[0039] Exemplarily, the substrate is a sapphire substrate, a silicon substrate or a silicon carbide substrate. The substrate can be a flat substrate or a patterned substrate.
[0040] As an example, in the embodiment of the present disclosure, the substrate is a sapphire substrate. The sapphire substrate is a commonly used substrate with mature technology and low cost. Specifically, it can be a patterned sapphire substrate or a sapphire flat sheet substrate.
[0041] In step 201, the substrate may be placed in a reaction chamber, the temperature in the reaction chamber may be controlled to grow to 1000° C. to 1200° C., hydrogen may be introduced into the reaction chamber, and the pressure in the reaction chamber may be controlled to be 150 torr to 250 torr for 5 to 10 minutes. This process may bake and clean the substrate surface and the graphite disk.
[0042] In step 201, the sapphire substrate may be pre-treated by placing the sapphire substrate in a MOCVD (Metal-organic Chemical Vapor Deposition) reaction chamber and baking the sapphire substrate for 12 to 18 minutes. As an example, in the embodiment of the present disclosure, the sapphire substrate is baked for 15 minutes.
[0043] Specifically, the baking temperature may be 1000° C. to 1200° C., and the pressure in the MOCVD reaction chamber during baking may be 100 mbar to 200 mbar.
[0044] It should be noted that the first semiconductor layer may also be grown on an AlN layer or a composite substrate, which is not limited in the embodiments of the present disclosure.
[0045] For example, when the first semiconductor layer is grown on the AlN layer, the thickness of the AlN layer can be controlled to be 160 angstroms to 220 angstroms.
[0046] Exemplarily, the AlN layer is deposited by magnetron sputtering using a physical vapor deposition (PVD) device.
[0047] The growth temperature in the PVD equipment is 400°C to 800°C, the sputtering power is 3000W to 5000W, the pressure is 1mtorr to 20mtorr, and the AlN layer deposition thickness is 10nm to 50nm.
[0048] In the embodiment of the present disclosure, before growing the epitaxial layer, the process may include: sequentially growing a nucleation layer and a non-doped GaN layer on the substrate.
[0049] Specifically, the method may include: first, placing the substrate coated with the buffer layer in an MOCVD system to grow a nucleation layer. The temperature of the MOCVD reaction chamber is 1030°C to 1100°C, the pressure of the reaction chamber is controlled at 150 torr to 500 torr, and the thickness of the nucleation layer is 0.3 μm to 2 μm under the mixed atmosphere of nitrogen, hydrogen and ammonia. Then, a non-doped GaN layer is grown on the nucleation layer.
[0050] In the embodiment of the present disclosure, an undoped GaN layer is also grown between the nucleation layer and the n-type layer. Compared with the substrate, since the crystal structure of the undoped GaN layer is similar to that of the n-type layer, the crystal quality of the subsequent epitaxial layer can be improved by providing the undoped GaN layer as a transition layer.
[0051] The thickness of the non-doped GaN layer is 0.5 μm to 3 μm. For example, the thickness of the non-doped GaN layer is 2 μm.
[0052] Specifically, the undoped GaN buffer recovery layer is grown by MOCVD. In an MOCVD system, the temperature is adjusted to 1000° C. to 1150° C., and the growth pressure is 100 Torr to 500 Torr, and a non-doped GaN layer with a thickness of 0.5 μm to 3 μm is grown.
[0053] Optionally, before preparing the epitaxial layer, the method may further include: etching the surface of the substrate to form a patterned structure, wherein the patterned structure includes at least one of a protrusion and a groove.
[0054] Illustratively, after a patterned structure is formed on the surface of the substrate, the epitaxial layer formed on the substrate will be more stable.
[0055] The specific process of preparing the epitaxial layer may include the following steps:
[0056] First, a first semiconductor layer is formed on a substrate, specifically by introducing TMGa and NH3 into a reaction chamber, using nitrogen and hydrogen as carrier gases, controlling the pressure in the reaction chamber to be 150 torr to 200 torr, and controlling the growth temperature to be 820° C. to 1140° C. to grow the first semiconductor layer.
[0057] Alternatively, the first semiconductor layer may be an n-type layer.
[0058] For example, the n-type layer may be an n-type GaN layer, the thickness of the n-type layer is 4 μm to 6 μm, and the dopant of the n-type layer is silane.
[0059] Specifically, in the MOCVD system, the temperature was adjusted to 1000°C and the growth pressure was 200 Torr. An n-type doped GaN layer with a thickness of 5 μm was grown. The concentration of Si doped in the n-type GaN layer was 1×10 18 cm -3 Up to 1×10 19 cm -3 .
[0060] For example, the flow rate of TMGa in the n-type layer may be controlled to be between 700 sccm and 2000 sccm.
[0061] Then, an active layer is formed on the surface of the first semiconductor layer.
[0062] Optionally, the active layer includes a plurality of quantum barrier layers and a plurality of quantum well layers stacked alternately.
[0063] The process of preparing the quantum barrier layer may include: introducing TMGa, TEGa, TMIn, and NH3 into the reaction chamber, using nitrogen and hydrogen as carrier gases, doping with SiH4, controlling the pressure in the reaction chamber to be 150 torr to 250 torr, controlling the growth temperature to be 800 °C to 910 °C, growing a GaN layer to obtain the quantum barrier layer.
[0064] Exemplarily, TMGa, TEGa, TMIn, and NH3 are introduced into the reaction chamber, nitrogen and hydrogen are used as carrier gases, doped with SiH4, the pressure in the reaction chamber is controlled to be 200 torr, the growth temperature is controlled to be 850 °C, and a GaN layer is grown to obtain the quantum barrier layer.
[0065] Exemplarily, the flow rate of TEGa may be 260 sccm to 330 sccm, and the flow rate of TMIn may be 800 sccm to 3000 sccm.
[0066] The process of preparing the quantum well layer may include: controlling the growth temperature to rise to 800 °C to 910 °C, growing an InGaN layer to obtain the quantum well layer.
[0067] Next, a second semiconductor layer is formed on the surface of the active layer.
[0068] Exemplarily, the second semiconductor layer may be a p-type layer.
[0069] Among them, the p-type layer includes a low-temperature p-type AlGaN layer, a p-type electron blocking layer, a high-temperature p-type GaN layer, and a p-type contact layer stacked in sequence on the active layer.
[0070] Exemplarily, the p-type electron blocking layer may be a p-type Al k Ga 1-k N(0.1 < k < 0.5) layer, and the thickness of the p-type electron blocking layer may be 10 nm to 100 nm.
[0071] In the embodiments of the present disclosure, both the low-temperature p-type AlGaN layer and the high-temperature p-type GaN layer are doped with Mg.
[0072] Exemplarily, the low-temperature p-type AlGaN layer includes Al w Ga 1-w N layer, 0.1 < w < 0.3.
[0073] The Mg doping concentration of the low-temperature p-type AlGaN layer is 5×10 20 cm -3 to 1×10 21 cm -3, the Mg doping concentration of the high-temperature p-type GaN layer is 1×10 18 cm -3 to 1×10 20 cm -3 .
[0074] Among them, the thickness of the low-temperature p-type AlGaN layer can be 10 nm to 100 nm. For example, the thickness of the low-temperature p-type AlGaN layer can be 80 nm.
[0075] Among them, the thickness of the high-temperature p-type GaN layer can be 10 nm to 100 nm. For example, the thickness of the low-high-temperature p-type GaN layer can be 50 nm.
[0076] When growing the low-temperature p-type AlGaN layer, adjust the growth temperature to 700 °C to 800 °C, and grow the low-temperature p-type AlGaN layer with a thickness of 10 nm to 100 nm under an environment where the growth pressure is 200 Torr to 500 Torr.
[0077] When growing the p-type electron blocking layer, adjust the growth temperature to 800 °C to 1000 °C, and under an environment where the growth pressure is 100 Torr to 300 Torr, the p-type electron blocking layer can be an Al k Ga 1-k N layer, where 0.2 < k < 0.5 and the thickness is 10 nm to 100 nm.
[0078] When growing the high-temperature p-type GaN layer, control the growth pressure to be in an environment of 200 Torr to 600 Torr, the growth temperature is 800 °C to 1000 °C, and grow a p-type GaN layer with a thickness of 10 nm to 100 nm.
[0079] When growing the p-type contact layer, control the growth temperature to be 850 °C to 1000 °C, control the growth pressure to be 100 Torr to 300 Torr, and grow a p-type contact layer with a thickness of 1 nm to 30 nm.
[0080] Among them, the Mg doping concentration in the p-type contact layer is 1×10 20 to 1×10 21 cm -3 .
[0081] Step 202: Anneal the epitaxial layer in an atmosphere without nitrogen and ammonia.
[0082] Specifically, it may include: controlling the annealing temperature to be greater than or equal to 700 °C, controlling the annealing pressure to be less than or equal to 500 torr, and controlling the atmosphere in the reaction chamber to include at least one of oxygen, hydrogen, and inert gas, and annealing the epitaxial layer.
[0083] Exemplarily, the atmosphere in the reaction chamber includes oxygen and hydrogen.
[0084] Annealing the epitaxial layer in this atmosphere can promote the decomposition of broken bonds on the side wall of the groove, thereby making the randomly distributed broken bonds on the side wall of the groove more flat, so as to improve the flatness of the side wall of the groove. Since there are not many randomly distributed broken bonds on the surface, even if water vapor invades the groove, it is not easy to corrode the side wall of the groove, thereby improving the problem of water vapor invading the active layer causing leakage failure of the light-emitting diode.
[0085] Exemplarily, the annealing temperature may be controlled to be 700°C to 800°C.
[0086] By setting the annealing temperature within the above range, the annealing temperature is relatively low. At a relatively low annealing temperature, the atomic bonds with relatively low bond energy and easy to break can be decomposed, so that during annealing, only the broken bonds on the sidewalls of the grooves are cleaned, and the internal materials of the active layer are not easily cleaned.
[0087] Exemplarily, the annealing pressure is controlled to be 450 torr.
[0088] Annealing is performed in an atmosphere free of nitrogen and ammonia. If the annealing pressure is too high, it will be detrimental to the decomposition of broken bonds. By controlling the annealing pressure within the above range, it is beneficial to decompose the broken bonds on the side walls of the groove.
[0089] Optionally, when the epitaxial layer is annealed in an atmosphere without nitrogen and ammonia, the annealing time is controlled to be greater than or equal to 1 minute. Too short an annealing time will affect the annealing effect, resulting in incomplete dissolution of the broken bonds on the sidewalls of the grooves.
[0090] Exemplarily, when annealing is performed in an atmosphere without nitrogen and ammonia, the annealing time is controlled to be 2 minutes.
[0091] Step 203: annealing the epitaxial layer again in an atmosphere of ammonia and nitrogen.
[0092] Through the first nitrogen-free and ammonia annealing, the broken bonds on the sidewalls of the grooves are dissolved, making the sidewalls of the grooves smoother. However, the surface chemical state of the sidewalls of the grooves is still very active. Therefore, after the surface of the sidewalls of the grooves is smoothed by the first nitrogen-free and ammonia annealing, the epitaxial layer is subjected to a second annealing treatment in an atmosphere of ammonia and nitrogen, using ammonia to make the surface chemical state of the active layer on the sidewalls of the grooves negative, making it difficult for the sidewalls of the grooves to decompose, improving the stability of the sidewalls of the grooves, and preventing the sidewalls of the grooves from being quickly corroded after water vapor intrusion.
[0093] In the embodiment of the present disclosure, the specific process of the second annealing may include: controlling the annealing temperature to be 750° C. to 950° C., controlling the annealing pressure to be greater than 200 torr, and annealing the epitaxial layer.
[0094] Illustratively, the annealing temperature is 850°C to 900°C.
[0095] During the second annealing, the annealing temperature is controlled to be higher, so that the surface lattice of the side wall of the groove is reorganized into a more stable chemical state, further improving the stability of the side wall of the groove to prevent the side wall of the groove from being corroded quickly after water vapor intrusion.
[0096] Exemplarily, the annealing pressure is 300 torr.
[0097] The annealing pressure is controlled within the above range to avoid the annealing pressure being too low, which may cause the active layer located on the side wall of the groove to be decomposed.
[0098] Optionally, when the epitaxial layer is annealed again, the volume ratio of nitrogen gas to ammonia gas in the reaction chamber is controlled to be 0 to 5.
[0099] Exemplarily, the volume ratio of nitrogen to ammonia is 1, that is, the volume of nitrogen and the volume of ammonia in the reaction chamber are equal.
[0100] In this way, a sufficient amount of nitrogen is filled in the reaction chamber, and ammonia is used to make the surface chemical state of the active layer located on the side wall of the groove more stable, making it difficult for the side wall of the groove to decompose, thereby improving the stability of the side wall of the groove to prevent the side wall of the groove from being quickly corroded after water vapor intrusion.
[0101] Optionally, when the epitaxial layer is annealed again in an atmosphere of ammonia and nitrogen, the annealing time is controlled to be greater than or equal to 3 minutes. Too short an annealing time will affect the annealing effect and make it difficult to stabilize the surface chemical state of the active layer on the sidewall of the groove, thereby making the sidewall of the groove easily decomposed.
[0102] Exemplarily, when annealing is performed in an atmosphere of ammonia and nitrogen, the annealing time is controlled to be 5 minutes.
[0103] Step 204: forming a passivation layer on the surface of the second semiconductor layer and in the groove, and forming through holes on the surface of the passivation layer that expose the second semiconductor layer and the first semiconductor layer respectively.
[0104] Exemplarily, the passivation layer may be a silicon oxide layer.
[0105] Exemplarily, the thickness of the silicon oxide layer may be 1 μm to 5 μm. Exemplarily, the thickness of the silicon oxide layer is 2 μm.
[0106] Step 205: forming at least two electrodes on the surface of the passivation layer.
[0107] Part of the electrode is located in the groove and connected to the first semiconductor layer, and another part of the electrode is located on the surface of the second semiconductor layer and connected to the second semiconductor layer.
[0108] Exemplarily, the electrode includes a first Al layer, a first Ti layer, a second Al layer, a second Ti layer, and an Au layer.
[0109] The thickness of the first Al layer is 8000 angstroms to 12000 angstroms, the thickness of the first Ti layer is 100 angstroms to 500 angstroms, the thickness of the second Al layer is 8000 angstroms to 12000 angstroms, the thickness of the second Ti layer is 500 angstroms to 1500 angstroms, and the thickness of the Au layer is 2000 angstroms to 5000 angstroms.
[0110] For example, the thickness of the first Al layer is 10000 angstroms, the thickness of the first Ti layer is 200 angstroms, the thickness of the second Al layer is 10000 angstroms, the thickness of the second Ti layer is 1000 angstroms, and the thickness of the Au layer is 3000 angstroms.
[0111] Figure 3 Schematic diagram of the structure of a light emitting diode provided by an embodiment of the present disclosure. Figure 3 As shown, the light emitting diode includes an epitaxial layer 20, which includes a first semiconductor layer 21, an active layer 22 and a second semiconductor layer 23 stacked in sequence, and the second semiconductor layer 23 has a groove 30 exposing the first semiconductor layer 21; the roughness Ra of the groove wall of the groove 30 is less than 0.05nm.
[0112] In the disclosed embodiment, after the epitaxial layer 20 is prepared, the epitaxial layer 20 is annealed in an atmosphere free of nitrogen and ammonia, which can promote the decomposition of the broken bonds on the side wall of the groove 30, thereby making the randomly distributed broken bonds on the side wall of the groove 30 more flat, so that the roughness Ra of the groove wall of the groove 30 is less than 0.05nm, so as to improve the flatness of the side wall of the groove 30. The flatter side wall of the groove 30 does not have many randomly distributed broken bonds on the surface, so even if water vapor invades the groove 30, it is not easy to corrode the side wall of the groove 30, thereby improving the problem of water vapor invading the active layer 22 and causing leakage failure of the light-emitting diode.
[0113] Alternatively, if Figure 3 As shown, the light emitting diode further includes a substrate 10 , and an epitaxial layer 20 is located on the surface of the substrate 10 .
[0114] Exemplarily, the substrate is a sapphire substrate, a silicon substrate or a silicon carbide substrate. The substrate can be a flat substrate or a patterned substrate.
[0115] Optionally, the active layer 22 includes a plurality of quantum barrier layers 221 and a plurality of quantum well layers 222 that are alternately stacked.
[0116] Optionally, the quantum barrier layer 221 may be a GaN layer, and the quantum well layer 222 may be an InGaN layer.
[0117] In the implementation of the present disclosure, the first semiconductor layer 21 may be an n-type layer, and the second semiconductor layer 23 may be a p-type layer.
[0118] Optionally, the n-type layer may be an n-type GaN layer. The thickness of the n-type layer is 2 μm to 6 μm.
[0119] Among them, the dopant of the n-type layer is silane, and the concentration of doped silane may be 5×10 18 cm -3 to 5×10 19 cm -3 .
[0120] Optionally, the p-type layer further includes a low-temperature p-type AlGaN layer, a p-type electron blocking layer, a high-temperature p-type GaN layer, and a p-type contact layer, and the low-temperature p-type AlGaN layer, the p-type electron blocking layer, the high-temperature p-type GaN layer, and the p-type contact layer are sequentially stacked on the active layer 22.
[0121] Exemplarily, the p-type electron blocking layer may be a p-type Al k Ga 1-k N layer, where 0.1 < k < 0.5, and the thickness of the p-type electron blocking layer may be 10 nm to 100 nm.
[0122] If the thickness of the p-type electron blocking layer is too thin, the blocking effect on electrons will be reduced. If the thickness of the p-type electron blocking layer is too thick, the absorption of light by the p-type electron blocking layer will increase, resulting in a decrease in the light emission efficiency of the LED.
[0123] In the embodiment of the present disclosure, both the low-temperature p-type AlGaN layer and the high-temperature p-type GaN layer are doped with Mg.
[0124] The Mg doping concentration of the low-temperature p-type AlGaN layer is 5×10 20 cm -3 to 1×10 21 cm -3 , and the Mg doping concentration of the high-temperature p-type GaN layer is 1×10 18 cm -3 to 1×10 20 cm -3 .
[0125] Among them, the thickness of the low-temperature p-type AlGaN layer may be 10 nm to 100 nm. For example, the thickness of the low-temperature p-type AlGaN layer may be 80 nm.
[0126] Among them, the thickness of the high-temperature p-type GaN layer may be 10 nm to 100 nm. For example, the thickness of the high-temperature p-type GaN layer may be 50 nm.
[0127] Optionally, the thickness of the p-type contact layer may be 1 nm to 30 nm. As an example, in the embodiment of the present disclosure, the thickness of the p-type contact layer is 20 nm.
[0128] The p-type contact layer is a p-type GaN layer, and the Mg doping concentration of the p-type GaN layer is 1×10 20 cm -3 Up to 1×10 21 cm -3 .
[0129] If the thickness of the p-type contact layer is too thin, it will affect the current contact between the epitaxial layer 20 and the electrode 50 . If the thickness of the p-type contact layer is too thick, it will increase the absorption of light by the p-type contact layer, thereby reducing the luminous efficiency of the LED.
[0130] Alternatively, if Figure 3 As shown, a buffer layer, a nucleation layer and a non-doped GaN layer are further included between the substrate and the n-type layer, and the buffer layer, the nucleation layer and the non-doped GaN layer are sequentially stacked on the substrate.
[0131] In the embodiment of the present disclosure, the buffer layer may be an AlN layer, and the AlN layer is an AlN layer grown at a temperature between 400° C. and 800° C.
[0132] The thickness of the buffer layer may be 10 nm to 50 nm. For example, the thickness of the buffer layer may be 20 nm.
[0133] By setting the thickness of the buffer layer within the above range, it is possible to avoid the buffer layer being too thin, thereby reducing the crystal quality of the epitaxial layer 20 grown on the thinner buffer layer; it is also possible to avoid the buffer layer being too thick, thereby increasing the buffer layer's absorption of light, thereby reducing the luminous efficiency of the light-emitting diode.
[0134] Alternatively, the nucleation layer may be a three-dimensional GaN nucleation layer.
[0135] Exemplarily, the three-dimensional GaN nucleation layer may be grown to a thickness of 0.3 μm to 0.5 μm.
[0136] In the embodiment of the present disclosure, an undoped GaN layer is also grown between the three-dimensional GaN nucleation layer and the n-type layer. Compared with the substrate, since the crystal structure of the undoped GaN layer is similar to that of the n-type layer, the crystal quality of the subsequent epitaxial layer 20 can be improved by providing the undoped GaN layer as a transition layer.
[0137] The thickness of the non-doped GaN layer is 0.5 μm to 3 μm. For example, the thickness of the non-doped GaN layer is 2 μm.
[0138] By setting the thickness of the undoped GaN layer within the above range, it is possible to avoid the undoped GaN layer being too thin, which would not play a transition role and reduce the crystal quality of the grown epitaxial layer 20; it is also possible to avoid the undoped GaN layer being too thick, which would increase the absorption of light by the undoped GaN layer and thus reduce the luminous efficiency of the light-emitting diode.
[0139] Alternatively, if Figure 3 As shown, the surface of the second semiconductor layer 23 has a groove 30 exposing the first semiconductor layer 21 .
[0140] like Figure 3 As shown, the light emitting diode further includes a passivation layer 40 and at least two electrodes 50 . The passivation layer 40 is located in the second semiconductor layer 23 and the recess 30 , and the passivation layer 40 has through holes respectively exposing the second semiconductor layer 23 and the first semiconductor layer 21 .
[0141] like Figure 3 As shown, the electrode 50 is located on the surface of the passivation layer 40, a portion of the electrode 50 is connected to the second semiconductor layer 23 through a through hole, and another portion of the electrode 50 is connected to the first semiconductor layer 21 through a through hole.
[0142] Exemplarily, the electrode includes a first Al layer, a first Ti layer, a second Al layer, a second Ti layer, and an Au layer.
[0143] The thickness of the first Al layer is 8000 angstroms to 12000 angstroms, the thickness of the first Ti layer is 100 angstroms to 500 angstroms, the thickness of the second Al layer is 8000 angstroms to 12000 angstroms, the thickness of the second Ti layer is 500 angstroms to 1500 angstroms, and the thickness of the Au layer is 2000 angstroms to 5000 angstroms.
[0144] For example, the thickness of the first Al layer is 10000 angstroms, the thickness of the first Ti layer is 200 angstroms, the thickness of the second Al layer is 10000 angstroms, the thickness of the second Ti layer is 1000 angstroms, and the thickness of the Au layer is 3000 angstroms.
[0145] The above description is only an optional embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure shall be included in the protection scope of the present disclosure.
Claims
1. A method for preparing a light emitting diode, characterized in that: The preparation method comprises: forming an epitaxial layer, the epitaxial layer comprising a first semiconductor layer, an active layer, and a second semiconductor layer stacked in sequence, the second semiconductor layer having a groove exposing the first semiconductor layer; The epitaxial layer is annealed in an atmosphere free of nitrogen and ammonia.
2. The preparation method according to claim 1, characterized in that: Annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia comprises: The annealing temperature is controlled to be greater than or equal to 700° C., the annealing pressure is controlled to be less than or equal to 500 torr, and the atmosphere in the reaction chamber is controlled to include at least one of oxygen, hydrogen and an inert gas to anneal the epitaxial layer.
3. The preparation method according to claim 2, characterized in that: When the epitaxial layer is annealed in an atmosphere without nitrogen and ammonia, the annealing time is controlled to be greater than or equal to 1 minute.
4. The preparation method according to any one of claims 1 to 3, characterized in that: After annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia, the method further comprises: The epitaxial layer is annealed again in an atmosphere of ammonia and nitrogen.
5. The preparation method according to claim 4, characterized in that: Annealing the epitaxial layer again in an atmosphere of ammonia and nitrogen comprises: The epitaxial layer is annealed at a temperature of 750° C. to 950° C. and a pressure of more than 200 torr.
6. The preparation method according to claim 5, characterized in that: When the epitaxial layer is annealed again, the volume ratio of nitrogen and ammonia in the reaction chamber is controlled to be 0 to 5.
7. The preparation method according to claim 4, characterized in that: When the epitaxial layer is annealed again in the atmosphere of ammonia and nitrogen, the annealing time is controlled to be greater than or equal to 3 minutes.
8. The preparation method according to any one of claims 1 to 3 and claims 5 to 7, characterized in that: After annealing the epitaxial layer in an atmosphere free of nitrogen and ammonia, the method further comprises: A passivation layer is formed on the surface of the second semiconductor layer and in the groove, and through holes are formed on the surface of the passivation layer to expose the second semiconductor layer and the first semiconductor layer respectively.
9. The preparation method according to any one of claims 1 to 3 and claims 5 to 7, characterized in that: Forming the epitaxial layer includes: Etching a patterned structure on the surface of the substrate, wherein the patterned structure includes at least one of a protrusion and a groove; The first semiconductor layer, the active layer and the second semiconductor layer are sequentially formed on the surface of the substrate.
10. A light emitting diode, characterized in that: The light emitting diode comprises an epitaxial layer (20), wherein the epitaxial layer (20) comprises a first semiconductor layer (21), an active layer (22) and a second semiconductor layer (23) stacked in sequence, and the second semiconductor layer (23) has a groove (30) exposing the first semiconductor layer (21); The roughness Ra of the groove wall of the groove (30) is less than 0.05 nm.