High-capacity long-cycle high-nickel positive electrode material and preparation method thereof

By adding boron-containing compounds to the high-nickel positive electrode material to form an ion complex, inhibiting the escape of lithium ions and improving boron coating uniformity, the problem of residual lithium and lithium ions in the high-nickel positive electrode material is solved, and the problem of residual lithium and lithium ions escape in the high-nickel positive electrode material is improved. Capacity and cycle life, while reducing internal resistance.

CN119008882AActive Publication Date: 2024-11-22安徽得壹能源科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411069931.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The residual lithium on the surface of high-nickel positive electrode material leads to negative effects such as slurry jelly and battery cell gas production, and the escape of internal lithium ions leads to the lithium deficiency state on the surface of the material, reducing capacity and increasing internal resistance.

Method used

By adding boron-containing compounds, an ionic complex is formed to adhere to the surface of the high-nickel positive electrode material and lithium ions, inhibit the escape of lithium ions, and improve the uniformity of boron coating through wet coating and improve the circulation life of the material.

Benefits of technology

It effectively improves the capacity and cycle life of high-nickel cathode materials, reduces internal resistance growth, and enhances the stability and high temperature life of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a high-capacity long-cycle high-nickel positive electrode material and a preparation method thereof, the high-nickel positive electrode material is a compound represented by the following general formula: LiaNixCoyMnzM1-x-y-zO2, M is selected from one or more of V, Ta, Nb, Sr, Mo, Mg, Al, Zr, Ti, Ca, La and W, a is more than or equal to 0.80 and less than or equal to 1.20, and x is more than or equal to 0.6 and less than or equal to 1.0. The material can form an ion complex with lithium ions, and after the compound is added into an aqueous solution, the compound can be attached to the surface of the high-nickel positive electrode material after complexing the lithium ions, so that excessive escape of the lithium ions is prevented, the structural lithium loss of the material in the washing process is minimized, and the high-nickel positive electrode material with the high capacity characteristic is prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium ion batteries, and in particular relates to a high-capacity, long-cycle, high-nickel positive electrode material and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, high specific energy, long cycle life, light weight, low self-discharge and high cost performance. They have broad application prospects in electronic equipment, electronic vehicles, space technology and other fields, and are now receiving more and more attention and attention. With the new national policy starting to lean towards energy density and range in subsidies for new energy vehicles, coupled with the increase in the number of cycles of charge and discharge of ternary materials and the improvement of safety, ternary materials have achieved rapid development in recent years. At present, the ternary material used in the market is mainly 523, but it still cannot meet consumers' demand for energy density. Therefore, people consider increasing the capacity of the material by increasing the nickel content in the material. Usually, there are high-nickel materials such as NCM811, NC91 and NCA specifications, and their 0.2C gram capacity can reach more than 190mAh / g, which is more than 15% higher than 523.

[0003] In recent years, with the rapid development of technologies such as electric vehicles, the demand for high-energy-density secondary batteries has continued to increase. Therefore, research on high-nickel positive electrode materials with excellent capacity characteristics is being actively carried out. Summary of the invention

[0004] The inventors found that the residual lithium on the surface of the high-nickel positive electrode material is high, which will cause negative effects such as jelly of slurry and gas production of battery core. The residual lithium remaining on the surface of the particles after high-temperature sintering is usually removed by water washing. Although the residual lithium on the surface is removed by this water washing process, the lithium ions inside the high-nickel positive electrode material are easy to escape and form NiO, NiOOH, etc. on the surface of the material, so that the surface of the material forms a lithium-deficient state, resulting in the problem of reduced material capacity. In order to solve the above problems, it is necessary to suppress the internal lithium ion escape of the high-nickel positive electrode material when washing, remove the residual lithium on the surface, and the surface will not form a lithium-deficient state, thereby improving the capacity of the high-nickel positive electrode material and reducing the internal resistance. The object of the present invention is to provide a high-capacity long-cycle high-nickel positive electrode material and a preparation method thereof, by adding a compound to suppress the escape of lithium ions inside the high-nickel positive electrode active material, improve the performance of the high-nickel positive electrode material and reduce the internal resistance, and at the same time, this compound is a boron-containing element, and the uniformity of the boron coating of the high-nickel positive electrode material is improved by a wet coating strategy, and the cycle life performance of the material is improved.

[0005] In one aspect of the present invention, a high-capacity, long-cycle, high-nickel cathode material is provided. According to an embodiment of the present invention, the high-nickel cathode material is a compound represented by the following general formula: Li a Nix Co y Mn z M 1-x-y-z O2, M is selected from one or more of V, Ta, Nb, Sr, Mo, Mg, Al, Zr, Ti, Ca, La and W, 0.80≤a≤1.20, 0.6≤x≤1.0. The compound can form an ion complex with lithium ions. When added to an aqueous solution, the compound can complex lithium ions and attach to the surface of a high-nickel positive electrode material to prevent excessive escape of lithium ions, thereby minimizing the loss of lithium in the structure of the material during the water washing process, and preparing a high-nickel positive electrode material with high capacity characteristics.

[0006] According to an embodiment of the present invention, the above-mentioned high-capacity, long-cycle, high-nickel positive electrode material may further include at least one of the following additional technical features:

[0007] According to an embodiment of the present invention, the high nickel positive electrode material is LiNi 0.90 Co 0.04 Mn 0.05 Zr 0.01 O2. This compound can form an ion complex with lithium ions. When added to an aqueous solution, it can complex lithium ions and attach to the surface of the high-nickel positive electrode material to prevent excessive escape of lithium ions, thereby minimizing the loss of lithium in the material structure during the water washing process, and preparing a high-nickel positive electrode material with high capacity characteristics.

[0008] In another aspect of the present invention, the present invention also proposes a method for preparing a high-capacity, long-cycle, high-nickel positive electrode material. According to an embodiment of the present invention, the method comprises:

[0009] 1) A precursor and a lithium source are subjected to a first sintering treatment, wherein the chemical formula of the precursor is Ni x Co y Mn z M 1-x-y-z (OH)2, so as to obtain a first material,

[0010] 2) mixing the first material with an aqueous solution of a boron compound and drying the mixture to obtain a second material;

[0011] 3) The second material is subjected to a second sintering treatment to obtain the high-capacity, long-cycle, high-nickel positive electrode material, wherein the high-nickel positive electrode material is a compound represented by the following general formula: Li a Ni x Co y Mn z M 1-x-y-zO2, M is selected from one or more of V, Ta, Nb, Sr, Mo, Mg, Al, Zr, Ti, Ca, La and W, 0.80≤a≤1.20, 0.6≤x≤1.0. The method according to the embodiment of the present invention can prepare a compound that can form an ion complex with lithium ions. This compound is added to the aqueous solution, which can complex lithium ions and attach to the surface of the high-nickel positive electrode material to prevent excessive escape of lithium ions, so that the structural lithium loss of the material during the water washing process is minimized, and a high-nickel positive electrode material with high capacity characteristics is prepared; and the added compound contains boron element, and a boron-containing coating layer is formed on the interface when complexing lithium ions. Therefore, compared with the traditional dry coating of boron elements, wet coating can improve the uniformity of coating and increase the cycle life of high-nickel materials.

[0012] According to an embodiment of the present invention, the above method may further include at least one of the following additional technical features:

[0013] According to an embodiment of the present invention, the precursor is Ni 0.90 Co 0.04 Mn 0.05 Zr 0.01 (OH)2.

[0014] According to an embodiment of the present invention, the high nickel positive electrode material is LiNi 0.90 Co 0.04 Mn 0.05 Zr 0.01 O2.

[0015] According to an embodiment of the present invention, the lithium source is one or a combination of lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, and lithium phosphate.

[0016] According to an embodiment of the present invention, the molar ratio of lithium in the lithium source to the sum of nickel, cobalt, manganese and M element in the precursor is 0.80-1.20:1.

[0017] According to an embodiment of the present invention, the D50 of the precursor is 3-20 um. Within this range, the initial charge and discharge efficiency is excellent and the initial internal resistance can be reduced.

[0018] According to an embodiment of the present invention, the D50 of the precursor is 10-13 um. Within this range, the initial charge and discharge efficiency is more excellent and the initial internal resistance can be reduced.

[0019] According to an embodiment of the present invention, the BET of the precursor is 3 to 10 m 2 / g. Within this range, the uniformity of material sintering can be further improved.

[0020] According to an embodiment of the present invention, the BET of the precursor is 5 to 7 m 2 / g. Within this range, the uniformity of material sintering can be further improved.

[0021] According to an embodiment of the present invention, the first sintering process is performed in an oxygen atmosphere.

[0022] According to an embodiment of the present invention, the sintering temperature of the first sintering treatment is 650°C to 1000°C. When the sintering temperature is lower than 650°C, the raw materials remain in the particles due to insufficient reaction, which will reduce the high temperature stability of the battery, and reduce the volume density and crystallinity, thereby reducing the structural stability. On the other hand, when the sintering temperature exceeds 1000°C, uneven growth of particles may occur, and the particles are difficult to break, thereby reducing the capacity.

[0023] According to an embodiment of the present invention, the sintering temperature of the first sintering process is 650°C to 880°C.

[0024] According to an embodiment of the present invention, the sintering time of the first sintering treatment is 5 to 30 hours. If the sintering time is less than 5 hours, the reaction time is too short and a positive electrode active material with high crystallinity cannot be obtained. If the sintering time exceeds 30 hours, the particle size is too large and the production efficiency is reduced.

[0025] According to an embodiment of the present invention, the sintering time of the first sintering treatment is 7 to 15 hours.

[0026] According to an embodiment of the present invention, the boron-containing compound in the aqueous solution of the boron-containing compound is one or a combination of lithium tetramethylborate, lithium bis(oxalate borate), and lithium tetrahydroxyborate.

[0027] According to an embodiment of the present invention, the molar concentration of the aqueous solution containing the boron compound is 0.01M to 0.58M. When the concentration of the compound capable of forming an ion complex with lithium cations contained in the water washing liquid is less than 0.01M, the lithium cations and the complex cannot be fully formed on the surface of the positive electrode active material, so that the lithium ions will escape from the inside of the positive electrode active material, thus causing a capacity drop problem. When the concentration of the compound capable of forming an ion complex with lithium cations contained in the water washing liquid exceeds 0.58M, the coating layer formed on the surface of the positive electrode active material is too thick, which increases the surface resistance, and there are problems of reduced high temperature life characteristics and increased manufacturing costs of the positive electrode active material.

[0028] According to an embodiment of the present invention, the molar concentration of the aqueous solution of the boron compound is 0.06M to 0.38M.

[0029] According to an embodiment of the present invention, the molar concentration of the aqueous solution of the boron compound is 0.08M to 0.25M.

[0030] According to an embodiment of the present invention, the molar ratio of the total molar number of Ni, Co, Mn and M in the precursor to the boron is 100:0.07 to 100:3. When the molar ratio is less than 100:0.0.7, a uniform coating layer cannot be formed, resulting in reduced capacity and reduced cycle life characteristics. When the molar ratio is greater than 100:3, the coating layer formed on the surface of the positive electrode active material is too thick, resulting in increased surface resistance, reduced cycle life characteristics, and increased manufacturing costs.

[0031] According to an embodiment of the present invention, the molar ratio of the total molar number of Ni, Co, Mn and M in the precursor to the boron is 100:0.25 to 100:2.5.

[0032] According to an embodiment of the present invention, the weight ratio of the first material to the aqueous solution is 1 to 2: 1. Within this range, it is possible to ensure that residual lithium is washed away and prevent the surface of the material from being excessively washed and causing lithium deficiency.

[0033] According to an embodiment of the present invention, the weight ratio of the first material to the aqueous solution is 1.5 to 2. According to an embodiment of the present invention,

[0034] Optionally, the temperature of the aqueous solution is 0-20° C. Within this range, it is possible to ensure that residual lithium is washed away and prevent the surface of the material from being excessively washed and causing lithium deficiency.

[0035] According to an embodiment of the present invention, the temperature of the aqueous solution is 0-5° C. Within this range, it is possible to ensure that residual lithium is washed away and prevent the surface of the material from being excessively washed and causing lithium deficiency.

[0036] According to an embodiment of the present invention, the drying process is performed under a vacuum environment.

[0037] According to an embodiment of the present invention, the drying temperature of the drying process is 50-250° C. Within this range, the moisture can be dried and the lithium in the structure can be prevented from diffusing to the surface.

[0038] According to an embodiment of the present invention, the drying temperature of the drying process is 130-150° C. Within this range, the moisture can be dried and the lithium in the structure can be prevented from diffusing to the surface.

[0039] According to an embodiment of the present invention, the drying time is 1 to 10 hours, within which the water can be dried and the lithium in the structure can be prevented from diffusing to the surface.

[0040] According to an embodiment of the present invention, the drying time is 2-5 hours, within which the water can be dried and the lithium in the structure can be prevented from diffusing to the surface.

[0041] According to an embodiment of the present invention, the temperature of the second sintering treatment is 100-400° C. Within this range, the cycle life of the battery is further improved while preventing the capacity from decreasing.

[0042] According to an embodiment of the present invention, the temperature of the second sintering process is 250-350° C. Within this range, the cycle life of the battery is further improved while preventing the capacity from decreasing.

[0043] According to an embodiment of the present invention, the second sintering treatment time is 3 to 10 hours. Within this range, the cycle life of the battery is further improved while preventing the capacity from decreasing.

[0044] According to an embodiment of the present invention, the second sintering treatment time is 5 to 8 hours. Within this range, the cycle life of the battery is further improved while preventing the capacity from decreasing.

[0045] In another aspect of the present invention, a method for preparing the long cycle high nickel positive electrode material as described above is provided. According to an embodiment of the present invention, the preparation method comprises the following steps:

[0046] S1: Mix the precursor and the lithium source and place them in a box-type atmosphere furnace for sintering and crushing to prepare the first material. The chemical formula of the precursor is Ni x Co y Mn z M 1-x-y-z (OH)2, where 0.6≤x≤1.0;

[0047] S2: adding the first material to an aqueous solution containing a boron compound, the boron compound in the aqueous solution forms a complex with the lithium ions escaped from the high-nickel positive electrode material, the complex adheres to the surface of the positive electrode material, while removing the residual carbonate and hydroxide ions on the surface of the high-nickel positive electrode material, it can effectively inhibit the escape of lithium ions inside the high-nickel positive electrode active material during the water washing process, and the washed material is dried at a certain temperature to obtain a second material;

[0048] S3: Sintering and crushing the second material at a certain temperature to obtain the required high-capacity, long-cycle, high-nickel positive electrode material.

[0049] According to an embodiment of the present invention, step S1 includes: the lithium source is one or a combination of lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, and lithium phosphate.

[0050] According to an embodiment of the present invention, step S1 includes: a molar ratio of lithium in the lithium source to the sum of nickel, cobalt, manganese and M elements in the nickel-cobalt-manganese hydroxide precursor is 0.80-1.20:1.

[0051] According to an embodiment of the present invention, step S1 includes: the D50 of the precursor is 3-20 um, preferably 10-13 um, within which the initial charge and discharge efficiency is excellent and the initial internal resistance can be reduced.

[0052] According to an embodiment of the present invention, step S1 includes: the BET of the precursor is between 3 and 10 m 2 / g, preferably 5 to 7 m 2 / g, within this range the uniformity of material sintering can be further improved.

[0053] According to an embodiment of the present invention, the S1 step includes: the sintering is carried out in an oxygen atmosphere, the sintering temperature is 650°C to 1000°C, preferably at a temperature of 650°C to 880°C. When the sintering temperature is lower than 650°C, the raw materials remain in the particles due to insufficient reaction, which will reduce the high temperature stability of the battery, and will reduce the volume density and crystallinity, thereby reducing the structural stability. On the other hand, when the sintering temperature exceeds 1000°C, uneven growth of particles may occur, and the particles are difficult to break, thereby reducing the capacity. The sintering time is 5 to 30 hours, preferably 7 to 15 hours. If the sintering time is less than 5 hours, the reaction time is too short and the positive electrode active material with high crystallinity cannot be obtained. When it exceeds 30 hours, the particle size is too large and the production efficiency is reduced.

[0054] According to an embodiment of the present invention, step S2 includes: the weight ratio of the first material to the aqueous solution is 1 to 2:1, preferably 1.5 to 2:1, the temperature of the aqueous solution is 0 to 20°C, preferably 0 to 5°C, and the washing time is 1 to 10 minutes, preferably 2 to 4 minutes. Within this range, it can be ensured that the residual lithium is washed away, and the surface of the material can be prevented from being excessively washed and causing lithium deficiency.

[0055] According to an embodiment of the present invention, step S2 includes: the boron-containing compound is one or a combination of lithium tetramethylborate, lithium bis(oxalate borate), and lithium tetrahydroxyborate.

[0056] According to an embodiment of the present invention, step S2 includes: the molar concentration of the boron-containing compound is 0.01M to 0.58M, preferably 0.06M to 0.38M, and more preferably 0.08M to 0.25M. When the concentration of the compound capable of forming an ion complex with lithium cations contained in the water washing liquid is less than 0.01M, the lithium cations and the complex cannot be fully formed on the surface of the positive electrode active material, so that the lithium ions will escape from the inside of the positive electrode active material, and thus there is a problem of capacity reduction. When the concentration of the compound capable of forming an ion complex with lithium cations contained in the water washing liquid exceeds 0.58M, the coating layer formed on the surface of the positive electrode active material is too thick, which increases the surface resistance, and there are problems of reduced high temperature life characteristics and increased manufacturing costs of the positive electrode active material.

[0057] According to an embodiment of the present invention, the S2 step includes: the molar ratio of the total molar number of Ni, Co, Mn and M to boron is 100:0.07 to 100:3, preferably 100:0.25 to 100:2.5. When the molar ratio is less than 100:0.0.7, a uniform coating layer cannot be formed, resulting in reduced capacity and reduced cycle life characteristics. When the molar ratio is greater than 100:3, the coating layer formed on the surface of the positive electrode active material is too thick, resulting in increased surface resistance, reduced cycle life characteristics, and increased manufacturing costs.

[0058] According to an embodiment of the present invention, step S2 includes: the drying is carried out in a vacuum environment at a temperature of 50 to 250° C., preferably 130 to 150° C., and a drying time of 1 to 10 hours, preferably 2 to 5 hours. Within this range, the moisture can be dried and the lithium in the structure will not diffuse to the surface.

[0059] According to an embodiment of the present invention, step S3 includes: a sintering temperature of 100 to 400° C., preferably 250 to 350° C., and a sintering time of 3 to 10 hours, preferably 5 to 8 hours. Within this range, the cycle life of the battery can be further improved while preventing the capacity from decreasing.

[0060] According to the embodiments of the present invention, the present invention has at least one of the following technical effects:

[0061] 1) The present invention uses a compound that can form an ion complex with lithium ions. The compound is added to the aqueous solution to complex lithium ions and attach them to the surface of the high-nickel positive electrode material, thereby preventing excessive escape of lithium ions, minimizing the structural lithium loss of the material during the water washing process, and preparing a high-nickel positive electrode material with high capacity characteristics;

[0062] 2) The added compound contains boron, and a boron-containing coating layer is formed on the interface when complexing lithium ions. Therefore, compared with the traditional dry coating of boron elements, the wet coating can improve the uniformity of the coating and increase the cycle life of the high-nickel material. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0064] Figure 1 This is a SEM (scanning electron microscope) photo of the high nickel positive electrode material prepared in Example 1 of the present invention at 10,000 times magnification;

[0065] Figure 2 This is a SEM (scanning electron microscope) photo of the high nickel positive electrode material prepared in Example 2 of the present invention at 10,000 times magnification;

[0066] Figure 3 This is a SEM (scanning electron microscope) photograph of the high nickel positive electrode material prepared in Example 3 of the present invention at 10,000 times magnification. DETAILED DESCRIPTION

[0067] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0068] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0069] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0070] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0071] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0072] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.

[0073] Example 1

[0074] This embodiment provides a high-capacity, long-cycle, high-nickel positive electrode material, which is a compound shown in the following formula: LiNi 0.90 Co 0.04 Mn 0.05 Zr 0.01 O2; its preparation method comprises the following steps:

[0075] S1, take 1000g of precursor Ni with D50 of 10μm 0.90 Co 0.04 Mn 0.05 Zr 0.01 (OH)2, 470g of LiOH.H2O are added to a high-speed mixer, first stirred at 300rpm for 5min, then stirred at 1000rpm for 25min before discharging; the mixture is put into a mullite sagger, the sagger is placed in a box-type atmosphere furnace, oxygen is introduced, the temperature is raised to 785°C and then kept constant for 5h, the material is discharged after the furnace temperature is cooled to room temperature, and the material is coarsely crushed by a roller device to obtain the first material;

[0076] S2, take 500g of the first material and add it to 400g of an aqueous solution, wherein the molar concentration of lithium bis(oxalate borate) in the aqueous solution is 0.02M, the water temperature is controlled at 2°C, stirred for 2min, separated and filtered with a filter press, so that the water content of the washed product is 2%-10%, and dried under vacuum at 140°C for 4h to obtain a second material;

[0077] S3, put the second material into a mullite sagger, place the sagger in a box-type atmosphere furnace, introduce oxygen, raise the temperature to 280°C and maintain the constant temperature for 6 hours, discharge the material after the furnace temperature cools to room temperature, and crush the material through a roller device for coarse crushing, remove iron, and pass through a 350-mesh sieve to prepare a high-nickel positive electrode material.

[0078] Example 2

[0079] In Example 2, except that the molar concentration of lithium bis(oxalate borate) in the aqueous solution in step S2 is 0.06 M, other conditions are the same as those in Example 1 to prepare a high-nickel positive electrode material.

[0080] Example 3

[0081] In Example 3, except that the molar concentration of lithium bis(oxalate borate) in the aqueous solution in step S2 is 0.1 M, other conditions are the same as those in Example 1 to prepare a high-nickel positive electrode material.

[0082] Comparative Example 1

[0083] In Comparative Example 1, except that the aqueous solution in step S2 is deionized water without adding anything, other conditions are the same as those in Example 1 to prepare a high-nickel positive electrode material.

[0084] Comparative Example 2

[0085] In Comparative Example 3, the aqueous solution in step S2 is deionized water without adding anything, and in step S3, 200 g of the second material and 11.44 g of boric acid are first dry-mixed, and other conditions are the same as in Example 1 to prepare a high-nickel positive electrode material.

[0086] The SEM test of the present invention is as follows: a Hitachi S4800 scanning electron microscope (SEM) is used to perform morphological analysis on the material; a powder sample of less than 1 g is weighed on a clean sample stage, the circulating water of the scanning electron microscope is connected, the sample stage is moved by a computer, and the magnification, focus, and astigmatism are adjusted. Generally, the magnification is adjusted from large to small until a clear and satisfactory image is obtained.

[0087] The buckle electricity production and testing in the present invention are as follows: the ingredients are prepared according to the production method of conductive agent: binder positive electrode material = 1.5:2:96.5, coated on one side, placed in a vacuum drying oven for more than 24 hours, the pressure is -0.1MPa, the drying temperature is 80°C, and placed in a glove box for use after drying. After the dried pole piece is compacted (no material falling off), a round piece with a diameter of 11mm is punched out with a puncher, and its mass is accurately weighed (accurate to 0.1mg). After the weighing paper is packed, it is placed in a surface dish. At the same time, the mass of the same model and size aluminum foil of each pole piece to be tested is also accurately weighed and recorded. The weighed pole piece to be tested is placed in an 80°C vacuum oven and baked for more than 12 hours. Assembly begins when the concentrations of H2O and O2 in the glove box are both lower than 5ppm. Various materials are placed in the battery shell in sequence (the placement order is: positive electrode cap → 2 drops of electrolyte → positive electrode sheet → diaphragm → lithium sheet & gasket → 3-4 drops of electrolyte → spring → negative electrode cap). The assembled battery is sealed with a hydraulic Kejing sealer. The capacity test voltage range is 2.75~4.25V, the charge and discharge rate is 0.1C, the cycle test voltage range is 2.75~4.25V (high voltage cycle), the charge and discharge rate is 1C, and the temperature is 25℃.

[0088] Table 1 is a comparison of the initial performance of the embodiment and the comparative example.

[0089]

[0090] As shown in Table 1, compared with the examples and comparative examples, the high nickel positive electrode material prepared by the method of the present invention has obvious advantages in initial capacity, first efficiency and initial DCR. During water washing, a compound that complexes lithium ions is added to prevent the escape of lithium ions in the structure, thereby minimizing the loss of lithium ions and effectively inhibiting the decrease in initial capacity.

[0091] Table 2 Capacity retention rate of the embodiments and comparative examples after 100 cycles

[0092]

[0093] Table 3 DC internal resistance growth rate after 100 cycles of the embodiments and comparative examples

[0094]

[0095] As shown in Tables 2 and 3, according to the embodiments, compared with the comparative examples, the high nickel positive electrode material prepared by the method of the present invention has excellent cycle life and lower internal resistance growth rate, wet coating can improve coating uniformity, the cycle life of the material is improved and the internal resistance growth can be suppressed.

[0096] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0097] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A high-capacity, long-cycle, high-nickel cathode material, characterized in that: The high nickel positive electrode material is a compound shown in the following general formula: Li a Ni x Co y Mn z M 1-x-y-z O2, M is selected from one or more of V, Ta, Nb, Sr, Mo, Mg, Al, Zr, Ti, Ca, La and W, 0.80≤a≤1.20, 0.6≤x≤1.

0.

2. The high-capacity, long-cycle, high-nickel positive electrode material according to claim 1, characterized in that: The high nickel positive electrode material is LiNi 0.90 Co 0.04 Mn 0.05 Zr 0.01 O2.

3. A method for preparing a high-capacity, long-cycle, high-nickel cathode material, characterized in that: include: 1) A precursor and a lithium source are subjected to a first sintering treatment, wherein the chemical formula of the precursor is Ni x Co y Mn z M 1-x-y-z (OH)2, so as to obtain a first material, 2) mixing the first material with an aqueous solution of a boron compound and drying the mixture to obtain a second material; 3) The second material is subjected to a second sintering treatment to obtain the high-capacity, long-cycle, high-nickel positive electrode material, wherein the high-nickel positive electrode material is a compound represented by the following general formula: Li a Ni x Co y Mn z M 1-x-y-z O2, M is selected from one or more of V, Ta, Nb, Sr, Mo, Mg, Al, Zr, Ti, Ca, La and W, 0.80≤a≤1.20, 0.6≤x≤1.

0.

4. The method according to claim 3, characterized in that The precursor is Ni 0.90 Co 0.04 Mn 0.05 Zr 0.01 (OH)2; Optionally, the high nickel cathode material is LiNi 0.90 Co 0.04 Mn 0.05 Zr 0.01 O2.

5. The method according to claim 3 or 4, characterized in that: The lithium source is one or a combination of lithium hydroxide, lithium carbonate, lithium nitrate, lithium sulfate, and lithium phosphate; Optionally, the molar ratio of lithium in the lithium source to the sum of nickel, cobalt, manganese and M element in the precursor is 0.80 to 1.20:

1.

6. The method according to claim 3 or 4, characterized in that: The D50 of the precursor is 3 to 20 um; Optionally, the D50 of the precursor is 10-13 um; Optionally, the BET of the precursor is 3 to 10 m 2 / g; Optionally, the BET of the precursor is 5 to 7 m 2 / g.

7. The method according to claim 3 or 4, characterized in that: The first sintering process is carried out in an oxygen atmosphere; Optionally, the sintering temperature of the first sintering treatment is 650°C to 1000°C; Preferably, the sintering temperature of the first sintering treatment is 650°C to 880°C; Optionally, the sintering time of the first sintering treatment is 5 to 30 hours; Preferably, the sintering time of the first sintering treatment is 7 to 15 hours.

8. The method according to claim 3 or 4, characterized in that: The boron-containing compound in the aqueous solution of the boron-containing compound is one or a combination of lithium tetramethylborate, lithium bis(oxalate)borate, and lithium tetrahydroxyborate; Optionally, the molar concentration of the aqueous solution of the boron-containing compound is 0.01M to 0.58M; Optionally, the molar concentration of the aqueous solution of the boron-containing compound is 0.06M to 0.38M; Optionally, the molar concentration of the aqueous solution of the boron-containing compound is 0.08M to 0.25M; Optionally, the molar ratio of the total molar number of Ni, Co, Mn and M in the precursor to the boron is 100:0.07 to 100:3; Preferably, the molar ratio of the total molar number of Ni, Co, Mn and M in the precursor to the boron is 100:0.25 to 100:2.5; Optionally, the weight ratio of the first material to the aqueous solution is 1 to 2:1; Preferably, the weight ratio of the first material to the aqueous solution is 1.5 to 2; Optionally, the temperature of the aqueous solution is 0 to 20°C; Preferably, the temperature of the aqueous solution is 0-5°C.

9. The method according to claim 3 or 4, characterized in that: The drying process is carried out in a vacuum environment; Optionally, the drying temperature of the drying treatment is 50 to 250° C.; Preferably, the drying temperature of the drying treatment is 130-150°C; Optionally, the drying time is 1 to 10 hours; Preferably, the drying process takes 2-5 hours.

10. The method according to claim 3 or 4, characterized in that: The temperature of the second sintering treatment is 100-400° C.; Preferably, the temperature of the second sintering treatment is 250-350°C; Optionally, the second sintering treatment time is 3 to 10 hours; Preferably, the second sintering treatment takes 5 to 8 hours.

Citation Information

Patent Citations

  • Method for preparing high-nickel positive electrode material and high-nickel positive electrode material obtained by using same

    CN109428077A

  • Positive electrode material with low surface residual alkali as well as preparation method and application thereof

    CN109817914A

  • Surface-modified high-nickel positive electrode material, and preparation method and application thereof

    CN111793824A

  • Modified positive electrode active material as well as preparation method and application thereof

    CN117317187A