Slurry for negative pole piece, negative pole piece and electrochemical device

By using conductive materials, polyfluoroolefin polymers and modified hydrogenated nitrile rubber on the negative electrode sheet of lithium-ion batteries to form an elastic functional layer, the battery capacity attenuation and safety performance problems caused by volume expansion of alloy negative electrode materials are solved, and the battery capacity attenuation and safety performance problems are improved. Cycling performance and safety performance.

CN119008933APending Publication Date: 2024-11-22HUAWEI TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310582265.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The alloy negative electrode material expands in volume during the lithium-ion battery circulation, resulting in the destruction and pulverization of active substance particles, the battery capacity decays rapidly, and the solid electrolyte interface repeatedly destroys, affecting the circulation and safety performance.

Method used

Provide a slurry for the negative electrode sheet, including conductive material, polyfluoroolefin polymer and modified hydrogenated nitrile rubber, to form an elastic functional layer, improve the adhesion between the negative electrode sheet and the separator, and to alleviate volume Expansion, promotes electron transport, reduces impedance and polarization.

Benefits of technology

It improves the circulation and safety performance of the negative electrode plate, extends the service life of the battery, reduces the expansion damage of the electrode plate and the electronic path failure, and enhances the flatness and lithium replenishment efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008933A_ABST
    Figure CN119008933A_ABST
Patent Text Reader

Abstract

The invention relates to slurry for a negative electrode plate, the negative electrode plate and an electrochemical device, and the slurry for the negative electrode plate provided by the invention comprises a conductive material, a polyfluoroolefin polymer, modified hydrogenated butadiene-acrylonitrile rubber and a solvent. The invention further provides a negative pole piece, the elastic functional layer is arranged on the surface of the negative active material layer of the negative pole piece, the elastic functional layer comprises the conductive material, the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber, and the elastic functional layer has excellent cohesiveness and elasticity, so that the interface bonding performance between the negative pole piece and the diaphragm can be improved; the volume expansion of the pole piece is relieved, the electron transmission is promoted, and the impedance and polarization of the negative pole piece are reduced, so that the cycle performance and the safety performance of the battery in the use process are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrochemical technology, and in particular to a slurry for a negative electrode sheet, a negative electrode sheet and an electrochemical device. Background Art

[0002] Lithium-ion batteries have the characteristics of high specific energy, long cycle life, high operating voltage, and wide operating temperature range. They are widely used in portable electronic devices, electric vehicles, and other fields. With the rapid development of electric vehicles, people have higher and higher requirements on the energy density and cycle performance of lithium-ion batteries. Alloy negative electrode materials are considered to be a very promising negative electrode material due to their higher specific capacity (Si ~ 4200mAh / g, P ~ 2760mAh / g).

[0003] However, the volume expansion of alloy negative electrode materials is large during the cycle of lithium-ion batteries, which can easily cause the destruction and crushing of active material particles, resulting in rapid battery capacity decay; at the same time, the large volume expansion leads to repeated destruction and generation of the solid electrolyte interface film (SEI), resulting in an increase in by-products and high electrolyte consumption, and is more prone to gas production, thereby affecting the battery's cycle performance and safety performance. Summary of the invention

[0004] The purpose of the present application is to provide a slurry for a negative electrode sheet, a negative electrode sheet and an electrochemical device. The slurry for a negative electrode sheet provided in the present application is coated on the surface of the negative electrode sheet to form an elastic functional layer, which has excellent adhesion and elasticity, can improve the interface adhesion performance between the negative electrode sheet and the separator, alleviate the volume expansion of the sheet, and promote electron transmission, reduce the impedance and polarization of the negative electrode sheet, thereby further improving the cycle performance and safety performance of the battery during use.

[0005] In a first aspect, the present application provides a slurry for a negative electrode plate, wherein the slurry comprises a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

[0006] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0007] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.

[0008] In some embodiments, the general structural formula of the olefin monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

[0009] In some embodiments, based on the total mass of the components in the slurry excluding the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4).

[0010] In some embodiments, the solid content of the slurry is 5 wt % to 10 wt %.

[0011] In some embodiments, the modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

[0012] In some embodiments, the viscosity of the slurry is 100 cP to 2000 cP.

[0013] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene.

[0014] In some embodiments, the solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, n-hexane or N-methylpyrrolidone.

[0015] In a second aspect, the present application provides a negative electrode plate, the negative electrode plate comprising:

[0016] A negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector; and

[0017] An elastic functional layer is covered on the surface of the negative electrode active material layer, and the elastic functional layer comprises a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

[0018] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0019] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, vinyl fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0020] In some embodiments, the general structural formula of the monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

[0021] In some embodiments, the modified hydrogenated nitrile rubber is obtained by polymerizing ethylene and acrylonitrile.

[0022] In some embodiments, the molar percentage of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

[0023] In some embodiments, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4).

[0024] In some embodiments, the thickness of the negative electrode current collector is 5 μm to 15 μm.

[0025] In some embodiments, the negative electrode active material layer has a thickness of 10 μm to 70 μm.

[0026] In some embodiments, the elastic functional layer has a thickness of 1 μm to 5 μm.

[0027] In some embodiments, the negative electrode sheet includes a negative electrode active material.

[0028] In some embodiments, the negative electrode active material includes a silicon-based material, and the silicon-based material is selected from at least one of elemental silicon, a silicon-oxygen compound, a silicon-carbon composite, a silicon-nitrogen composite, and a silicon alloy.

[0029] In some embodiments, the negative electrode active material includes a phosphorus-based material, and the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite.

[0030] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes, and graphene.

[0031] In a third aspect, the present application provides an electrochemical device, comprising the negative electrode sheet described in the second aspect.

[0032] In a fourth aspect, the present application further provides an electronic device, wherein the electronic device is the electrochemical device described in the third aspect.

[0033] Compared with the prior art, this application has at least the following beneficial effects:

[0034] The slurry for the negative electrode provided in the present application includes a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent. The polyfluoroolefin polymer can improve the bonding effect of the elastic functional layer formed by the slurry coating; the polyfluoroolefin polymer can form a miscible layer with the polymer materials such as polyvinylidene fluoride (abbreviated as PVDF) in the diaphragm coating during the shaping and hot pressing process, thereby improving the bonding force between the diaphragm and the negative electrode, thereby improving the contact interface; it can also provide mechanical strength, and the synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can adjust the balance between the toughness and elasticity of the elastic functional layer, thereby achieving a toughening effect.

[0035] Second, modified hydrogenated nitrile rubber is used as a dispersant to improve the uniformity of the dispersion of the conductive material in the slurry, inhibit the pulverization or agglomeration of the conductive material in the slurry, and make the slurry have both low solid content and high stability; thus, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the negative electrode plate, and the excellent elasticity can adapt to the extension of the plate caused by the volume expansion and prevent it from falling off the plate.

[0036] Third, the conductive material in the slurry is evenly dispersed, so that the elastic functional layer formed by the slurry coating has excellent conductivity and equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / replenishment process.

[0037] In the negative electrode plate provided by the present application, the elastic functional layer covers the surface of the negative electrode active material layer; first, the elastic functional layer can make the negative electrode plate and the diaphragm have excellent bonding effect, which can improve the stress distribution of the plate, alleviate the problems of interface expansion and battery cell deformation, thereby further improving the cycle life and safety performance of the battery in actual use; second, the elastic functional layer has excellent elasticity and buffering performance (functional layer deformation force < plate adhesion force and plate expansion stress and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative electrode plate, alleviate the volume expansion of the negative electrode plate during the cycle, and can also alleviate the shedding of some particles and the destruction of the electron path caused by particle expansion and crushing, inhibiting the active material The cycle capacity attenuation phenomenon caused by quality loss can improve the flatness of the surface of the negative electrode, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be dispersed, which promotes electron transmission and reduces the impedance and polarization of the negative electrode; and acts as a lithium replenishment buffer layer to reduce the interfacial side reactions caused by direct contact between metallic lithium and the negative electrode active material layer during metal lithium replenishment, thereby improving the lithium replenishment efficiency; in the late stage of the cycle, the elastic functional layer can also ensure the complete electronic path of the electrode, so that the electric field on the surface of the electrode is dispersed, and the uniform deposition of lithium ions is promoted, thereby improving the cycle performance and safety performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] The present application is further described below in conjunction with the accompanying drawings and embodiments.

[0039] Figure 1 A schematic diagram of a lithium-ion battery provided for this application;

[0040] Figure 2 A schematic diagram of the structure of the negative electrode provided in this application;

[0041] Figure 3 A schematic diagram of the bonding between the negative electrode plate and the separator provided in this application;

[0042] Figure 4 A schematic diagram of the surface flatness of the negative electrode after cycling provided by this application;

[0043] Figure 5 A schematic diagram of the conductive performance of the elastic functional layer of the negative electrode sheet provided in this application;

[0044] Figure 6 This is a SEM image of the negative electrode sheet provided in Example 1 of the present application;

[0045] Figure 7a A schematic diagram of the surface flatness of the negative electrode sheet after cycling provided in Example 1 of the present application;

[0046] Figure 7b This is a local SEM image of the negative electrode sheet after cycling provided in Example 1 of the present application;

[0047] Figure 8a A schematic diagram of the surface flatness of the negative electrode plate after cycling provided in Comparative Example 1 of the present application;

[0048] Figure 8b This is a local SEM image of the negative electrode sheet after cycling provided in Comparative Example 1 of the present application;

[0049] Fig. 9 Schematic diagram of the cycle capacity retention rate of the lithium-ion battery provided in Example 1 and Comparative Example 1 of the present application.

[0050] Figure 2 middle:

[0051] 1- negative electrode current collector;

[0052] 2- negative electrode active material layer;

[0053] 3- Elastic functional layer. DETAILED DESCRIPTION

[0054] In order to better understand the technical solution of the present application, the embodiments of the present application are described in detail below with reference to the accompanying drawings.

[0055] It should be clear that the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0056] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0057] It should be understood that the term "and / or" used in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0058] Figure 1 A schematic diagram of a lithium-ion battery provided for this application, such as Figure 1As shown, it includes a positive electrode sheet, a negative electrode sheet, an electrolyte, a diaphragm and a corresponding circuit, wherein the lithium-ion battery realizes energy storage and release by the intercalation and deintercalation of lithium ions between the positive and negative electrodes, the electrolyte is the carrier for the transmission of lithium ions between the positive and negative electrodes, and the ion-conducting but electronically insulating diaphragm ensures the migration of lithium ions while separating the positive and negative electrodes to prevent short circuits. The positive and negative active materials are the main parts of the lithium battery that perform the energy storage function, and determine the energy density, cycle performance and safety performance of the battery cell. After determining the positive electrode material system, the capacity of the negative electrode material is crucial to the improvement of the energy density of the entire battery cell.

[0059] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on the surface of the positive electrode current collector, and the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on the surface of the negative electrode current collector.

[0060] Battery energy density is positively correlated with the negative electrode gram capacity. Compared with graphite materials (theoretical capacity 372mAh / g), the use of alloy negative electrode materials with higher gram capacity (Si~4200mAh / g, P~2760mAh / g) is undoubtedly the preferred route to improve battery energy density. However, alloy negative electrode materials undergo huge volume changes (200%~300%) during the battery cycle. Their dramatic volume changes have the following negative effects: (1) The volume expansion of the negative electrode plate is large, and the destruction and crushing of the alloy particles lead to rapid battery capacity decay; (2) The rate of lithium alloying reaction is poor; (3) The first cycle coulomb efficiency is low, and additional active lithium needs to be supplemented; (4) The solid electrolyte interface (SEI) of the alloy negative electrode material is repeatedly destroyed and generated during the cycle, resulting in more by-products and more electrolyte consumption, and it is easier to produce gas, which will cause a reduction in the contact interface between the negative electrode plate and the separator, and also have a significant impact on the interface bonding performance between the positive and negative electrode plates and the separator, thereby affecting the battery's cycle performance and safety performance. The existence of these problems has hindered the commercialization of alloy negative electrode materials.

[0061] In some embodiments, the negative electrode plate includes a lithium metal layer or a current collector, and a functional layer is provided on the surface of the lithium metal layer, the functional layer includes M conductive layers and N dielectric layers stacked, and the conductive layer includes a lithium wetting material; wherein M≥1, N≥1. The dielectric layer can more effectively reduce the electron concentration on the surface of the functional layer, forcing lithium ions to enter the functional layer for deposition, reducing lithium deposition at the negative electrode interface, thereby inhibiting the formation of lithium dendrites at the negative electrode interface, and improving the cycle life and safety performance of the electrochemical device. Although this method can improve the cycle life and safety performance of the electrochemical device, the dielectric layer is an insulating layer, which will increase the contact impedance of the electrode interface, thereby increasing polarization, which will have a harmful effect on the cycle performance and capacity of the battery.

[0062] In other embodiments, the functional layer may also include a catechol structure polymer compound, which can prevent oxidation of the current collector substrate and prevent the current collector substrate from dissolving or precipitating when the lithium-ion battery is charged in an over-discharge state. Similarly, this type of functional layer is an insulating layer, which will increase the contact impedance of the electrode interface, thereby increasing polarization, which will have a harmful effect on the cycle performance and capacity of the battery.

[0063] Therefore, how to make the electrochemical device have both excellent cycle performance and safety performance, improve the interfacial adhesion between the negative electrode plate and the separator, and at the same time reduce the impedance and polarization of the negative electrode plate, alleviate volume expansion, etc., is still the goal that has been explored.

[0064] Based on this, in a first aspect, the present application provides a slurry for a negative electrode plate, the slurry comprising a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

[0065] The slurry for the negative electrode provided in the present application includes a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent. The polyfluoroolefin polymer can improve the bonding effect of the elastic functional layer formed by the slurry coating; the polyfluoroolefin polymer can form a miscible layer with the polymer materials such as polyvinylidene fluoride in the diaphragm coating during the shaping and hot pressing process, thereby improving the bonding force between the diaphragm and the negative electrode, thereby improving the contact interface; it can also provide mechanical strength, and the synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can adjust the balance between the toughness and elasticity of the elastic functional layer, thereby achieving a toughening effect.

[0066] Second, modified hydrogenated nitrile rubber is used as a dispersant to improve the uniformity of the dispersion of the conductive material in the slurry, inhibit the pulverization or agglomeration of the conductive material in the slurry, and make the slurry have both low solid content and high stability; thus, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the negative electrode plate, and its excellent elasticity can also adapt to the extension of the plate caused by the volume expansion and prevent it from falling off the plate.

[0067] Third, the conductive material in the slurry is evenly dispersed, so that the elastic functional layer formed by the slurry coating has excellent conductivity and equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / replenishment process.

[0068] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

[0069] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, vinyl fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0070] In some embodiments, the general structural formula of the monomer containing polar functional groups is R1CH=CR1R2, wherein R1 is selected from H or CH3; R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN. It can be understood that the polar functional group can be a carbonate group, a carboxyl group, an amino group, an amide group, an imide group, a cyano group, etc. Since these polar functional groups have good affinity with polymer materials such as polyvinylidene fluoride in the diaphragm coating, the entanglement and mutual solubility of the polymer molecular chains in the diaphragm coating and the elastic functional layer can be achieved during the hot pressing shaping process. After hot pressing shaping, the elastic functional layer can form a complete interface with the surface of the negative electrode sheet of the negative electrode active material layer, thereby improving the contact interface and improving the interface adhesion between the negative electrode sheet and the diaphragm.

[0071] Optionally, the molar proportion of the fluorine-containing olefin monomer in the polyfluoroolefin polymer can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc., and of course it can also be other values ​​between 20% and 60%, which are not limited here.

[0072] Optionally, the molar proportion of the polar functional group-containing olefin monomer in the polyfluoroolefin polymer can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., and of course it can also be other values ​​between 40% and 80%, which are not limited here.

[0073] It can be understood that the presence of polar functional groups in the polymer molecular chain can increase the adhesion of the polymer. The polyfluoroolefin polymer in the present application is obtained by copolymerization of fluorine-containing olefin monomers and olefin monomers containing polar functional groups. Therefore, the molecular chain structure of the polyfluoroolefin polymer in the present application contains polar functional groups, which can improve the adhesion of the polyfluoroolefin polymer; therefore, using it in the above-mentioned slurry can improve the adhesion between the negative electrode plate and the separator, thereby improving the cycle performance and safety performance of the battery.

[0074] In some embodiments, based on the total mass of the components in the slurry except the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4). Specifically, the mass ratio of the conductive material, the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can be 2:2:4, 2:3:4, 2:4:4, 3:2:4, 3:3:4, 3:4:3, 4:2:4 or 4:4:2, etc., which are not limited here. Preferably, the mass ratio of the polyfluoroolefin polymer: the modified hydrogenated nitrile rubber: the conductive material is (2-3): (3-4): (3-4).

[0075] In some embodiments, the solid content of the slurry is 5wt% to 10wt%, specifically 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0076] In some embodiments, the modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber can be 20%, 25%, 30%, 35%, 40%, 41%, 42%, 43%, 44% or 45%, etc., and of course, it can also be other values ​​within the above range, which is not limited here. The content of acrylonitrile is controlled within the above range, which is conducive to making the elastic functional layer formed by the slurry have excellent elasticity, and at the same time can adapt to the extension of the pole piece caused by volume expansion, and will not fall off the pole piece.

[0077] In some embodiments, the viscosity of the slurry is 100cP to 2000cP, specifically 100cP, 200cP, 300cP, 400cP, 500cP, 700cP, 800cP, 1000cP, 1500cP, 1800cP, 2000cP, etc., which are not limited here. It can be understood that a slurry with too high or too low viscosity is not conducive to the coating of the pole piece. A slurry with high viscosity is not easy to precipitate and has better dispersibility, but when the viscosity of the slurry is too high, it is not conducive to the leveling effect and the coating of the pole piece; when the viscosity of the slurry is low, although the slurry has good fluidity, it is difficult to dry, which reduces the drying efficiency of the coating, and may also cause problems such as coating cracking, slurry particle agglomeration, and poor surface density consistency.

[0078] In some embodiments, the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene. The conductive material can be evenly dispersed in the elastic functional layer, so that the functional layer has excellent conductivity and equipotentiality. When electrons contact the functional layer, the electric field on the surface of the pole piece can be evenly dispersed, promoting uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / dissolution / replenishment process.

[0079] In some embodiments, the solvent is selected from at least one of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dimethyl sulfoxide (DMSO), n-hexane or N-methylpyrrolidone (NMP). It is understood that the polymer can be dissolved in the solvent.

[0080] Second, as Figure 2 As shown, the present application provides a negative electrode plate, the negative electrode plate comprising:

[0081] A negative electrode current collector 1, a negative electrode active material layer 2 disposed on the negative electrode current collector 1; and

[0082] The elastic functional layer 3 covers the surface of the negative electrode active material layer 2 . The elastic functional layer 3 includes a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

[0083] In the negative electrode plate provided by the present application, the elastic functional layer covers the surface of the negative electrode active material layer; first, the elastic functional layer can make the negative electrode plate and the diaphragm have excellent bonding effect, which can improve the stress distribution of the plate, alleviate the problems of interface expansion and battery cell deformation, thereby further improving the cycle life and safety performance of the battery in actual use; second, the elastic functional layer has excellent elasticity and buffering performance (functional layer deformation force < plate adhesion force and plate expansion stress and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative electrode plate, alleviate the volume expansion of the negative electrode plate during the cycle, and can also alleviate the shedding of some particles and the electric shock caused by particle expansion and crushing. The elastic functional layer can destroy the sub-pathway and inhibit the cycle capacity attenuation phenomenon caused by the loss of active materials, thereby improving the flatness of the surface of the negative electrode plate, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode plate can be dispersed, which promotes electron transmission and reduces the impedance and polarization of the negative electrode plate; and acts as a lithium replenishment buffer layer to reduce the side reactions of the lithium replenishment interface and improve the lithium replenishment efficiency; in the later stage of the cycle, the elastic functional layer can also ensure the complete electronic path of the electrode plate, so that the electric field on the surface of the electrode plate is dispersed, and the uniform deposition of lithium ions is promoted, thereby improving the cycle performance and safety performance of the battery.

[0084] Figure 2 The schematic diagram of the structure of the negative electrode provided in this application is as follows: Figure 2 As shown, the negative electrode plate is a negative electrode plate having a negative electrode active material layer 2 and an elastic functional layer 3 on both sides.

[0085] When prepared as Figure 2 When the negative electrode sheet is shown, the preparation method comprises the following steps:

[0086] Step S1, adding a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber into an organic solvent according to a preset ratio, and mixing them evenly to obtain an elastic functional layer slurry;

[0087] Step S2, adding the negative electrode active material and the conductive material into the binder, and mixing them evenly to obtain a negative electrode active material slurry;

[0088] Step S3, coating the negative electrode active material slurry on the surface of the negative electrode current collector, and drying to obtain a negative electrode sheet having a negative electrode active material layer;

[0089] Step S4: coating the elastic functional layer slurry on the surface of the negative electrode active material layer, and drying to obtain a negative electrode sheet having the negative electrode active material layer and the elastic functional layer.

[0090] Wherein, in step S4, the method of coating the elastic functional layer slurry on the surface of the negative electrode active material layer includes at least one of transfer coating or doctor blade coating.

[0091] In some embodiments, the material of the negative electrode current collector includes at least one of copper foil, copper mesh, carbon-coated copper foil, stainless steel foil, or carbon-coated stainless steel foil.

[0092] In some embodiments, the organic solvent includes at least one of N-methylpyrrolidone, ethanol, and acetone. Preferably, the organic solvent is N-methylpyrrolidone.

[0093] In some embodiments, the polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of a monomer containing a polar functional group.

[0094] Optionally, the molar proportion of the fluorine-containing olefin monomer in the polyfluoroolefin polymer can be 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc., and of course it can also be other values ​​between 20% and 60%, which are not limited here.

[0095] Optionally, the molar proportion of the polar functional group-containing monomer in the polyfluoroolefin polymer can be 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75% or 80%, etc., and of course it can also be other values ​​between 40% and 80%, which are not limited here.

[0096] In some embodiments, the fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, vinyl fluoride, trifluoroethylene (TrFE), tetrafluoroethylene (TFE), chlorotrifluoroethylene (CTFE), hexafluoropropylene (HFP), and the like.

[0097] In some embodiments, the general structural formula of the monomer containing polar functional groups is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN. It can be understood that the polar functional group can be a carbonate group, a carboxyl group, an amino group, an amide group, an imide group, a cyano group, etc. Since these polar functional groups have good affinity with polymer materials such as polyvinylidene fluoride in the diaphragm coating, the entanglement and mutual solubility of the polymer molecular chains in the diaphragm coating and the elastic functional layer can be achieved during the hot pressing shaping process. After hot pressing shaping, the elastic functional layer can form a complete interface with the surface of the negative electrode sheet of the negative electrode active material layer, thereby improving the contact interface and improving the interface adhesion between the negative electrode sheet and the diaphragm.

[0098] In the above scheme, by introducing polar groups into the polyfluoroolefin polymer structure, the adhesion of the polyfluoroolefin polymer is further improved, so that the elastic functional layer and the diaphragm have excellent bonding effect, thereby improving the adhesion between the negative electrode plate and the diaphragm, and improving the cycle performance and safety performance of the battery; and the synergistic effect of the polyfluoroolefin polymer and the modified hydrogenated nitrile rubber can also adjust the balance between the toughness and elasticity of the elastic functional layer, thereby achieving a toughening effect.

[0099] Figure 3 A schematic diagram of the bonding between the negative electrode plate and the separator provided in this application, such as Figure 3 As shown, the elastic functional layer has good affinity with the diaphragm coating. During the hot pressing process, the entanglement and mutual dissolution of the polymer molecular chains in the diaphragm coating and the elastic functional layer can be achieved. After hot pressing, the elastic functional layer can form a complete interface with the surface of the negative electrode active material layer and the negative electrode plate, thereby improving the contact interface, improving the interface bonding between the negative electrode plate and the diaphragm, and further improving the interface bonding between the negative electrode plate and the diaphragm.

[0100] In some embodiments, the modified hydrogenated nitrile rubber is obtained by polymerization of ethylene and acrylonitrile. The modified hydrogenated nitrile rubber of the present application is used as a dispersant to improve the uniformity of the dispersion of the conductive material in the slurry, inhibit the pulverization or agglomeration of the conductive material in the slurry, and make the slurry have both low solid content and high stability; thus, the elastic functional layer formed by the slurry coating can buffer the volume expansion of the side close to the negative electrode plate, and the excellent elasticity can adapt to the extension of the plate caused by the volume expansion and will not fall off the plate.

[0101] Figure 4 The schematic diagram of the surface flatness of the negative electrode plate after cycling provided in this application is as follows: Figure 4 As shown, the elastic functional layer has excellent elasticity and buffering properties, and the deformation force of the elastic functional layer is smaller than the adhesion force of the negative electrode sheet, the expansion stress of the electrode sheet and the interface shaping force, which can reduce the extrusion and expansion damage of the negative electrode active material particles to the negative electrode sheet, alleviate the volume expansion of the negative electrode sheet during the cycle, thereby improving the flatness of the negative electrode sheet surface and the battery cell, and further improving the cycle performance and safety performance of the battery.

[0102] In some embodiments, the molar percentage of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%. Specifically, the molar percentage of acrylonitrile in the modified hydrogenated nitrile rubber and / or its derivatives can be 20%, 25%, 30%, 35%, 40%, 41%, 42%, 43%, 44% or 45%, etc., and of course, it can also be other values ​​between 20% and 45%, which are not limited here.

[0103] In some embodiments, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4). Specifically, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material can be 2:2:4, 2:3:4, 2:4:3, 2:4:4, 3:2:4, 3:3:4, 3:4:3, 4:2:4 or 4:4:2, etc., which is not limited here. Preferably, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-3): (3-4): (3-4).

[0104] In some embodiments, the solid content of the elastic functional layer slurry is 5wt% to 10wt%, specifically 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt% or 10wt%, etc., and of course it can also be other values ​​within the above range, which is not limited here.

[0105] In some embodiments, the conductive material of the elastic functional layer includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene.

[0106] Figure 5 A schematic diagram of the conductive performance of the elastic functional layer of the negative electrode provided in this application, such as Figure 5 As shown, it can be understood that the conductive material is evenly dispersed in the elastic functional layer, so that the elastic functional layer has excellent conductivity and equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be evenly dispersed, promoting the uniform deposition of ions, improving the cycle life and safety performance of the battery, and providing an electron path for the lithium insertion / extraction / replenishment process; the conductive material can also improve the electronic conductivity of the electrode without providing additional capacity and causing additional chemical reactions; in addition, the conductive material can also reduce the impedance of the negative electrode and improve the battery rate performance.

[0107] In some embodiments, the thickness of the negative electrode current collector is 5 μm to 15 μm, specifically 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, etc., and of course, it can also be other values ​​within the above range, which is not limited here.

[0108] In some embodiments, the thickness of the negative electrode active material layer is 10 μm to 70 μm. Specifically, the thickness of the negative electrode active material can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 65 μm or 70 μm, etc., which is not limited here.

[0109] In some embodiments, the thickness of the elastic functional layer is 1 μm to 5 μm, specifically 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm 4 μm, 4.5 μm or 5 μm, etc. Of course, it can also be other values ​​within the above range, which are not limited here. It can be understood that if the elastic functional layer is too thin, the elastic functional layer may not cover the negative electrode material layer perfectly, and it cannot buffer the volume expansion of the negative electrode sheet and improve the interface bonding performance between the negative electrode sheet and the diaphragm; if the elastic functional layer is too thick, it is equivalent to increasing the thickness of the negative electrode sheet in disguise, which will cause the overall energy density of the battery cell to decrease, which is not conducive to the improvement of the energy density of the lithium-ion battery. Therefore, controlling the thickness of the elastic functional layer within the above range can, on the one hand, alleviate the volume expansion of the negative electrode sheet during the cycle; on the other hand, it is also beneficial to improve the energy density of the lithium-ion battery. Preferably, the thickness of the elastic functional layer is 2 μm to 3 μm.

[0110] In some embodiments, the negative electrode active material layer includes a negative electrode active material. Specifically, the negative electrode active material includes a silicon-based material, and the silicon-based material is selected from at least one of elemental silicon, silicon oxide, silicon carbon composite, silicon nitrogen composite and silicon alloy. Exemplarily, the silicon oxide can be silicon monoxide.

[0111] In some embodiments, the silicon-carbon composite can be a silicon-carbon composite material obtained by carbon coating a silicon material, a silicon-carbon composite material obtained by sintering a silicon material, a silicon-carbon composite material obtained by ball milling a silicon material and a carbon material, or a silicon-carbon composite material obtained by chemical vapor deposition a silicon material and a carbon material, etc., and is not limited here.

[0112] In some embodiments, the negative electrode active material may further include a phosphorus-based material, wherein the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite. Exemplarily, the elemental phosphorus includes at least one of red phosphorus, black phosphorus, purple phosphorus, or blue phosphorus.

[0113] In some embodiments, the phosphorus-carbon composite is prepared by compounding elemental phosphorus and a carbon material by ball milling or vapor deposition, and the carbon material includes at least one of graphite, carbon nanotubes, porous carbon, hard carbon, soft carbon or graphene, which is not limited here.

[0114] In some embodiments, the negative electrode active material also includes a carbon-based negative electrode material, the carbon-based negative electrode material includes at least one of graphite, hard carbon, soft carbon, carbon nanotubes and graphene, and the graphite includes at least one of natural graphite, artificial graphite and surface-modified natural graphite.

[0115] In some embodiments, the negative electrode active material layer further includes a binder, and the binder includes at least one of carboxymethyl cellulose, styrene-butadiene rubber, polyimide, polyacrylic acid, polyacrylonitrile, and polyvinyl alcohol. It can be understood that the binder can bond the negative electrode active material, the conductive material, and the negative electrode current collector to enhance the contact between the negative electrode active material and the conductive material and the negative electrode current collector, while also ensuring the integrity of the pole piece structure and ensuring that the battery cycle charge and discharge can proceed normally.

[0116] In a third aspect, the present application provides an electrochemical device, the electrochemical device comprising the negative electrode sheet described in the second aspect. It can be understood that in addition to the negative electrode sheet, the above electrochemical device generally also includes a positive electrode sheet, a separator and an electrolyte; the positive electrode sheet includes a positive electrode active material, a conductive material and a binder, wherein the positive electrode active material includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate or a ternary material; the conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene; the binder is polyvinylidene fluoride (PVDF).

[0117] In the above electrochemical device, the electrolyte includes a lithium salt and a solvent, the lithium salt includes at least one of lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium trifluoromethylsulfonate (LiCF3SO3); the solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC). The electrolyte also includes additives, and the type of additives is not particularly limited. It can be a negative electrode film-forming additive, a positive electrode film-forming additive, or an additive that can improve certain battery properties, such as an additive that improves the battery overcharge performance, an additive that improves the battery high temperature performance, an additive that improves the battery low temperature performance, etc.

[0118] In a specific embodiment, the electrochemical device may be a primary battery, a secondary battery, a solid-state battery or a lithium-ion battery, which is not limited here.

[0119] In a fourth aspect, the present application further provides an electronic device, wherein the electronic device is the electrochemical device described in the third aspect. The electrochemical device of the present application has good cycle performance and safety performance, and therefore, the above electrochemical device is applied in the electronic device, so that the electronic device has good safety performance and can also extend the service life of the electronic device.

[0120] The electronic device in this application can specifically be a mobile phone, a computer, a tablet computer, a smart bracelet, a smart watch, etc., and is not limited here.

[0121] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application should be included in the scope of protection of the present application.

[0122] The present application is further described below by taking lithium-ion batteries as an example through specific embodiments and comparative examples.

[0123] Example 1

[0124] (1) Preparation of slurry for negative electrode sheet (elastic functional layer slurry)

[0125] 1.0 g of raw materials of polyfluoroolefin polymers (including 80 mol% of vinylidene fluoride and 20 mol% of monomers containing polar functional groups, CH2=CHCOOCH3) and 2.0 g of modified hydrogenated nitrile rubber (including 36% of acrylonitrile) were added to 95 g of N-methylpyrrolidone (NMP) and stirred at room temperature until the reactants were completely dissolved. Then 2.0 g of conductive carbon black was added and stirred at room temperature for 24 h to obtain an elastic functional layer slurry with a solid content of 5 wt%.

[0126] (2) Preparation of negative electrode sheet

[0127] 80g SiO (Shin-Etsu Chemical) and 10g SP conductive carbon black were added to 70g modified polyacrylic acid binder solution (Chengdu Indile PAA, solid content 7wt%), stirred and mixed for 10min, deionized water was added to adjust the solid content and viscosity, and stirred evenly to obtain a uniform negative electrode slurry; the negative electrode slurry was coated on one surface of a 10μm thick copper foil current collector, and dried at 100°C for 12h to obtain a negative electrode active material layer. After that, the above steps were repeated on the other surface of the negative electrode sheet, and after rolling and sheeting, a negative electrode sheet with a negative electrode active material layer on both sides was obtained, wherein the compaction density of the negative electrode sheet was 1.2g / cm 3 , active substance loading is 3mg / cm 2 .

[0128] Then, the elastic functional layer slurry is coated on the surface of one of the negative electrode active material layers, and dried at 85°C for 20 minutes to obtain an elastic functional layer with a single-side thickness of 2μm. After that, the above steps are repeated on the other surface of the negative electrode sheet to obtain a negative electrode sheet with a negative electrode active material layer and an elastic functional layer on both sides. After that, the negative electrode sheet is physically replenished with lithium, and a metal lithium foil is rolled onto the surface of the elastic functional layer (the thickness of the metal lithium foil is determined by the amount of lithium replenishment, and the thickness is adjustable), and then left to stand.

[0129] (3) Production of positive electrode

[0130] 97g of lithium cobalt oxide, 0.5g of carbon nanotubes, and 2.5g of polyvinylidene fluoride (PVDF) were mechanically mixed, and then N-methylpyrrolidone (NMP) was added as a solvent to prepare a slurry with a solid content of 65wt%, and stirred evenly to obtain a uniform positive electrode slurry. The positive electrode slurry was coated on one surface of an aluminum foil current collector with a thickness of 12μm and dried at 90°C. After the above steps were completed, the single-sided coating of the positive electrode sheet was completed. After that, the above steps were repeated on the other surface of the positive electrode sheet. After roller pressing, a positive electrode sheet with a double-sided coating of positive electrode active materials was obtained, wherein the compaction density of the positive electrode sheet was 4.0g / cm 3, the active material loading matches the negative electrode active material loading, N / P = 1.1.

[0131] (4) Production of lithium-ion batteries

[0132] The positive electrode sheet, separator (Celgard 2400), and negative electrode sheet prepared above are stacked in order to obtain a bare cell. The bare cell is placed in an aluminum-plastic film packaging bag, and after drying, an electrolyte (a mixed solution of 1 mol / L LiPF6 ethylene carbonate (EC) and diethyl carbonate (EMC) (v / v=1:1), with an FEC addition amount of 10wt%) is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, formation, degassing, and other processes.

[0133] The negative electrode sheet prepared in this embodiment includes a negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector; and an elastic functional layer, wherein the elastic functional layer covers the surface of the negative electrode active material layer; Figure 6 , which is a SEM image of the negative electrode sheet prepared in this embodiment.

[0134] Example 2

[0135] The preparation was carried out according to the preparation method of Example 1, and the difference from Example 1 was that:

[0136] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:2:4, and the rest is the same as in Example 1.

[0137] Example 3

[0138] The preparation was carried out according to the preparation method of Example 1, and the difference from Example 1 was that:

[0139] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 2:3:4. The olefin monomer of the polyfluoroolefin polymer is different, and the rest is the same as in Example 1.

[0140] Example 4

[0141] The preparation was carried out according to the preparation method of Example 1, and the difference from Example 1 was that:

[0142] The thickness of the elastic functional layer is 3 μm, and the rest is the same as in Example 1.

[0143] Example 5

[0144] The preparation was carried out according to the preparation method of Example 1, and the difference from Example 1 was that:

[0145] The thickness of the elastic functional layer is 1 μm. The amount of lithium supplementation in Example 5 is different, and the rest is the same as that in Example 1.

[0146] Example 6

[0147] The preparation was carried out according to the preparation method of Example 1, and the difference from Example 1 was that:

[0148] The negative electrode active material is a black phosphorus-graphite composite (abbreviated as BP) with a mass ratio of 7:3. The amount of lithium supplement in Example 6 is different, and the rest is the same as that in Example 1.

[0149] Example 7

[0150] The preparation was carried out according to the preparation method of Example 6, and the difference from Example 6 was that:

[0151] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:2:4. The olefin monomer of the polyfluoroolefin polymer is different, and the rest is the same as Example 6.

[0152] Example 8

[0153] The preparation was carried out according to the preparation method of Example 6, and the difference from Example 6 was that:

[0154] The thickness of the elastic functional layer is 3 μm, and the rest is the same as that of Example 6.

[0155] Example 9

[0156] The preparation was carried out according to the preparation method of Example 6, and the difference from Example 6 was that:

[0157] During the preparation of the elastic functional layer slurry, the mass ratio of polyfluoroolefin polymer: modified hydrogenated nitrile rubber: conductive material is 3:4:4, and the rest is the same as in Example 6.

[0158] Comparative Example 1

[0159] The difference from Example 1 is that:

[0160] In step (2), during the manufacturing process of the negative electrode plate, the elastic functional layer is not covered on the surface of the negative electrode active material layer.

[0161] Comparative Example 2

[0162] The difference from Example 5 is that:

[0163] In step (2), during the manufacturing process of the negative electrode plate, the elastic functional layer is not covered on the surface of the negative electrode active material layer.

[0164] Comparative Example 3

[0165] The difference from Example 6 is that:

[0166] In step (2), during the manufacturing process of the negative electrode plate, the elastic functional layer is not covered on the surface of the negative electrode active material layer.

[0167] The specific parameter differences between Examples 1 to 9 and Comparative Examples 1 to 3 are shown in Table 1.

[0168] Table 1. Parameters of various embodiments and comparative examples

[0169]

[0170] Performance Test:

[0171] (1) Test of the expansion rate of the negative electrode plate: The lithium-ion batteries of Examples 1 to 9 and Comparative Examples 1 to 3 were subjected to 10 charge and discharge tests, and then charged to different battery states of charge (State of Charge, SOC) (50%, 100%). The batteries were then taken out and the plates were disassembled. The surface of the negative electrode plate was cleaned with dimethyl carbonate solvent and then dried. The thickness of different areas of the negative electrode plate was measured using a micrometer, and the average value was taken. The difference between the average value and the initial thickness of the negative electrode plate was divided by the initial thickness of the negative electrode plate (the thickness of the remaining part after excluding the thickness of the current collector). The value obtained is the expansion rate of the negative electrode plate.

[0172] (2) The first coulombic efficiency test of lithium-ion batteries:

[0173] The first charge and discharge capacities of the soft-pack lithium-ion batteries of the above-mentioned embodiments 1 to 9 and comparative examples 1 to 3 were measured by a blue electricity tester CT3001A, and the first coulomb efficiency was calculated, wherein the first coulomb efficiency = first discharge capacity / first charge capacity×100%.

[0174] (3) Test of lithium-ion battery cycle capacity retention rate:

[0175] The capacity retention rate of the soft-pack lithium-ion batteries of Examples 1 to 9 and Comparative Examples 1 to 3 after 200 cycles at a charge and discharge rate of 0.5C / 0.7C, wherein 0.5C refers to a battery charge C rate (charge and discharge rate) of 0.5C, and 0.7C refers to a battery discharge C rate (charge and discharge rate) of 0.7C.

[0176] (4) Test of electrode peeling force:

[0177] The negative electrode sheets of Examples 1 to 9 and Comparative Examples 1 to 3 were cut into 2 cm × 10 cm strip test specimens, and the electrode sheets were adhered to the side to be tested with 3M double-sided tape, and compacted with a roller to make it completely fit with the electrode sheets; then the other side of the double-sided tape was adhered to the surface of the stainless steel plate, one end of the specimen was bent in the opposite direction with a bending angle of 180 degrees, and the specimen and the stainless steel plate were clamped and stretched respectively with a universal material testing machine, and the force required for stretching was recorded in real time, and the average value of all forces was the peeling force of the negative electrode sheet.

[0178] The performance test results of Examples 1 to 8 and Comparative Examples 1 to 3 are shown in Table 2.

[0179] Table 2. Performance test results of Examples 1 to 8 and Comparative Examples 1 to 3

[0180]

[0181] According to the battery performance test results of Examples 1 to 9 and Comparative Examples 1 to 3 in Table 2, the battery pole piece expansion rate in Examples 1 to 9 is lower, and the first coulomb efficiency and capacity retention rate are higher, indicating that the elastic functional layer in the negative pole piece of the present application can inhibit the volume expansion of the pole piece and improve the cycle performance and safety performance of the lithium-ion battery. The reason is that, first, the elastic functional layer can make the negative pole piece and the diaphragm have excellent bonding effect, which can improve the pole piece stress distribution, alleviate the interface expansion and battery cell deformation problems, thereby further improving the cycle life and safety performance of the battery during actual use; second, the elastic functional layer has excellent elasticity and buffering performance (deformation force < pole piece adhesion and interface shaping force), which can reduce the extrusion and expansion damage of particles to the negative pole piece, alleviate the volume expansion of the negative pole piece during the cycle, and can also alleviate the partial particle shedding and electronic path destruction caused by particle expansion and crushing, and inhibit the cycle caused by active material loss. The capacity attenuation phenomenon can improve the flatness of the surface of the negative electrode, thereby improving the cycle performance and safety performance of the battery; finally, the conductive material in the elastic functional layer makes the elastic functional layer have equipotentiality. When electrons contact the elastic functional layer, the electric field on the surface of the electrode can be dispersed, which promotes electron transmission and reduces the impedance and polarization of the negative electrode; and acts as a lithium replenishment buffer layer to reduce the side reactions of the lithium replenishment interface and improve the lithium replenishment efficiency; in the later stage of the cycle, the elastic functional layer can also ensure the complete electronic path of the electrode, so that the electric field on the surface of the electrode is dispersed, and the uniform deposition of lithium ions is promoted, thereby improving the cycle performance and safety performance of the battery.

[0182] Figure 7a A schematic diagram of the surface flatness of the negative electrode sheet after cycling provided in Example 1 of the present application; Figure 7b This is a SEM image of the negative electrode after cycling provided in Example 1 of the present application, as shown in Figure 7a and Figure 7bAs shown in the figure, it can be seen that the surface of the negative electrode plate in Example 1 after the cycle is relatively flat, and the flatness of the electrode plate is high; Figure 8a A schematic diagram of the surface flatness of the negative electrode plate after cycling provided in Comparative Example 1 of the present application; Figure 8b The SEM image of the negative electrode after cycling provided in Comparative Example 1; Figure 8a and Figure 8b As shown in the figure, it can be seen that the surface of the negative electrode sheet in Comparative Example 1 after cycling is uneven and the flatness of the electrode sheet is low; it can be seen that adding an elastic functional layer to the negative electrode sheet can reduce the extrusion and expansion damage of the negative electrode active material particles to the negative electrode sheet, improve the flatness of the surface of the negative electrode sheet, and keep the surface of the electrode sheet flat after cycling, thereby alleviating the volume expansion of the negative electrode sheet during the cycle, and further improving the cycle performance of the lithium-ion battery.

[0183] Fig. 9 Schematic diagram of the cycle capacity retention rate of the lithium ion battery provided in Example 1 and Comparative Example 1 of the present application, as shown in Fig. 9 As shown, and referring to the battery performance test results of Example 1 and Comparative Example 1, it can be seen that since the lithium-ion soft-pack battery has been hot-pressed, the negative electrode plate and the separator have excellent bonding effect, and the cycle capacity retention rate of the battery in Example 1 is significantly higher than that in Comparative Example 1.

[0184] Further reference to the battery performance test results of Example 5 and Comparative Example 2 shows that for the silicon-based negative electrode system, when the negative electrode sheet has an elastic functional layer, the sheet peeling force remains stable, the initial sheet expansion rate of the negative electrode sheet is reduced by about 10%, the cycle expansion rate of the negative electrode sheet is reduced by about 15%, the first coulomb efficiency is increased by about 5% to 6%, and the capacity retention rate is increased by about 16% to 17%. This shows that the elastic functional layer of the negative electrode sheet can effectively alleviate the volume expansion of the negative electrode sheet, thereby improving the cycle performance and safety performance of the lithium-ion battery.

[0185] According to the performance test results of Example 1 and Example 4, for the silicon-based negative electrode system, increasing the thickness of the elastic functional layer within a certain range is beneficial to improving the lithium replenishment efficiency of the negative electrode plate, while reducing the interface side reactions and thus reducing the cycle expansion rate of the plate, thereby improving the cycle performance of the battery.

[0186] According to the performance test results of Example 1 and Example 5, there is a design space for the amount of lithium supplementation for the elastic functional layer. Reducing the amount of lithium supplementation is beneficial to reducing the initial and cycle expansion rate of the negative electrode plate, but the cycle capacity retention rate of the lithium-ion battery is limited.

[0187] According to the battery performance test results of Example 6 and Comparative Example 3, for the phosphorus-based negative electrode system, when the negative electrode plate has an elastic functional layer, the initial expansion rate of the negative electrode plate is reduced by about 7%, the cycle expansion rate of the negative electrode plate is reduced by about 10%, the first coulomb efficiency is increased by about 5%, and the capacity retention rate after 200 cycles is increased by 17%. This shows that the elastic functional layer of the negative electrode plate can effectively alleviate the volume expansion of the negative electrode plate, thereby improving the cycle performance and safety performance of the lithium-ion battery.

[0188] According to the battery performance test results of Example 6 and Example 8, for the phosphorus-based negative electrode system, increasing the thickness of the elastic functional layer is beneficial to reducing the cycle expansion rate of the electrode piece and improving the cycle capacity rate of the battery.

[0189] In summary, the elastic functional layer in the negative electrode plate can effectively alleviate the stress layout of the plate, reduce the initial expansion rate of the plate, and at the same time, reduce the side reaction of lithium replenishment and improve the efficiency of lithium replenishment; it can also reduce the interfacial side reaction during the battery cycle, balance polarization, reduce the cycle expansion rate of the plate, and greatly improve the battery's cycle capacity retention rate, thereby improving the battery's cycle performance and safety performance.

Claims

1. A slurry for a negative electrode sheet, characterized in that: The slurry comprises a conductive material, a polyfluoroolefin polymer, a modified hydrogenated nitrile rubber and a solvent.

2. The slurry according to claim 1, characterized in that The polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

3. The slurry according to claim 2, characterized in that The fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, ethylene fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene; and / or, The general structural formula of the olefin monomer containing polar functional groups is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

4. The slurry according to any one of claims 1 to 3, characterized in that The slurry meets at least one of the following characteristics: (1) Based on the total mass of the components in the slurry excluding the solvent, the mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4); (2) The solid content of the slurry is 5wt% to 10wt%; (3) The modified hydrogenated nitrile rubber contains acrylonitrile, and the mass content of acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%; (4) The viscosity of the slurry is 100 cP to 2000 cP; (5) The conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene; (6) The solvent is selected from at least one of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, n-hexane or N-methylpyrrolidone.

5. A negative electrode plate, characterized in that: The negative electrode plate comprises: A negative electrode current collector, a negative electrode active material layer disposed on the negative electrode current collector; and An elastic functional layer is covered on the surface of the negative electrode active material layer, and the elastic functional layer comprises a conductive material, a polyfluoroolefin polymer and a modified hydrogenated nitrile rubber.

6. The negative electrode sheet according to claim 5, characterized in that: The polyfluoroolefin polymer is obtained by polymerizing 20% ​​to 60% by mole of a fluorine-containing olefin monomer and 40% to 80% by mole of an olefin monomer containing a polar functional group.

7. The negative electrode sheet according to claim 6, characterized in that: It meets at least one of the following characteristics: (1) The fluorine-containing olefin monomer includes at least one of vinylidene fluoride, vinylidene fluoride, vinyl fluoride, trifluoroethylene, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene; (2) The general structural formula of the olefin monomer containing a polar functional group is R1CH=CR1R2, wherein R1 is selected from H or CH3, and R2 is selected from at least one of COOH, COOLi, COOCH3, COOCH2CH3, CONH2, CONHCH3, CONHCH2CH3 or CN.

8. The negative electrode sheet according to claim 5, characterized in that: The modified hydrogenated nitrile rubber is obtained by polymerizing ethylene and acrylonitrile.

9. The negative electrode sheet according to claim 8, characterized in that: The molar proportion of the acrylonitrile in the modified hydrogenated nitrile rubber is 20% to 45%.

10. The negative electrode sheet according to claim 5, characterized in that: The negative electrode plate meets at least one of the following characteristics: DD230916I-MS (1) The thickness of the negative electrode current collector is 5 μm to 15 μm; (2) The thickness of the negative electrode active material layer is 10 μm to 70 μm; (3) The thickness of the elastic functional layer is 1 μm to 5 μm; (4) The mass ratio of the polyfluoroolefin polymer, the modified hydrogenated nitrile rubber and the conductive material is (2-4): (2-4): (2-4).

11. The negative electrode sheet according to claim 5, characterized in that: The negative electrode plate includes a negative electrode active material, which satisfies at least one of the following characteristics: (1) The negative electrode active material comprises a silicon-based material, wherein the silicon-based material is selected from at least one of elemental silicon, silicon-oxygen compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys; (2) The negative electrode active material includes a phosphorus-based material, and the phosphorus-based material includes at least one of elemental phosphorus and a phosphorus-carbon composite; (3) The conductive material includes at least one of conductive graphite, conductive carbon black, acetylene black, carbon nanotubes and graphene.

12. An electrochemical device, characterized in that The electrochemical device comprises the negative electrode sheet according to any one of claims 5 to 11.

13. An electronic device, characterized in that: The electronic device comprises the electrochemical device according to claim 12.

Citation Information

Cited By

  • Negative electrode for lithium secondary battery and lithium secondary battery comprising same