Composite current collector and preparation method thereof, negative plate, battery and electric device
By using a polymer layer composed of porous polyimide, surface modified boride and carboxyl-containing binder in a lithium-ion battery, the problems of poor conductivity of the composite liquid collector and low peel strength of the metal layer are solved, and the battery is realized Reduced internal resistance and improved cycling performance.
Patent Information
- Application Number
- CN202411252272.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
The poor conductivity of the existing composite fluid collector and the low peel strength between the metal layer and the polymer layer lead to an increase in internal resistance and a decrease in cycling performance of lithium-ion batteries.
The polymer layer composed of porous polyimide, surface modified boride and carboxyl-containing binder improves conductivity through hydrogen bonding and ester group connection, and enhances the metal layer and polymer layer during the electrodeposition process. Peel strength.
It effectively reduces the internal resistance of the battery and improves energy density and cycling performance.
Smart Images

Figure BDA0005033639940000141 
Figure BDA0005033639940000151
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a composite current collector and a preparation method thereof, a negative electrode sheet, a battery and an electrical device. Background Art
[0002] Lithium-ion batteries are widely used in all aspects of human life due to their advantages such as high specific energy, long cycle life, no memory and low self-discharge rate. In the field of 3C electronic products (computers, communications and consumer electronics), lithium-ion batteries almost occupy the entire market. Against the background of the country's dual carbon goals of "carbon peak" and "carbon neutrality", electric vehicles (electric vehicles, electric bicycles, electric ships, electric rails) will also be further developed, which is undoubtedly a huge opportunity for lithium-ion batteries.
[0003] Energy density is an important indicator of lithium-ion batteries. The greater the energy density of a battery, the more electricity it can store per unit volume or weight, and the longer the battery life it can provide when used in new energy vehicles. Therefore, it is particularly important to improve the energy density of lithium-ion batteries.
[0004] Reducing the weight of the current collector is an important way to increase the energy density of lithium-ion batteries, so composite current collectors were born. Composite current collectors are a new type of composite current collector that uses organic polymer materials such as PET / PP as a support layer, deposits metals (copper or aluminum) on the upper and lower surfaces, and is plated into a "metal conductive layer-PET / PP polymer material support layer-metal conductive layer" sandwich structure. Since the middle layer of the composite current collector is a lighter polymer layer, the energy density of the battery can be effectively improved. However, since the middle layer is a polymer layer, the conductivity of the composite current collector is poor, which leads to an increase in the internal resistance of the battery. At the same time, since the metal layer is magnetron sputtered or electroplated on the surface of the polymer layer, the peeling strength between the metal layer and the polymer layer is low, resulting in a decrease in the cycle performance of the battery.
[0005] Therefore, a new composite current collector is urgently needed to solve the above problems. Summary of the invention
[0006] In order to solve the problems of the prior art, the present application provides a composite current collector and a preparation method, a negative electrode sheet and an electrical device, which can reduce the internal resistance of the battery and enhance the peel strength between the metal layer and the polymer layer, thereby enhancing the cycle performance of the battery.
[0007] In the first aspect, the present application provides a composite current collector, comprising a polymer layer and a metal layer arranged on both sides of the polymer layer, wherein the polymer layer comprises a porous polyimide, a boride and a binder, wherein the boride contains hydroxyl groups and the binder contains carboxyl groups; the hydroxyl groups in the porous polyimide and the hydroxyl groups in the boride are connected by hydrogen bonds, the carboxyl groups in the porous polyimide and the hydroxyl groups in the boride are connected by ester groups, the carboxyl groups in the porous polyimide and the binder are connected by hydrogen bonds, and the hydroxyl groups in the porous polyimide and the binder are connected by ester groups.
[0008] In some embodiments, the surface of the boride has a hydroxyl group, and the boride includes at least one of MoB, CrB, MnB, FeB, FeB2, V3B4, Nb3B4, and Mo2B.
[0009] In some embodiments, the thickness ratio of the polymer layer to the metal layer is (1:2) to (1:6);
[0010] and / or,
[0011] The thickness of the polymer layer is 3 to 10 μm;
[0012] and / or,
[0013] The thickness of the metal layer is 0.5-2.5 μm.
[0014] In some embodiments, the mass ratio of the boride, the binder, and the porous polyimide in the polymer layer is (4:1:50) to (6:1:70).
[0015] In a second aspect, the present application provides a method for preparing a composite current collector as described in any one of the first aspects, comprising:
[0016] S1: adding a boron salt into an alkaline solution to perform an etching reaction to obtain a first intermediate;
[0017] S2: subjecting the supernatant of the first intermediate to ultrasonication, washing, and freeze-drying in sequence to obtain a second intermediate, wherein the second intermediate is a boride with a surface modified with a hydroxyl group;
[0018] S3: adding the second intermediate and the binder to the amino source, wherein the mass ratio of the second intermediate to the binder is (200-800): (50-150), and mixing them uniformly to obtain a third intermediate; adding a carboxyl source to the third intermediate, mixing them uniformly, dissolving them in a solvent, and performing ultrasonic treatment; adding an acid at a first preset temperature and reacting for a first preset time to obtain a fourth intermediate containing carboxyl groups on the surface;
[0019] S4: coating the fourth intermediate on a substrate for drying, and then heating under an inert gas atmosphere for imidization to obtain a polymer layer.
[0020] S5: Plating a metal coating on the surface of the polymer layer to obtain the composite current collector.
[0021] In some embodiments, the boron salt comprises MoBTx, wherein Tx comprises a hydroxyl group, and the alkali solution comprises a NaOH solution;
[0022] The amino source includes amine substances containing two or more amino groups;
[0023] and / or,
[0024] The carboxyl source includes pyromellitic dianhydride;
[0025] and / or,
[0026] The binder includes polyacrylic acid;
[0027] and / or,
[0028] The acid includes at least one of acetic acid, sulfuric acid and phosphoric acid;
[0029] and / or,
[0030] The first preset temperature is 100-140°C;
[0031] and / or,
[0032] The first preset time is 3 to 7 hours.
[0033] In some embodiments, the fourth intermediate is coated on a substrate for drying, and then heated under an inert gas atmosphere for imidization to obtain a polymer layer, comprising:
[0034] The fourth intermediate is coated on a glass substrate, dried in a vacuum oven at 30 to 70° C. for 6 to 10 hours, and then heated in an inert gas atmosphere at 280 to 400° C. for 3 to 7 hours for imidization to obtain the polymer layer;
[0035] and / or,
[0036] The step of plating a metal coating on the surface of the polymer layer to obtain the composite current collector comprises:
[0037] The polymer layer is used as a working electrode, a platinum sheet and an Ag / AgCl electrode are used as a counter electrode and a reference electrode respectively, and electroplating is performed for 300 to 900 seconds at a constant potential of -1.4 to -0.8 V in a 0.2 to 0.8 mol / L copper sulfate solution to plate a metal coating on the surface of the polymer layer to obtain the composite current collector.
[0038] In a third aspect, the present application further provides a negative electrode sheet, comprising the composite current collector described in any one of the first aspects.
[0039] In a fourth aspect, the present application further provides a battery, comprising a positive electrode sheet, the negative electrode sheet described in the third aspect, and an electrolyte.
[0040] In a fifth aspect, the present application also provides an electrical device, comprising the battery described in the fourth aspect.
[0041] The present application provides a composite current collector and a preparation method, a negative electrode sheet, a battery and an electrical device. By including a polymer layer containing a porous polyimide, a surface-modified boride and a carboxyl-containing binder, the conductivity of the composite current collector can be effectively improved, and the peel strength between the polymer layer and the metal layer can be enhanced, thereby effectively reducing the internal resistance of the battery, improving the battery energy density, and enhancing the battery cycle performance. Specifically, the surface-modified boride can reduce the resistance of the composite current collector, thereby reducing the internal resistance of the battery, and the carboxyl-containing binder can enhance the peel strength between the metal layer and the polymer layer, thereby enhancing the battery cycle performance.
[0042] Furthermore, in the present application, the polymer layer contains more hydrophilic groups such as hydroxyl and carboxyl, which can better absorb the copper sulfate solution during the electrodeposition process. At the same time, the porous structure can provide a larger reactive active area, which is beneficial to the deposition of copper.
[0043] Furthermore, in the present application, the modified polymer layer contains a binder, which can enhance the peel strength between the metal layer and the polymer layer, thereby enhancing the battery cycle performance. DETAILED DESCRIPTION
[0044] Some embodiments of the present application are described below. Those skilled in the art should understand that these embodiments are only used to explain the technical principles of the present application and are not intended to limit the protection scope of the present application.
[0045] As described in the background technology, in order to increase the amount of electricity stored in a battery per unit volume or weight and improve the lithium ion energy density, a composite current collector is usually used to reduce the weight of the current collector. The middle layer of the composite current collector uses a lighter polymer layer. However, since the middle layer of the composite current collector is a polymer layer, the conductivity of the composite current collector is poor, which leads to an increase in the internal resistance of the battery. At the same time, since the metal layer is magnetron sputtered or electroplated on the surface of the polymer layer, the peel strength between the metal layer and the polymer layer is low, resulting in a decrease in the cycle performance of the battery.
[0046] In order to solve the above problems, the present application creatively proposes a composite current collector and preparation method, a negative electrode sheet and an electrical device, which can reduce the internal resistance of the battery and enhance the peel strength between the metal layer and the polymer layer, thereby enhancing the cycle performance of the battery.
[0047] The following are optional technical solutions for this application, but are not intended to limit the technical solutions provided in this application. Through the following optional technical solutions, the technical objectives and beneficial effects of this application can be better achieved and realized.
[0048] In the first aspect, the present application provides a composite current collector, comprising a polymer layer and a metal layer arranged on both sides of the polymer layer, wherein the polymer layer comprises a porous polyimide, a boride and a binder, wherein the boride contains hydroxyl groups and the binder contains carboxyl groups; the hydroxyl groups in the porous polyimide and the hydroxyl groups in the boride are connected by hydrogen bonds, the carboxyl groups in the porous polyimide and the hydroxyl groups in the boride are connected by ester groups, the carboxyl groups in the porous polyimide and the binder are connected by hydrogen bonds, and the hydroxyl groups in the porous polyimide and the binder are connected by ester groups.
[0049] In a specific embodiment, the surface of the boride has hydroxyl groups, and the boride includes at least one of MoB, CrB, MnB, FeB, FeB2, V3B4, Nb3B4, and Mo2B. Mo boride can enhance conductivity, has a large specific surface area, and can also better deposit Cu. There are abundant -OH groups on the surface of the boride, indicating that there is a chemical bond between the surface functional groups of the boride and the polymer PI.
[0050] In a specific embodiment, the thickness ratio of the polymer layer to the metal layer is (1:2) to (1:6). Schematically, the thickness ratio of the polymer layer to the metal layer can be 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1.5:2, 2:1, 2:3, 2:5, 2:6, and any specific ratio within the above ratio range. Due to space limitations and for the sake of simplicity, this application no longer exhaustively lists the specific ratios included in the range. The thickness of the polymer layer is 3 to 10 μm. Exemplarily, the thickness of the polymer layer is 3 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, and specific point values between the above point values. Due to space limitations and for the sake of simplicity, this application no longer exhaustively lists the specific point values included in the range. The thickness of the metal layer is 0.5 to 2.5 μm. Exemplarily, the thickness of the metal layer is 0.5 μm, 1 μm, 1.3 μm, 1.8 μm, 2 μm, 2.2 μm, 2.5 μm and specific values between the above-mentioned points. Due to limited space and for the sake of brevity, this application no longer exhaustively lists the specific points included in the range.
[0051] In a specific embodiment, the mass ratio of the boride, the binder and the porous polyimide in the polymer layer is (4:1:50) to (6:1:70). Illustratively, the mass ratio of the boride, the binder and the porous polyimide in the polymer layer can be 4:1:50, 4.3:1:51, 4.5:1:58, 4.6:1:67, 4:1:65, 4.1:1:68, 5:1:66, 5:1:70, 6:1:56, 6:1:65, 6:1:70, and any specific ratio within the above ratio range. Due to space limitations and for simplicity, this application no longer exhaustively lists the specific ratios included in the range.
[0052] In a second aspect, the present application also provides a method for preparing a composite current collector, comprising:
[0053] S1: Adding a boron salt into an alkaline solution to perform an etching reaction to obtain a first intermediate.
[0054] S2: The supernatant of the first intermediate is subjected to ultrasonication, washing, and freeze-drying in sequence to obtain a second intermediate, wherein the second intermediate is a boride with a surface modified with hydroxyl groups.
[0055] Exemplarily, the supernatant of the first intermediate is ultrasonically treated at a power of 200 to 280 W for 15 to 45 minutes, and then centrifugally washed with deionized water until the pH is about 7, and the washing is stopped. The washed supernatant is freeze-dried to obtain the second intermediate, which is a boride flocculent solid with a hydroxyl group modified on the surface.
[0056] S3: adding the second intermediate and a binder to an amino source, wherein the mass ratio of the second intermediate to the binder is (200-800):(50-150), and mixing them evenly to obtain a third intermediate; adding a carboxyl source to the third intermediate, mixing them evenly, and dissolving them in a solvent for ultrasonic treatment; adding an acid at a first preset temperature and reacting for a first preset time to obtain a fourth intermediate having carboxyl groups on its surface.
[0057] Exemplarily, the mass ratio of the second intermediate to the binder is 200:50, 200:90, 300:50, 300:80, 400:60, 400:100, 500:70, 500:110, 600:55, 700:120, 750:135, 800:150 and any specific ratio within the above ratio range. Due to space limitations and for simplicity, this application will no longer exhaustively list the specific ratios included in the range. The solvent is DMSO.
[0058] S4: coating the fourth intermediate on a substrate for drying, and then heating under an inert gas atmosphere for imidization to obtain a polymer layer.
[0059] S5: Plating a metal coating on the surface of the polymer layer to obtain the composite current collector.
[0060] Further, the boron salt includes MoBTx, wherein Tx contains a hydroxyl group, and the alkali solution includes a NaOH solution. The alkali solution can also be at least one or more of potassium hydroxide, lithium hydroxide and calcium hydroxide. The amino source includes an amine substance containing two or more amino groups, which can be at least one of 4-4' p-aminoanisole, aliphatic amines and aromatic amines, preferably one or more of ethylenediamine, melamine, butanediamine, propylenediamine, p-phenylenediamine and phthalic acid. The carboxyl source includes benzenetetracarboxylic anhydride. The binder includes polyacrylic acid. The acid includes at least one of acetic acid, sulfuric acid and phosphoric acid. The first preset temperature is 100 to 140°C. The first preset time is 3 to 7 hours.
[0061] Furthermore, step S4 specifically includes: coating the fourth intermediate on a glass substrate, drying in a vacuum oven at 30-70° C. for 6-10 hours, and then heating in an inert gas atmosphere at 280-400° C. for 3-7 hours for imidization to obtain the polymer layer.
[0062] Exemplarily, the fourth intermediate coating glass is further thermally imidized by heat treatment in a tube furnace at 340° C. (280-400° C.) under argon at a heating rate of 4° C. / min (2-6° C.) for 5 h (3-7 h) to form a modified polyimide film.
[0063] Step S5 specifically includes:
[0064] The polymer layer is used as a working electrode, a platinum sheet and an Ag / AgCl electrode are used as a counter electrode and a reference electrode respectively, and electroplating is performed for 300 to 900 seconds at a constant potential of -1.4 to -0.8 V in a 0.2 to 0.8 mol / L copper sulfate solution to plate a metal coating on the surface of the polymer layer to obtain the composite current collector.
[0065] Exemplarily, the polymer layer obtained in step S4, i.e. the modified polyimide film, is used as a working electrode using the electrolytic cell principle, and a platinum sheet and an Ag / AgCl electrode are used as a counter electrode and a reference electrode, respectively. They are immersed in a 0.5 mol / L copper sulfate solution containing a sulfuric acid solution, and are electroplated at a constant potential of -1.1 V (relative to the Ag / AgCl electrode) for 600 seconds to obtain a metal layer, i.e. a copper layer, on the surface of the modified polyimide film. The surface is then lightly rinsed with anhydrous ethanol and then vacuum dried at 25 to 45° C. for 8 to 16 hours to obtain a composite current collector.
[0066] In a third aspect, the present application also provides a negative electrode sheet, comprising the above-mentioned composite current collector.
[0067] In the embodiment of the present application, the negative electrode sheet includes the above-mentioned composite current collector and the negative electrode active material coated on the surface of the composite current collector. The negative electrode active material can be attached to one side or both sides of the negative electrode current collector. The negative electrode active material includes at least one of graphite, hard carbon, soft carbon and carbon fiber material.
[0068] In a fourth aspect, the present application also provides a battery, comprising a positive electrode sheet, the above-mentioned negative electrode sheet and an electrolyte.
[0069] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, a positive electrode conductive agent and a positive electrode binder.
[0070] There is no particular restriction on the positive electrode current collector in the embodiments of the present application, as long as it has conductivity and does not cause chemical changes in the battery. Specifically, the positive electrode current collector includes but is not limited to any one of aluminum, nickel or stainless steel, such as the positive electrode current collector is aluminum foil, etc. The shape of the positive electrode current collector includes but is not limited to metal foil, metal grid, metal mesh, etc., and the user can choose according to actual needs, and no specific limitation is made here.
[0071] The positive electrode active material is a compound that can reversibly intercalate and deintercalate lithium. The positive electrode active material in the present application can be any positive electrode active material known in the art.
[0072] The positive electrode conductor is a material that provides conductivity without causing adverse chemical reactions in the battery. In the embodiment of the present application, the positive electrode conductor may include a carbon-based material, powdered nickel or other metal particles or a conductive polymer. The carbon-based material may include particles such as carbon black, graphite, super-P, acetylene black (such as KETCHENTM black or DENKATM black), carbon fibers and nanotubes, graphene, etc. Examples of conductive polymers include polyaniline, polythiophene, polyacetylene, polypyrrole, poly (3,4-ethylenedioxythiophene) polystyrene sulfonate, etc. Preferably, the positive electrode conductor includes one or more of conductive carbon black (Super-P), acetylene black, Ketjen black, carbon nanotubes (CNTs), graphene (rGO), activated carbon, and carbon nanofibers (CNFs).
[0073] The positive electrode binder is a component that helps the positive electrode active material and the positive electrode conductor to bond with each other and with the positive electrode current collector. In the embodiment of the present application, the positive electrode binder includes but is not limited to polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), styrene butadiene styrene copolymer (SBS), lithium polyacrylate (LiPAA), sodium polyacrylate (NaPAA), sodium alginate, lithium alginate. One or more. Users can choose according to actual needs, and no specific limitation is made here.
[0074] In the embodiment of the present application, the electrolyte includes an organic solvent and a lithium salt, wherein the organic solvent may use any organic solvent without particular limitation, as long as it can serve as a medium through which ions participating in the electrochemical reaction of the battery can move. Specifically, as organic solvents, there can be used: ester solvents, such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents, such as dibutyl ether or tetrahydrofuran; ketone solvents, such as cyclohexanone; aromatic hydrocarbon solvents, such as benzene or fluorobenzene; carbonate solvents, such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents, such as ethanol or isopropanol; nitriles, such as R-CN (wherein R is a linear, branched or cyclic C2-C20 hydrocarbon group, and may include a double bond aromatic ring or an ether bond); amides, such as dimethylformamide; dioxolanes, such as 1,3-dioxolane; or cyclopentane sulfones.
[0075] In a fifth aspect, the present application also provides an electrical device, which includes the above-mentioned battery. The electrical device includes but is not limited to mobile devices, electric vehicles, spacecraft, electric toys, and electric tools. Mobile devices can be mobile phones, laptops, etc.; electric vehicles can be pure electric vehicles, hybrid electric vehicles, electric bicycles, etc.; spacecraft can be airplanes, rockets, spacecrafts, etc.; electric toys can be game consoles, electric car toys, electric ship toys, and electric airplane toys, etc.; electric tools can be metal cutting electric tools, grinding electric tools, assembly electric tools, etc.
[0076] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents and instruments used, they are all conventional products that can be purchased commercially.
[0077] The embodiments of the present application will be described in more detail below through examples. However, the embodiments of the present application are not limited to these examples.
[0078] Embodiment 1:
[0079] 1) Preparation of composite current collector:
[0080] (a) Synthesis of MoBTx (wherein Tx includes hydroxyl groups): First, 2 g of MoAlB was weighed into a reaction kettle, and then 30 ml of NaOH solution was added thereto, and etching was performed at room temperature for 24 h. After etching, the supernatant was extracted and ultrasonicated at 240 W for 30 min, and then centrifuged and washed with deionized water until the pH was about 7, and then the washing was stopped. The washed supernatant was freeze-dried to obtain MoBTx flocculent solid.
[0081] (b) Preparation of modified PI nanosheets: First, 500 mg of the MoBTx flocculent solid prepared above was added to 4-4'-p-aminoanisole, and 100 mg of polyacrylic acid was added thereto, and the three were fully mixed. Then, the mixture of the MoBTx, polyacrylic acid and 4-4'-p-aminoanisole was added to pyromellitic anhydride, and the mixture was mixed at a molar ratio of 1.54:1, dissolved in DMSO and ultrasonically treated, and 30 wt% acetic acid was added at 120 ° C for 5 h to make its surface contain a large number of carboxyl groups, thereby obtaining an intermediate rich in carboxyl groups. The intermediate solution was uniformly coated on the original glass substrate. Then it was dried in a vacuum oven at 50 ° C for at least 8 h. The intermediate coated glass was further thermally imidized by heat treatment at 340 ° C in argon in a tube furnace at a heating rate of 4 ° C / min for 5 h. Finally, the fully acylated polyimide film was peeled off from the glass substrate to obtain the desired polyimide film.
[0082] (c) Using the electrolytic cell principle, the modified polyimide film obtained in step (b) is used as a working electrode, a platinum sheet and an Ag / AgCl electrode are used as a counter electrode and a reference electrode, respectively, and immersed in a 0.5 mol / L copper sulfate solution containing a sulfuric acid solution. Electroplating is performed at a constant potential of -1.1 V (relative to the Ag / AgCl electrode) for 600 s to obtain a metal layer, i.e., a copper layer, on the surface of the modified polyimide film. The surface is then lightly rinsed with anhydrous ethanol and vacuum dried at 25 to 45° C. for 8 to 16 h to obtain a composite current collector.
[0083] 2) Preparation of negative electrode sheet: Graphite powder, conductive carbon and binder PVDF are mixed in a mass ratio of 8:1:1 to obtain a mixed material, and the mixed material is fully stirred in deionized water to obtain an active slurry of the corresponding negative electrode sheet, and the negative electrode slurry is coated on the composite current collector prepared in step 1), and the obtained electrode sheet contains a main material graphite mass fraction of 80wt%, and dried and pressed to obtain a negative electrode sheet.
[0084] 3) Preparation of positive electrode sheet: nickel cobalt lithium manganese oxide powder, conductive carbon and adhesive PVDF are mixed in a mass ratio of 8:1:1 to obtain a mixed material, the mixed material is fully stirred in NMP to obtain a corresponding active slurry for the positive electrode sheet, the positive electrode slurry is coated on a conventional aluminum foil to obtain a nickel cobalt lithium manganese oxide mass fraction of 80wt% in the electrode sheet, and the positive electrode sheet is obtained by drying and pressing.
[0085] 4) Preparation of electrolyte: Ethylene carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (DEC) are mixed in a volume ratio of 1:1:1, and then fully dried lithium salt LiPF6 is dissolved in a mixed organic solvent at a ratio of 1 mol L-1 to prepare an electrolyte.
[0086] 5) Battery assembly: The negative electrode sheet, separator, positive electrode sheet, etc. are wound or stacked, and then dried, electrolyte injected, packaged, formed, and capacity divided to obtain a lithium-ion battery.
[0087] 6) Physical properties of composite current collectors:
[0088] (a) Tensile strength test: The composite current collector prepared in step 1) was cut into long test samples with a width of 15 mm and a length of 200 mm. The upper and lower ends of the test sample were clamped on a tensile testing machine. The tensile direction was 180° and the tensile speed was 250 mm / min. The sample gauge width was 100 mm. The tensile test was completed until the test sample broke. The tensile strength value of this experiment was obtained on the tensile testing machine.
[0089] (b) Foil surface resistance test: The prepared composite current collector sample foil is placed in a membrane resistance test to obtain the membrane resistance of the corresponding electrode.
[0090] (c) Composite current collector peel strength test: The prepared composite current collector is cut into a certain width, the cut electrode and diaphragm are rolled at the same pressure, and then pasted to an iron plate with double-sided tape. The composite current collector is pulled upward at a speed of 50 mm / min at a horizontal angle of 180°, i.e. perpendicular to the ground, using a tensile testing machine to calculate the peel strength.
[0091] 7) Battery performance test: The prepared battery is subjected to the first coulombic efficiency and cycle capacity retention rate test. The specific test process is as follows:
[0092] (a) Energy density test: The prepared battery was charged at 0.33C to 4.25V, charged at 4.25V constant voltage until the current decreased to 0.05C, and discharged at 0.33C constant current to 2.8V. The obtained discharge capacity was recorded as Q, and the platform voltage of the discharge curve was recorded as U. Then, according to the battery weight m, the energy density of the lithium-ion battery cell was calculated using Q*U / m. The test results are shown in Table 2.
[0093] (b) Cycle capacity retention rate: At 25°C, the battery was first charged to 4.25V at 1C constant current, then charged to current I≤0.05C at 4.25V constant voltage, and the battery 1C charging capacity was recorded as C0. After standing for 15 minutes, it was discharged to 2.8V at 1C constant current, and the discharge capacity of 1 cycle was C1. According to this cycle process, the discharge capacity of 100 cycles was recorded as C100, and the battery capacity retention rate of 100 cycles was obtained. The relevant test results are shown in Table 2.
[0094] Example 2
[0095] The difference between Example 2 and Example 1 is that in step (b) of preparing the composite current collector, the amount of MoBTx added is 200 mg.
[0096] Example 3
[0097] The difference between Example 3 and Example 1 is that in step (b) of preparing the composite current collector, the amount of MoBTx added is 800 mg.
[0098] Example 4
[0099] The difference between Example 4 and Example 1 is that in step (b) of preparing the composite current collector, the amount of polyacrylic acid added is 50 mg.
[0100] Example 5
[0101] The difference between Example 5 and Example 1 is that in step (b) of preparing the composite current collector, the amount of polyacrylic acid added is 150 mg.
[0102] Example 6
[0103] The difference between Example 6 and Example 1 is that in step (c) of preparing the composite current collector, the electrodeposition is performed for 300 seconds.
[0104] Example 7
[0105] The difference between Example 7 and Example 1 is that in step (c) of preparing the composite current collector, the electrodeposition is performed for 900 s.
[0106] Comparative Example 1
[0107] The difference between Comparative Example 1 and Example 1 is that the current collector in the negative electrode sheet adopts commercially available conventional copper foil.
[0108] Comparative Example 2
[0109] The difference between Comparative Example 2 and Example 1 is that MoBTx is not added in the preparation of the composite current collector.
[0110] Comparative Example 3
[0111] The difference between Comparative Example 3 and Example 1 is that polyacrylic acid is not added in the preparation of the composite current collector.
[0112] Comparative Example 4
[0113] The difference between Comparative Example 4 and Example 1 is that MoBTx and polyacrylic acid are not added in the preparation of the composite current collector.
[0114] Comparative Example 5
[0115] The difference between Comparative Example 5 and Example 1 is that acetic acid modification is not used in the preparation of the composite current collector.
[0116] Comparative Example 6
[0117] The difference between Comparative Example 6 and Example 1 is that the negative electrode sheet adopts a commercially available PP layer composite current collector.
[0118] Comparative Example 7
[0119] The difference between Comparative Example 7 and Example 1 is that the negative electrode sheet adopts a commercially available PET layer composite current collector.
[0120] The tensile strength test results of the current collectors in Examples 1 to 7 and Comparative Examples 1 to 7, the surface resistance test results of the foils, and the peel strength test results are shown in Table 1, and the performance test results of the batteries are shown in Table 2.
[0121] Table 1
[0122]
[0123] It can be seen from Table 1 that the composite current collector provided in the present application can have excellent peeling strength while maintaining good tensile strength and surface resistance.
[0124] Table 2
[0125]
[0126] It can be seen from Table 2 that the modified composite current collector battery provided in the present application can obtain better energy density and cycle performance.
[0127] It should be noted that, in this article, the term "comprise" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "including one" do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the method and device in the embodiment of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0128] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A composite current collector, characterized in that: The invention comprises a polymer layer and a metal layer arranged on both sides of the polymer layer, wherein the polymer layer comprises a porous polyimide, a boride and a binder, wherein the boride contains a hydroxyl group and the binder contains a carboxyl group; the hydroxyl group in the porous polyimide and the hydroxyl group in the boride are connected by hydrogen bonds, the carboxyl group in the porous polyimide and the hydroxyl group in the boride are connected by ester groups, the carboxyl group in the porous polyimide and the binder are connected by hydrogen bonds, and the hydroxyl group in the porous polyimide and the binder are connected by ester groups.
2. The composite current collector according to claim 1, characterized in that: The surface of the boride has a hydroxyl group, and the boride includes at least one of MoB, CrB, MnB, FeB, FeB2, V3B4, Nb3B4, and Mo2B.
3. The composite current collector according to claim 1, characterized in that: The thickness ratio of the polymer layer to the metal layer is (1:2) to (1:6); and / or, The thickness of the polymer layer is 3 to 10 μm; and / or, The thickness of the metal layer is 0.5-2.5 μm.
4. The composite current collector according to claim 1, characterized in that: The mass ratio of the boride, the binder and the porous polyimide in the polymer layer is (4:1:50) to (6:1:70).
5. A method for preparing the composite current collector according to any one of claims 1 to 4, characterized in that: include: S1: adding a boron salt into an alkaline solution to perform an etching reaction to obtain a first intermediate; S2: subjecting the supernatant of the first intermediate to ultrasonication, washing, and freeze-drying in sequence to obtain a second intermediate, wherein the second intermediate is a boride with a surface modified with a hydroxyl group; S3: adding the second intermediate and the binder to the amino source, wherein the mass ratio of the second intermediate to the binder is (200-800): (50-150), and mixing them uniformly to obtain a third intermediate; adding a carboxyl source to the third intermediate, mixing them uniformly, dissolving them in a solvent, and performing ultrasonic treatment; adding an acid at a first preset temperature and reacting for a first preset time to obtain a fourth intermediate containing carboxyl groups on the surface; S4: coating the fourth intermediate on a substrate for drying, and then heating under an inert gas atmosphere for imidization to obtain a polymer layer; S5: Plating a metal coating on the surface of the polymer layer to obtain the composite current collector.
6. The method for preparing a composite current collector according to claim 5, characterized in that: The boron salt comprises MoBTx, wherein Tx comprises a hydroxyl group, and the alkali solution comprises a NaOH solution; The amino source includes amine substances containing two or more amino groups; and / or, The carboxyl source includes pyromellitic dianhydride; and / or, The binder includes polyacrylic acid; and / or, The acid includes at least one of acetic acid, sulfuric acid and phosphoric acid; and / or, The first preset temperature is 100-140°C; and / or, The first preset time is 3 to 7 hours.
7. The method for preparing a composite current collector according to claim 5, characterized in that: The fourth intermediate is coated on a substrate for drying, and then heated under an inert gas atmosphere for imidization to obtain a polymer layer, comprising: The fourth intermediate is coated on a glass substrate, dried in a vacuum oven at 30 to 70° C. for 6 to 10 hours, and then heated in an inert gas atmosphere at 280 to 400° C. for 3 to 7 hours for imidization to obtain the polymer layer; and / or, The step of plating a metal coating on the surface of the polymer layer to obtain the composite current collector comprises: The polymer layer is used as a working electrode, a platinum sheet and an Ag / AgCl electrode are used as a counter electrode and a reference electrode respectively, and electroplating is performed for 300 to 900 seconds at a constant potential of -1.4 to -0.8 V in a 0.2 to 0.8 mol / L copper sulfate solution to plate a metal coating on the surface of the polymer layer to obtain the composite current collector.
8. A negative electrode sheet, characterized in that: A composite current collector comprising any one of claims 1 to 4.
9. A battery, characterized in that: The invention comprises a positive electrode sheet, the negative electrode sheet as claimed in claim 8 and an electrolyte.
10. An electrical device, characterized in that: A battery comprising the battery of claim 9.