Microsphere material or nickel electrode and preparation and application thereof
By growing nickel/nickel selenide nanosheets in situ on nickel hydroxide particles to form composite microspheres, the stability and conductivity issues of nickel hydroxide in alkaline zinc-iron-nickel flow batteries are solved, improving battery performance and cycle stability, making it suitable for commercial applications.
Patent Information
- Application Number
- CN202310558954.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-22
AI Technical Summary
In alkaline zinc-iron-nickel flow batteries, nickel hydroxide, as the positive electrode material, suffers from poor stability, low conductivity, and electrode expansion due to the formation of byproducts, which affects battery performance.
In situ growth of metallic nickel/nickel selenide nanosheets on nickel hydroxide particles was achieved using hydrazine hydrate and selenium powder, which improved conductivity and coated nickel hydroxide, forming a metallic nickel/nickel selenide/nickel hydroxide composite microsphere material.
The conductivity and stability of nickel hydroxide are improved, the formation of byproducts is suppressed, the proportion of targeted reactions is increased, the nickel electrode remains stable under high areal capacity, and the coulombic efficiency and energy efficiency are improved, making it suitable for large-scale commercial production.
Smart Images

Figure CN119008983A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a preparation method of a metal nickel / nickel selenide / nickel hydroxide composite microsphere material with catalytic activity and its application, belonging to the technical field of energy storage batteries, and specifically to the field of alkaline zinc-iron-nickel hybrid liquid flow batteries. Background Art
[0002] The proposal of the dual carbon goals marks the transformation of the future energy structure towards clean, low-carbon and sustainable development. Energy storage technology is a key supporting technology in the energy revolution, improving the absorption capacity of clean energy, regulating the frequency of the power grid, and providing users with high-quality electricity.
[0003] Soluble Fe(CN)6 in alkaline zinc-iron flow batteries 4- / Fe(CN)6 3- The positive electrode of the alkaline zinc-nickel flow battery has a soluble Fe(CN)6 4- / Fe(CN)6 3- The electrode pair and the solid-solid phase Ni(OH)2 / NiOOH electrode pair combine the advantages of both to give them high energy density and high rate performance. However, nickel hydroxide as a semiconductor material in alkaline zinc-iron-nickel flow batteries has poor stability at high surface capacity, its conductivity is low, and it is easy to generate byproducts on the surface of the microspheres, causing the microspheres to break, which in turn causes the nickel electrode to expand and the battery internal resistance to increase. Summary of the invention
[0004] In view of the above technical problems, the purpose of this application is to propose a metal nickel / nickel selenide / nickel hydroxide composite microsphere material with catalytic activity, its preparation method and its application in alkaline zinc-iron-nickel flow batteries. This application uses hydrazine hydrate and selenium powder as raw materials to in-situ grow a layer of metal nickel / nickel selenide nanosheets on nickel hydroxide particles. The coated metal nickel can improve the conductivity of the nickel hydroxide particles, and the nickel selenide increases the targeted reaction ratio of the nickel electrode in the alkaline zinc-iron-nickel flow battery, while solving the problem of fragmentation caused by overcharging of nickel hydroxide microspheres. The preparation method of the metal nickel / nickel selenide / nickel hydroxide composite microsphere material with catalytic activity provided in this application is low-cost, simple and convenient, easy to scale up, has excellent battery performance and cycle stability, and is expected to achieve large-scale commercial production.
[0005] In one aspect of the present application, a method for preparing metal nickel / nickel selenide / nickel hydroxide microspheres having catalytic activity is provided, the preparation method comprising:
[0006] The raw materials containing hydrazine hydrate, selenium, nickel hydroxide, sodium hydroxide and water are reacted, filtered, washed and dried I to obtain the metal nickel / nickel selenide / nickel hydroxide composite microsphere material with catalytic activity.
[0007] As a specific implementation, the method for preparing the catalytically active metal nickel / nickel selenide / nickel hydroxide composite microsphere material comprises:
[0008] (1) Dispersing hydrazine hydrate, selenium, nickel hydroxide and sodium hydroxide in 40 mL of water, wherein the molar number of selenium is 0% to 20% of the molar number of nickel hydroxide, the molar number of hydrazine hydrate is 20% to 160% of the molar number of nickel hydroxide, and the sodium hydroxide is 1 to 5 g;
[0009] (2) Pour the above solution into a polytetrafluoroethylene liner, which is screwed into a stainless steel shell, and react at 90°C to 180°C for 2 to 24 hours;
[0010] (3) filtering the solution obtained in step (2) to obtain a filter residue, washing, and drying to obtain a metal nickel / nickel selenide / nickel hydroxide composite microsphere material with catalytic activity.
[0011] Optionally, the washing in step (3) is specifically rinsing with ultrapure water.
[0012] Optionally, the molar number of the hydrazine hydrate is 70% to 90% of the molar number of the nickel hydroxide.
[0013] Optionally, the molar amount of the selenium is 5% to 15% of the molar amount of the nickel hydroxide.
[0014] Optionally, the mass volume ratio of the nickel hydroxide to water is 1-8g:40mL.
[0015] Optionally, the nickel hydroxide has a particle size of 1 to 20 μm.
[0016] The mass volume ratio of the sodium hydroxide to water is 1-5 g:40 mL.
[0017] Optionally, the reaction temperature is 90°C to 180°C.
[0018] Optionally, the reaction temperature is 110-150°C.
[0019] Optionally, the reaction temperature is 120-140°C.
[0020] Optionally, the reaction time is 2 to 24 hours.
[0021] Optionally, the reaction time is 8 to 16 hours.
[0022] Optionally, the reaction time is 10 to 14 hours.
[0023] Optionally, the drying temperature is 40-100°C.
[0024] Optionally, the reaction is carried out in a closed container, and the volume of the reactants accounts for 30%-60% of the polytetrafluoroethylene liner.
[0025] In another aspect of the present application, a method for preparing the above-mentioned nickel electrode is provided, the preparation method comprising:
[0026] (1) dispersing the metal nickel / nickel selenide / nickel hydroxide composite microsphere material into a solution containing a binder to obtain a dispersion;
[0027] (2) Immersing the porous electrode in the dispersion obtained in step (1), soaking it, taking it out and drying it II to obtain the nickel electrode.
[0028] As a specific implementation, the method for preparing the nickel electrode includes:
[0029] (1) dissolving polyvinylidene fluoride (PVDF) in an organic solvent and stirring the mixture to obtain a binder having a polyvinylidene fluoride concentration of 40 to 100 g / L;
[0030] (2) Dispersing the above-mentioned metal nickel / nickel selenide / nickel hydroxide composite microsphere material into the binder prepared in step (1), wherein the mass ratio of nickel hydroxide microspheres to polyvinylidene fluoride is (1:30) to (1:5), to obtain a dispersion containing nickel hydroxide microspheres, completely immersing the porous electrode in the dispersion for more than 1 minute, taking out the electrode, and drying it to obtain a nickel electrode.
[0031] Optionally, the binder is selected from at least one of polyvinylidene fluoride, sulfonated polyetheretherketone, and perfluorosulfonic acid resin;
[0032] In the solution containing the binder, the concentration of the binder is 40-100 g / L.
[0033] Optionally, the solution containing the binder further includes an organic solvent;
[0034] The organic solvent includes N,N-dimethylacetamide and / or N,N-dimethylformamide.
[0035] Optionally, in the dispersion, the mass ratio of the binder to the metal nickel / nickel selenide / nickel hydroxide composite microsphere material is (1:30) to (1:5).
[0036] Optionally, the material of the porous electrode is selected from at least one of graphite felt, carbon felt, carbon cloth and carbon paper.
[0037] Optionally, the porous electrode is completely immersed in the dispersion for more than 1 minute.
[0038] Optionally, the drying temperature II is 40-100°C.
[0039] Another aspect of the present application provides the use of the above-mentioned nickel electrode or the nickel electrode obtained by the above-mentioned preparation method as a positive electrode in an alkaline zinc-iron-nickel liquid flow battery.
[0040] Optionally, the negative electrode electrolyte of the alkaline zinc-iron-nickel liquid flow battery is 0.4 molL -1 ZnO+1.9mol L -1 NaOH + 1.9 mol L -1 KOH solution. The positive electrolyte is 0.4 molL -1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 KOH solution.
[0041] Optionally, the negative electrode of the alkaline zinc-iron-nickel liquid flow battery is a porous carbon felt, and the positive electrode is a nickel electrode.
[0042] The beneficial effects of this application include:
[0043] (1) In addition to the two conventional electrochemical reactions, the positive electrode of the alkaline zinc-iron-nickel flow battery also includes a redox targeted reaction between two electrodes. That is, during charging, the positive electrode Fe(CN)6 4- The ion loses electrons at the electrode to generate Fe(CN)6 3- ions. Subsequently, Fe(CN)6 3- The ions oxidize the Ni(OH)2 on the nickel electrode to NiOOH and are reduced to Fe(CN)6 4- ions. On the electrode, Fe(CN)6 4- The ion loses electrons again and generates Fe(CN)6 3- Ions. The discharge process is the opposite.
[0044] Positive electrode reaction:
[0045] Electrochemical reaction:
[0046] Ni(OH)2-e - +OH - →NiOOH+H2O
[0047] Fe(CN)6 4- -e -→Fe(CN)6 3-
[0048] Redox Targeted Reactions:
[0049] Ni(OH)2+Fe(CN)6 3- +OH - →NiOOH+Fe(CN)6 4- +H2O
[0050] Based on the targeted reaction, nickel hydroxide microspheres can be free from the limitation of conductivity, fully utilize the capacity inside the microspheres and near the current collector, inhibit the generation of by-products, and improve the stability of nickel electrode materials. However, the reaction rate of the targeted reaction is slow, and the utilization rate of nickel electrodes at high current density is low.
[0051] (2) Metallic nickel / nickel selenide promotes Fe(CN)6 4- / Fe(CN)6 3- The redox targeted reaction between the electrode pair and the Ni(OH)2 / NiOOH electrode pair increases the proportion of the targeted reaction in the nickel electrode. -2 The microspheres remained stable under high surface capacity test conditions and no breakage occurred. -2 At a current density of , the alkaline zinc-iron-nickel flow battery assembled with nickel selenide / metallic nickel hydroxide electrodes achieved a coulombic efficiency of 99.02%, an energy efficiency of 80.61%, and stable cycling for more than 60 cycles.
[0052] At 40mA cm -2 The current density is 160 mAh cm -2 At a high charge surface capacity, the SEM results show that the morphology of the metal nickel / nickel selenide / nickel hydroxide composite microspheres is intact and there is no fragmentation. This indicates that the catalytic activity of metal nickel / nickel selenide increases the proportion of targeted reactions and further improves the stability of the nickel electrode.
[0053] At 80 mA cm -2 At a current density of , the voltage efficiency of the alkaline zinc-iron-nickel flow battery assembled with metal nickel / nickel selenide / nickel hydroxide composite microspheres exceeds 80%;
[0054] (3) The preparation method of nickel hydroxide microspheres of the present application is low-cost, simple and convenient, easy to scale up, and is expected to achieve large-scale commercial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 XRD spectrum of nickel selenide / metallic nickel / nickel hydroxide microspheres;
[0056] Figure 2Middle, SEM images of a, b unmodified nickel hydroxide microspheres and c, d nickel selenide / metallic nickel / nickel hydroxide microspheres;
[0057] Figure 3 Schematic diagram of the device for quantifying the contribution of redox-targeted reactions to the capacity of Zn-Fe-Ni hybrid batteries.
[0058] Figure 4 This is a schematic diagram of an alkaline zinc-iron-nickel flow battery test device;
[0059] Figure 5 (ab) is at 40 mA cm -2 The current density and 160 mAh cm -2 SEM image of unmodified nickel hydroxide positive electrode under high surface capacity conditions;
[0060] Figure 6 (ab) is at 40 mA cm -2 The current density and 160 mAh cm -2 SEM image of nickel selenide / metallic nickel / nickel hydroxide positive electrode under high surface capacity conditions;
[0061] Figure 7 At 80 mA cm -2 (a) Long cycle performance diagram of alkaline zinc-iron-nickel liquid flow battery assembled with nickel selenide / metallic nickel / nickel hydroxide positive electrode and (b) charge and discharge surface capacity diagram under current density. DETAILED DESCRIPTION
[0062] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0063] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0064] The single cell in the embodiment is assembled in the following order: positive terminal plate, graphite current collector, positive electrode 3×3 cm 2 Nickel felt, PBI membrane, negative electrode 3×3cm 2 Carbon felt, graphite current collector, negative terminal plate.
[0065] Battery performance test: The flow rate of electrolyte in the battery is 60 mL min -1 , using the capacity cutoff method, the current density is 40 / 80mA cm -2 , discharge cut-off voltage is 0.8V, PBI film.
[0066] Example 1
[0067] 1) Add 0.05 mol nickel hydroxide (particle size 1-20 μm, i.e., unmodified nickel hydroxide microspheres), 0.005 mol (accounting for 10% of the molar amount of nickel hydroxide) selenium powder, 0.04 mol (accounting for 80% of the molar amount of nickel hydroxide) hydrazine hydrate, 2 g sodium hydroxide, and 40 mL ultrapure water to the polytetrafluoroethylene liner of a stainless steel reactor. Put the polytetrafluoroethylene liner into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 130° C. for reaction for 12 hours.
[0068] 2) The nickel hydroxide microsphere dispersion prepared in step 1) is filtered with filter paper, the solid is washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain nickel selenide / metal nickel / nickel hydroxide microspheres.
[0069] 3) XRD and SEM tests were performed on the above samples and unmodified nickel hydroxide.
[0070] from Figure 1 It can be seen from a that the nickel hydroxide powder after hydrothermal synthesis still has the β-Ni(OH)2 crystal form, and the diffraction peaks at 44.5°, 51.8° and 76.4° are respectively attributed to the characteristic peaks of metallic nickel (111), (200) and (220), which indicates that the reducibility of hydrazine hydrate can partially convert the semiconductor nickel hydroxide into highly conductive metallic nickel, thereby improving the electronic transport performance of the nickel hydroxide electrode. In addition, the diffraction characteristic peaks of Ni3Se2 appeared at 20.9°, 29.7°, 42.6° and 47.8°, indicating that nickel selenide was successfully loaded on the nickel hydroxide.
[0071] Figure 2 a and b show that the unmodified nickel hydroxide microspheres (raw materials with a particle size of 1-20 μm) are composed of nanoscale spindle-shaped particles with a length of about 200 nm and a width of about 40 nm. Compared with the unmodified nickel hydroxide microspheres, the surface of the nickel selenide / metal nickel / nickel hydroxide microspheres is rougher ( Figure 2 c) From Figure 2 The dSEM magnified image shows that the surface of the nickel hydroxide microspheres is coated with nano-scale nickel selenide / metallic nickel (the coating is sponge-like). This is because hydrazine hydrate and selenium powder react to generate H2Se, and the hydroxyl ions in Ni(OH)2 react with Se 2- The exchange generates a thin layer of Ni3Se2 on the surface of nickel hydroxide. Due to the lattice mismatch between nickel hydroxide and Ni3Se2, Ni3Se2 nanosheets are formed after high pressure hydrothermal treatment. The length and width of the nanosheet are about 70-100nm, and the thickness is about 5-10nm. The Ni3Se2 nanosheets doped with metallic nickel are deposited on the surface of nickel hydroxide.
[0072] Example 2
[0073] 1) Add 0.05 mol nickel hydroxide (particle size 1-20 μm, i.e., unmodified nickel hydroxide microspheres), 0.01 mol (accounting for 20% of the molar amount of nickel hydroxide) selenium powder, 0.08 mol (accounting for 160% of the molar amount of nickel hydroxide) hydrazine hydrate, 2 g sodium hydroxide, and 40 mL ultrapure water (the total volume of all the aforementioned reaction materials accounts for about 40% of the volume of the polytetrafluoroethylene liner) into the polytetrafluoroethylene liner of a stainless steel reactor, put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 130° C. for reaction for 12 hours.
[0074] 2) The nickel hydroxide microsphere dispersion prepared in step 1) is filtered with filter paper, the solid is washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain nickel selenide / metal nickel / nickel hydroxide microspheres.
[0075] 3) Perform XRD test on the above samples and unmodified nickel hydroxide.
[0076] from Figure 1 As can be seen in b, the excessive amount of hydrazine hydrate and selenium powder weakens the diffraction peak signal of nickel hydroxide, while the signal peaks of metallic nickel and nickel selenide are enhanced accordingly.
[0077] Example 3
[0078] Sample No. 1 is unmodified nickel hydroxide (particle size 1-20 μm) purchased from Aladdin.
[0079] Preparation of nickel / nickel hydroxide microsphere samples (N2H4)
[0080] 1) Add 0.05 mol nickel hydroxide (particle size 1-20 μm, i.e., unmodified nickel hydroxide microspheres), 0.02 mol (accounting for 40% of the molar amount of nickel hydroxide) hydrazine hydrate, 2 g sodium hydroxide, and 40 mL ultrapure water (the total volume of all the aforementioned reaction materials accounts for about 40% of the volume of the polytetrafluoroethylene liner) into the polytetrafluoroethylene liner of a stainless steel reactor, put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 130° C. for reaction for 12 hours.
[0081] 2) The nickel hydroxide microsphere dispersion prepared in step 1) was filtered with filter paper, washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain metal nickel / nickel hydroxide microspheres (sample No. 2 in Table 1).
[0082] Preparation of nickel selenide / metal nickel / nickel hydroxide microsphere samples (N2H4+Se)
[0083] 1) Add 0.05 mol of nickel hydroxide (particle size 1-20 μm, i.e., unmodified nickel hydroxide microspheres) to the polytetrafluoroethylene liner of a stainless steel reactor, selenium powder accounting for 5, 10, and 15% of the molar amount of nickel hydroxide, respectively (see Table 1 for details), hydrazine hydrate accounting for 40, 80, 120, and 160% of the molar amount of nickel hydroxide, respectively (see Table 1 for details), 2 g of sodium hydroxide, and 40 mL of ultrapure water (the total volume of all the aforementioned reaction raw materials accounts for about 40% of the volume of the polytetrafluoroethylene liner), put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 100, 130, and 160° C. (see Table 1 for details), and react for 6, 12, and 18 hours, respectively (see Table 1 for details).
[0084] 2) The nickel hydroxide microsphere dispersion prepared in step 1) was filtered with filter paper, and the solids were washed with 1L ultrapure water, and then dried in an oven at 80°C to obtain nickel selenide / metallic nickel / nickel hydroxide microspheres (samples No. 3-12 in Table 1, where sample No. 6 had the same reaction conditions as the sample in Example 1).
[0085] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0086] First, 72 g of polyvinylidene fluoride (PVDF) was dissolved in 1 L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder solution (PVDF solution); 3 g of the samples prepared in Example 3 (respectively, the samples with sample numbers 1-12 in Table 1) were dispersed in 4.5 g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30 * 30 * 4.2 mm 3 ) was completely immersed in the above dispersion for 1 minute, the porous carbon felt was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0087] The electrolyte was prepared as follows:
[0088] The negative electrolyte of the alkaline zinc-iron-nickel flow battery is 0.4 mol L -1 ZnO+1.9mol L -1 NaOH + 1.9 mol L -1 KOH aqueous solution. The positive electrode electrolyte is 0.4 mol L - 1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 Aqueous KOH solution.
[0089] Alkaline zinc-iron-nickel flow battery test conditions: The negative electrode is porous carbon felt (length * width * thickness = 30 * 30 * 4.2mm 3 ), the positive electrode is the nickel electrode prepared as above, the negative electrode electrolyte is 100 mL, the positive electrode electrolyte is 50 mL, the diaphragm is an ion exchange membrane prepared from an aromatic polymer containing a nitrogen heterocycle (polybenzimidazole is dissolved in N, N-dimethylacetamide, and a polybenzimidazole ion exchange membrane is obtained after scraping and drying), the battery charge cut-off voltage is 2 V, the discharge cut-off voltage is 0.8 V, and the charge and discharge current density is 40 mA cm -2 .
[0090] use Figure 3 A battery device was developed to explore the proportion of redox targeted reactions in different nickel hydroxide electrodes. Figure 3 1 is an ion exchange membrane, 2 is a porous carbon felt electrode, 3 is a tank filled with negative electrode electrolyte, 4 is a tank filled with positive electrode electrolyte, 5 is a sealed container with a nickel positive electrode inside (with an electrolyte inlet and outlet), and 6 is a current collector; two sheet-like porous carbon felt electrodes 2 and an ion exchange membrane 1 placed between the two porous carbon felt electrodes 2 are stacked between the two flat current collectors 6, the negative electrode electrolyte in the tank 3 filled with negative electrode electrolyte circulates between the tank 3 of the negative electrode electrolyte and a porous carbon felt electrode between a flat current collector and the ion exchange membrane through a liquid pump, and the positive electrode electrolyte in the tank 4 filled with positive electrode electrolyte circulates between the tank 4 of the positive electrode electrolyte, the sealed container with a nickel positive electrode inside, and another porous carbon felt electrode between another flat current collector and the ion exchange membrane through a liquid pump. The device places the nickel hydroxide electrode in an external sealed container (not connected to the current collector). Therefore, the cell only produces Fe(CN)6 4- / Fe(CN)6 3- The electrochemical reaction of the electrode pair and the redox targeted reaction between the two electrode pairs do not cause the electrochemical reaction of nickel hydroxide. The ferrocyanide ion concentration of the positive electrode electrolyte is 0.8 mol L -1 , the volume is 50mL, the molar number of ferrocyanide ion is 0.04mol, and the capacity per mole of active substance is 26.8AhL -1 Therefore, Fe(CN)6 4- / Fe(CN)6 3- The theoretical capacity of the battery is 1.072Ah.
[0091] Thanks to Fe(CN)6 4- / Fe(CN)6 3- The couple has excellent reversibility, with a charge cutoff voltage of 2 V and a charge current of 40 mA cm -2 At a current density of 2.5 Å, the positive electrode Fe(CN)6 4- / Fe(CN)6 3-The charge and discharge capacity of the pair is 1.072Ah. Therefore, the total charge capacity is subtracted from the Fe(CN)6 4- / Fe(CN)6 3- The volume capacity of the electrode pair (1.072Ah) can be used to obtain the capacity provided by the redox targeted reaction (redox targeted reaction capacity). The ratio of the redox targeted reaction capacity to the theoretical capacity of the nickel electrode is the proportion of the redox targeted reaction in the nickel electrode.
[0092] Table 1 The proportion of targeted reactions in different nickel hydroxide electrodes.
[0093]
[0094] Discussion of the results in the above table
[0095] From the results of sample 1, it can be seen that the targeted reaction accounts for only 2% in the unmodified nickel hydroxide electrode. After adding 40% hydrazine hydrate, the targeted reaction ratio did not change, indicating that the generated metal nickel can only improve its conductivity and has no catalytic effect on the targeted reaction.
[0096] It can be seen from samples 3-5 that after adding 5% and 10% selenium powder, the proportion of targeted reactions of nickel electrodes increased to 4% and 10%, respectively. When 15% selenium powder was added, the nickel hydroxide active substance performed well, and the proportion of targeted reactions was still 8%. Therefore, the proportion of 10% selenium powder is the optimal condition. As can be seen from sample 6, by increasing the content of hydrazine hydrate to 80%, the selenium powder is fully utilized, and the proportion of targeted reactions is as high as 30%. Further increasing the content of hydrazine hydrate to 120% and 160%, the nickel hydroxide active substance performed well, and the proportion of targeted reactions was 25% and 20%, respectively. At this ratio, the XRD results show that the microsphere material is still a mixture of nickel hydroxide / metal nickel / nickel selenide.
[0097] From sample 9, it can be seen that at too low a reaction temperature (100°C), the selenium powder does not react fully, but the generated nickel selenide can still effectively catalyze the targeted reaction, and the proportion of the targeted reaction is still 20%. From sample 10, it can be seen that at too high a reaction temperature (160°C), the nickel hydroxide active substance performs well, and the proportion of the targeted reaction can still be maintained at 25%.
[0098] From sample 11, it can be seen that under a shorter reaction time (6h), the selenium powder does not react fully, but the generated nickel selenide can still effectively catalyze the targeted reaction, which still accounts for 20%. From sample 12, it can be seen that under a longer reaction time (18h), the nickel hydroxide active substance performs well, and the targeted reaction accounts for 25%. Finally, the molar number of hydrazine hydrate is 80% of the molar number of nickel hydroxide, the molar number of selenium powder is 10% of the molar number of nickel hydroxide, the hydrothermal reaction temperature is 130°C, and the reaction time is 12h.
[0099] Comparative Example 1
[0100] The sample is consistent with sample No. 1 in Table 1 of Example 3.
[0101] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0102] First, 72g of polyvinylidene fluoride (PVDF) was dissolved in 1L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder; unmodified nickel hydroxide (particle size 1-20 μm) was dispersed in 4.5g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30*30*4.2mm 3 ) was completely immersed in the above dispersion for 2 minutes, the electrode was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0103] The electrolyte was prepared as follows:
[0104] The negative electrolyte of the alkaline zinc-iron-nickel flow battery is 0.4 mol L -1 ZnO+1.9mol L -1 NaOH + 1.9 mol L -1 KOH aqueous solution. The positive electrode electrolyte is 0.4 mol L - 1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 Aqueous KOH solution.
[0105] use Figure 4 A battery device was used to explore the battery performance of nickel hydroxide electrodes. Figure 41 is an ion exchange membrane (polybenzimidazole is dissolved in N, N-dimethylacetamide, and the polybenzimidazole ion exchange membrane is obtained after scraping and drying), 2 is a porous carbon felt electrode, 3 is a storage tank filled with negative electrode electrolyte, 4 is a storage tank filled with positive electrode electrolyte, 5 is a nickel hydroxide electrode, and 6 is a current collector; a sheet-like porous carbon felt electrode 2 and a nickel hydroxide electrode 5 and an ion exchange membrane 1 placed therebetween are stacked between two flat current collectors 6, the negative electrode electrolyte in the storage tank 3 filled with negative electrode electrolyte circulates between the storage tank 3 of the negative electrode electrolyte and a porous carbon felt electrode between a flat current collector and the ion exchange membrane through a liquid pump, and the positive electrode electrolyte in the storage tank 4 filled with positive electrode electrolyte circulates between the storage tank 4 of the positive electrode electrolyte and a nickel hydroxide electrode between a flat current collector and the ion exchange membrane through a liquid pump. The device connects the nickel hydroxide electrode to the current collector. Therefore, the battery undergoes electrochemical reactions of two electrode pairs and a redox targeted reaction between the two electrode pairs.
[0106] At a current density of 40 mA / cm 2 , surface capacity is 160mAh / cm 2 The test conditions were as follows: the discharge cut-off voltage was 0.8 V. At the end of the charge, the nickel felt was taken out, rinsed, freeze-dried, and then SEM tested.
[0107] Figure 5 (ab) is at 40 mA cm -2 The current density and 160 mAh cm -2 SEM image of the unmodified nickel hydroxide positive electrode under high surface capacity conditions. -2 The current density and 160 mAh cm -2 Under high surface capacity conditions, the morphology of the unmodified nickel hydroxide electrode microspheres shows that some nickel hydroxide microspheres have cracks or even completely broken. Although the targeted reaction can carry out redox reactions on nickel hydroxide without being restricted by conductivity, when the targeted reaction is too low, the nickel hydroxide microspheres are prone to side reactions at high surface capacity, resulting in microsphere breakage.
[0108] Example 4
[0109] The sample is consistent with sample No. 6 in Table 1 of Example 3. (80% N2H4+10% Se)
[0110] 1) Add 0.05 mol of nickel hydroxide (particle size 1-20 μm), 0.005 mol (accounting for 10% of the molar amount of nickel hydroxide) of selenium powder, 0.04 mol (accounting for 80% of the molar amount of nickel hydroxide) of hydrazine hydrate, 2 g of sodium hydroxide, and 40 mL of ultrapure water (the total volume of all the aforementioned reaction materials accounts for about 40% of the volume of the polytetrafluoroethylene liner) into the polytetrafluoroethylene liner of a stainless steel reactor, put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 130° C. for reaction for 12 hours.
[0111] 2) The nickel hydroxide microsphere dispersion prepared in step 1) is filtered with filter paper, the solid is washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain nickel selenide / metal nickel / nickel hydroxide microspheres.
[0112] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0113] First, 72g of polyvinylidene fluoride (PVDF) was dissolved in 1L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder; 3g of the sample prepared above was dispersed in 4.5g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30*30*4.2mm 3 ) was completely immersed in the above dispersion for 3 minutes, the electrode was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0114] The electrolyte was prepared as follows:
[0115] The negative electrolyte of the alkaline zinc-iron-nickel flow battery is 0.4 mol L -1 ZnO+1.9mol L -1 NaOH + 1.9 mol L -1 KOH aqueous solution. The positive electrode electrolyte is 0.4 mol L - 1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 Aqueous KOH solution.
[0116] use Figure 4 The battery device was tested at a current density of 40 mA / cm 2 , surface capacity is 160mAh / cm 2 , the test was conducted under the test condition of discharge cut-off voltage of 0.8 V. At the end of charging, the nickel felt was taken out, rinsed, freeze-dried, and then SEM test was conducted.
[0117] Compared with the alkaline zinc-iron-nickel hybrid flow battery based on nickel selenide / metal nickel / nickel hydroxide electrode test under the same test conditions, even at 160mAh / cm 2 Under the ultra-high surface capacity, the morphology of nickel hydroxide microspheres remains intact without any fragmentation ( Figure 6 ). This is because the targeted reaction can carry out redox reaction on nickel hydroxide without being restricted by conductivity, so the nickel hydroxide material with a high targeted reaction ratio remains stable at high surface capacity.
[0118] Example 5
[0119] The sample is consistent with sample No. 6 in Table 1 of Example 3. (80% N2H4+10% Se)
[0120] 1) Add 0.05 mol of nickel hydroxide (particle size 1-20 μm), 0.005 mol (accounting for 10% of the molar amount of nickel hydroxide) of selenium powder, 0.04 mol (accounting for 80% of the molar amount of nickel hydroxide) of hydrazine hydrate, 2 g of sodium hydroxide, and 40 mL of ultrapure water (the total volume of all the aforementioned reaction materials accounts for about 40% of the volume of the polytetrafluoroethylene liner) into the polytetrafluoroethylene liner of a stainless steel reactor, put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 130° C. for reaction for 12 hours.
[0121] 2) The nickel hydroxide microsphere dispersion prepared in step 1) is filtered with filter paper, washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain nickel selenide / metal nickel / nickel hydroxide microspheres.
[0122] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0123] First, 72 g of polyvinylidene fluoride (PVDF) was dissolved in 1 L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder; 3 g of the sample prepared in Example 5 was dispersed in 4.5 g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30 * 30 * 4.2 mm 3 ) was completely immersed in the above dispersion for 3 minutes, the electrode was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0124] The electrolyte was prepared as follows:
[0125] The negative electrolyte of the alkaline zinc-iron-nickel flow battery will be 0.4 mol L -1 ZnO+1.9mol L -1 NaOH+1.9molL -1The KOH aqueous solution was obtained after being fully stirred. The positive electrode electrolyte was 0.4 mol L -1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 The KOH aqueous solution is obtained after being fully stirred.
[0126] use Figure 4 The battery device was tested by first conducting a test at 40 mA cm -2 Current density, 120 mAh cm -2 The alkaline zinc-iron-nickel flow battery was activated for 6 cycles at a discharge cut-off voltage of 0.8 V, and then at 80 mA cm -2 The current density and 120 mAh cm -2 The battery was tested for long cycle performance under the charged surface capacity. The alkaline zinc-iron-nickel flow battery assembled based on nickel selenide / metal nickel / nickel hydroxide electrodes has a coulombic efficiency of 99.02% and an energy efficiency of 80.61%. It can run stably for more than 60 cycles, and the surface capacity does not decrease significantly ( Figure 7 ), the performance remains stable.
[0127] Comparative Example 2
[0128] 1) Add 0.05 mol of nickel hydroxide (particle size 1-20 μm), 0.0125 mol (accounting for 25% of the molar amount of nickel hydroxide) of selenium powder, 0.1 mol (accounting for 200% of the molar amount of nickel hydroxide) of hydrazine hydrate, 2 g of sodium hydroxide, and 40 mL of ultrapure water (the total volume of all the aforementioned reaction materials accounts for about 40% of the volume of the polytetrafluoroethylene liner) into the polytetrafluoroethylene liner of a stainless steel reactor, put it into the outer shell of the stainless steel reactor, tighten the sealing cover of the reactor to seal the reactor, and then put it into an oven and heat it to 200° C. for reaction for 30 hours.
[0129] 2) The nickel hydroxide microsphere dispersion prepared in step 1) is filtered with filter paper, washed with 1 L of ultrapure water, and then dried in an oven at 80° C. to obtain nickel selenide / metal nickel / nickel hydroxide microspheres.
[0130] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0131] First, 72g of polyvinylidene fluoride (PVDF) was dissolved in 1L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder; 3g of the sample prepared in Comparative Example 2 was dispersed in 4.5g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30*30*4.2mm 3) was completely immersed in the above dispersion for 2 minutes, the electrode was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0132] The electrolyte was prepared as follows:
[0133] The negative electrolyte of the alkaline zinc-iron-nickel flow battery will be 0.4 mol L -1 ZnO+1.9mol L -1 NaOH+1.9molL -1 The KOH aqueous solution was obtained after being fully stirred. The positive electrode electrolyte was 0.4 mol L -1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 The KOH aqueous solution is obtained after being fully stirred.
[0134] use Figure 4 The battery device was tested at 40 mA cm -2 Current density, 120 mAh cm -2 The charge surface capacity, under the condition of discharge cut-off voltage of 0.8V, the battery capacity is only Fe(CN)6 4- / Fe(CN)6 3- The electrode pair has a capacity of 1.072 Ah, indicating that the excess amount of hydrazine hydrate and selenium powder completely converts the active substance nickel hydroxide into metallic nickel / nickel selenide material.
[0135] Comparative Example 3
[0136] A nickel hydroxide electrode is prepared by using porous carbon felt as a substrate for a nickel electrode, which is prepared by the following steps:
[0137] First, 72g of polyvinylidene fluoride (PVDF) was dissolved in 1L of N, N-dimethylacetamide (DMAc) solvent and stirred thoroughly to obtain a binder; 3g of commercial nickel hydroxide was dispersed in 4.5g of the above PVDF solution, and a porous carbon felt (length * width * thickness = 30*30*4.2mm 3 ) was completely immersed in the above dispersion for 2 minutes, the electrode was taken out, and placed in an oven at 80°C for complete drying to obtain a nickel electrode.
[0138] The electrolyte was prepared as follows:
[0139] The negative electrolyte of the alkaline zinc-iron-nickel flow battery will be 0.4 mol L -1 ZnO+1.9mol L -1 NaOH+1.9molL -1The KOH aqueous solution was obtained after being fully stirred. The positive electrode electrolyte was 0.4 mol L -1 Na4Fe(CN)6+0.4mol L -1 K3Fe(CN)6+0.4mol L -1 NaOH + 0.4 mol L -1 The KOH aqueous solution is obtained after being fully stirred.
[0140] use Figure 3 The device tests the proportion of targeted reactions. Battery test conditions: The negative electrode is porous carbon felt (length * width * thickness = 30 * 30 * 4.2 mm 3 ), the positive electrode is the nickel electrode prepared as above, the negative electrode electrolyte is 100 mL, the positive electrode electrolyte is 50 mL, the diaphragm is an ion exchange membrane prepared from an aromatic polymer containing a nitrogen heterocycle (polybenzimidazole is dissolved in N, N-dimethylacetamide, and a polybenzimidazole ion exchange membrane is obtained after scraping and drying), the battery charge cut-off voltage is 2 V, the discharge cut-off voltage is 0.8 V, and the charge and discharge current density is 40 mA cm -2 .
[0141] The method of cobalt coating in commercial nickel hydroxide can effectively improve the conductivity of nickel hydroxide, but cobalt has no catalytic effect on the targeted reaction. The commercial cobalt-containing nickel hydroxide electrode assembly Figure 3 In alkaline zinc-iron-nickel flow batteries, the targeted reaction accounts for only 10%.
[0142] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a microsphere material, characterized in that: include: The raw materials containing hydrazine hydrate, selenium, nickel hydroxide, sodium hydroxide and water are reacted in a closed reactor, and the solid product is collected by filtration, washed and dried to obtain a microsphere material.
2. The preparation method according to claim 1, characterized in that: The molar number of the hydrazine hydrate is 20% to 160% of the molar number of the nickel hydroxide; preferably, the molar number of the hydrazine hydrate is 40% to 130% of the molar number of the nickel hydroxide; more preferably, the molar number of the hydrazine hydrate is 70% to 90% of the molar number of the nickel hydroxide; The molar number of selenium is 1% to 20% of the molar number of nickel hydroxide; preferably, the molar number of selenium is 5% to 15% of the molar number of nickel hydroxide; more preferably, the molar number of selenium is 7% to 13% of the molar number of nickel hydroxide; The mass volume ratio of the nickel hydroxide to water is 1-8 g:40 mL; preferably, the mass volume ratio of the nickel hydroxide to water is 3-6 g:40 mL; The particle size of the nickel hydroxide is 1 to 20 μm; preferably, the particle size of the nickel hydroxide is 5 to 15 μm.
3. The preparation method according to claim 1 or 2, characterized in that: The mass volume ratio of the sodium hydroxide to water is 1-5 g:40 mL; Preferably, the mass volume ratio of the sodium hydroxide to water is 2-4 g:40 mL; More preferably, the mass volume ratio of the sodium hydroxide to water is 2-3 g:40 mL; The reaction temperature is 90°C to 180°C, preferably 110°C to 150°C, more preferably 120°C to 140°C; The reaction time is 2 to 24 hours, preferably 8 to 16 hours, and more preferably 10 to 14 hours.
4. The preparation method according to claim 1, characterized in that: The reaction is carried out in a closed reactor, and the total volume of the reaction raw materials (the reaction raw materials include hydrazine hydrate, selenium, nickel hydroxide, sodium hydroxide and water) accounts for 30%-60% of the volume of the reactor; The microsphere material is a composite microsphere material containing metallic nickel, nickel selenide and nickel hydroxide.
5. A microsphere material obtained by the preparation method according to any one of claims 1 to 4.
6. Use of the microsphere material according to claim 5 as a positive electrode active material in an alkaline zinc-iron-nickel liquid flow battery.
7. A nickel electrode, characterized in that The nickel electrode comprises the microsphere material of claim 5.
8. The method for preparing the nickel electrode according to claim 7, characterized in that: The preparation method comprises: (1) dispersing the microsphere material into a solution containing a binder to obtain a dispersion; (2) Immersing the porous electrode in the dispersion obtained in step (1) to wet it, taking out the wetted porous electrode and drying it to obtain the nickel electrode.
9. The preparation method according to claim 8, characterized in that: The binder is selected from at least one or more of polyvinylidene fluoride, sulfonated polyetheretherketone, and perfluorosulfonic acid resin; The solution containing the binder is an organic solution of the binder, wherein the concentration of the binder is 40 to 100 g / L; The organic solvent used in the solution includes N, N-dimethylacetamide and / or N, N-dimethylformamide; Preferably, in the dispersion, the mass ratio of the binder to the microsphere material is (1:30) to (1:5); Preferably, the material of the porous electrode is selected from at least one or more of graphite felt, carbon felt, carbon cloth and carbon paper; Preferably, the impregnation time is 1 min to 5 min; the impregnation process is an impregnation process of equal volume or excess solution impregnation method; Preferably, the drying temperature is 40-100°C.
10. Use of the nickel electrode according to claim 7 or the nickel electrode obtained by the preparation method according to any one of claims 8 to 9 as a positive electrode in an alkaline zinc-iron-nickel liquid flow battery.
Citation Information
Patent Citations
Method of nickel hydroxide surface metallization
CN101000959A
Water-based zinc-nickel battery nickel composite positive electrode material and preparation method thereof
CN112614992A
Alkaline zinc-iron-nickel mixed flow battery
CN112652798A
Iron-doped nickel hydroxide composite nickel selenide material as well as preparation method and application thereof
CN115928135A
SURFACE MODIFIED CATHOD MATERIAL, AND CATHODE MATERIAL, CATHODE AND Zn-Ni FLOW SECONDARY BATTERY COMPRISING THE SURFACE MODIFIED CATHOD MATERIAL
KR1020180072448A