MOF-derived two-dimensional cobalt-nitrogen-doped carbon material as well as preparation method and application thereof
The MOF-derived two-dimensional cobalt nitrogen-doped carbon material solves the problems of high cost and poor durability of precious metal catalysts, and achieves high-efficiency oxygen reduction electrocatalytics and excellent performance of zinc-air batteries.
Patent Information
- Application Number
- CN202411100923.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The precious metal catalysts used in existing zinc-air batteries have high cost and poor durability, and the traditional two-dimensional carbon-based electrocatalyst preparation methods have problems such as sample contamination and impurity introduction, resulting in a reduction in catalytic activity.
By using two-dimensional metal organic frame materials (MOFs) as templates, MOF derived two-dimensional cobalt nitrogen doped carbon materials are prepared, and uniform dispersion of metal active centers and high-efficiency oxygen are achieved by using graphite carbon structure and strong coordination bonds during the calcination process. Reduction electrocatalysis.
A low-cost and high-stability oxygen reduction electrocatalyst is achieved, with a half-wave potential better than commercial Pt/C, and the assembled zinc-air battery has better discharge performance and flexible foldability.
Smart Images

Figure CN119008986A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of electrochemical catalyst technology, and in particular to a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material and a preparation method and application thereof. Background Art
[0002] Zinc-air batteries (ZABs), as a new generation of energy storage and conversion technology, have the advantages of high energy density, low cost, and environmental friendliness, and are considered to be an ideal solution to alleviate the energy crisis. Although platinum group noble metal catalysts show good oxygen reduction reaction (ORR) performance, their high cost and poor durability hinder their widespread application. Therefore, the development of non-noble metal catalysts with excellent catalytic performance and stability is crucial to achieve sustainable energy conversion. In recent years, single-atom catalysts have attracted widespread attention due to their unique electronic structure and high atom utilization. In particular, transition metal single-atom carbon-based catalysts have become a research hotspot due to their excellent ORR activity and stability. However, due to the high surface energy of isolated metal single atoms, they are easy to aggregate after synthesis or catalysis, resulting in reduced catalytic activity. Therefore, achieving single-atom dispersion while maintaining high catalytic activity remains a major challenge.
[0003] Two-dimensional (2D) carbon-based materials are ideal supports for single-atom catalysts due to their unique physicochemical properties and high specific surface area. Compared with traditional three-dimensional materials, they not only have a high degree of structural order and electronic properties, but also provide a large number of active sites for catalytic reactions; their ultrathin structure can greatly increase the contact area between the catalyst and the reactant, thereby improving the catalytic efficiency; in addition, they usually have excellent conductivity, which is conducive to the rapid transfer of charge carriers, thereby accelerating the electrocatalytic process. At present, the common methods for preparing two-dimensional carbon-based electrocatalysts are mainly vapor deposition and mechanically assisted exfoliation. For vapor deposition, the product is inevitably transferred from the growth substrate to the target substrate, which often leads to sample contamination and breakage. Mechanically assisted exfoliation methods such as ball milling, although simple to operate, may introduce impurities and destroy the crystal structure of the material during long processing, which has an adverse effect on the performance of the final product. Therefore, it is crucial to explore alternative strategies for preparing two-dimensional carbon-based catalysts.
[0004] The researchers found that preparing two-dimensional carbon-based electrocatalysts by direct pyrolysis of two-dimensional metal-organic framework materials (MOFs) is a simple and effective method, because the morphology of the precursor has a great influence on the morphology and performance of two-dimensional carbon-based materials. The two-dimensional electrocatalysts derived from two-dimensional MOFs retain their ultra-high specific surface area and porosity well, which is conducive to exposing active sites in catalytic reactions. The graphitic carbon structure produced during the calcination process is crucial to improving the conductivity of the material. In addition, the heteroatoms in the organic ligands can form strong coordination bonds with metal atoms to achieve uniform dispersion of metal active centers. By selecting different metal nodes and organic ligands, the type and configuration of active centers can be regulated at the molecular level, thereby optimizing the electrocatalytic performance. Therefore, the strategy of preparing two-dimensional carbon-based electrocatalysts using two-dimensional MOFs as templates has broad prospects in the field of electrocatalysis. Summary of the invention
[0005] In view of this, the embodiments of the present application provide a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material and a preparation method and application thereof. The MOF-derived two-dimensional cobalt-nitrogen-doped carbon material provides a new idea for the development of efficient oxygen reduction electrocatalysts, and can effectively solve the problem of expensive and poor durability of precious metal catalysts in the prior art.
[0006] The first aspect of the embodiment of the present application provides a method for preparing a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material, comprising the following steps:
[0007] (1) Dissolving a surfactant in a mixed organic solvent to obtain a solution A; dissolving a metal salt and 1-carboxymethylpyrazole-4-carboxylic acid in water to obtain a solution B and a solution C respectively; dropping the solution B and the solution C into the solution A successively, stirring at room temperature for reaction, and after the reaction is completed, centrifuging, washing and drying to obtain a precursor Co x Zn 1-x -MOF;
[0008] (2) The precursor Co x Zn 1-x -MOF is calcined under an inert gas atmosphere to obtain MOF-derived two-dimensional cobalt-nitrogen-doped carbon material.
[0009] In some embodiments that may include the above embodiments, in step (2), the calcination temperature is 800-1000° C., the calcination time is 2-4 h, the heating rate is 4-6° C. / min, and the inert atmosphere is nitrogen.
[0010] In some embodiments that may include the above embodiments, in step (1), the stirring reaction time is 2 to 4 hours.
[0011] In some embodiments that may include the above embodiments, in step (1), the molar ratio of 1-carboxymethylpyrazole-4-carboxylic acid, metal salt, and surfactant is 1: [1-2]: [1-3].
[0012] In some embodiments that may include the above embodiments, in step (1), the metal salt includes Zn salt and Co salt; wherein, the Zn salt is zinc acetate dihydrate, the Co salt is cobalt acetate tetrahydrate, and the molar ratio of Co ions to total metal ions is (0-0.1]:1.
[0013] In some embodiments that may include the above embodiments, in step (1), the surfactant is at least one of cetyltrimethylammonium bromide, sodium dodecyl sulfate, and sodium cetyl sulfate.
[0014] In some embodiments that may include the above embodiments, in step (1), the mixed organic solvent includes a hydrophilic solvent and an oil-phase solvent; wherein, the hydrophilic solvent is n-propanol and / or n-butanol, the oil-phase solvent is n-heptane and / or cyclohexane; the volume ratio of water, hydrophilic solvent, and oil-phase solvent is 1:1: [4-6].
[0015] Preferably, when the surfactant is cetyltrimethylammonium bromide, the hydrophilic solvent is n-butanol, and the oil-phase solvent is n-heptane, the yield of the precursor Co x Zn 1-x -MOF is the highest.
[0016] In some embodiments that may include the above embodiments, in the precursor Co x Zn 1-x -MOF, the value of x is 0 < x ≤ 0.1.
[0017] Preferably, when x = 0.05, the oxygen reduction activity and stability of the two-dimensional MOF-derived two-dimensional cobalt-nitrogen-doped carbon material calcined from the precursor Co 0.05 Zn 0.95 -MOF are significantly higher than those of commercial Pt / C, and it has the best electrocatalytic oxygen reduction performance.
[0018] Specifically, the precursor Co x Zn 1-x -MOF is a metal-organic framework material with 1-carboxymethylpyrazole-4-carboxylic acid as a ligand and containing Co and Zn ions, and its chemical formula is [Co x Zn 1-x L(H2O)]·H2O, where 0 < x ≤ 0.1. The asymmetric unit of this precursor Co x Zn 1-x -MOF includes 1 metal ion and 1 deprotonated organic ligand L 2-, 1 coordinated water, 1 lattice water, the metal atom has a five-coordinate environment, with 3 carboxyl oxygen atoms (O1A, O2A, O4B), 1 pyrazole nitrogen atom (N1) and 1 coordinated water oxygen atom (O1W); the precursor Co x Zn 1-x -MOF consists of asymmetric units connected to each other through pyrazole carboxylic acid bridges to form a two-dimensional layered structure as shown below:
[0019]
[0020] The second aspect of the embodiments of the present application also provides a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material, which is a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material prepared by the above method.
[0021] A third aspect of the embodiments of the present application also provides the application of the above-mentioned MOF-derived two-dimensional cobalt-nitrogen-doped carbon material in battery positive electrode materials.
[0022] Compared with the prior art, the embodiments of the present application have the following beneficial effects:
[0023] 1. This application is provided by 2D Co x Zn 1-x - Two-dimensional cobalt-nitrogen-doped carbon materials prepared from MOF precursors can be used as oxygen reduction electrocatalysts. Compared with commercial precious metal electrocatalysts Pt / C, they are low-cost, have easily accessible raw materials, and are easy to prepare;
[0024] 2. This application is provided by 2D Co x Zn 1-x -The two-dimensional cobalt-nitrogen-doped carbon material prepared from the MOF precursor can obtain an electrocatalyst with good electrocatalytic oxygen reduction performance by adjusting the metal ion ratio. The electrocatalyst has abundant and exposed active sites, and the electrocatalyst performance (half-wave potential 0.886V) is significantly better than that of the commercial noble metal electrocatalyst Pt / C (half-wave potential 0.845V);
[0025] 3. The MOF-derived two-dimensional cobalt-nitrogen-doped carbon material in the embodiment of the present application has a better discharge performance in the flexible and foldable zinc-air battery assembled compared with the commercial precious metal electrocatalyst Pt / C. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0027] Figure 1Powder X-ray diffraction spectra of NC, Co SAs-NC, and Co NPs-NC materials prepared in Comparative Example 1 and Examples 1-2;
[0028] Figure 2 is the Co 2p X-ray photoelectron spectrum of the Co SAs-NC and Co NPs-NC materials prepared in Examples 1 and 2;
[0029] Figure 3 The precursor Co prepared in Example 1 0.05 Zn 0.95 -Scanning electron microscopy images of MOF (before calcination) and Co SAs-NC (after calcination);
[0030] Figure 4 are the linear scan cyclic voltammetry curves of NC, Co SAs-NC, Co NPs-NC and commercial Pt / C prepared in Comparative Example 1 and Examples 1-2;
[0031] Figure 5 is the stability test curve of Co SAs-NC prepared in Example 1 and commercial Pt / C;
[0032] Figure 6 The discharge curve and power density curve of the aqueous zinc-air battery assembled with Co SAs-NC prepared in Example 1 and commercial Pt / C, respectively;
[0033] Figure 7 This is a photo of an aqueous zinc-air battery assembled with Co SAs-NC prepared in Example 1 lighting up an LED;
[0034] Figure 8 1 are the discharge curves and power density curves of the flexible zinc-air battery assembled with the Co SAs-NC prepared in Example 1 and commercial Pt / C, respectively;
[0035] Fig. 9 Photos of the flexible zinc-air battery assembled with Co SAs-NC prepared in Example 1 lighting up the LED at different bending angles. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0037] Unless otherwise specified, the experimental methods used in the examples of this application are all conventional methods.
[0038] In the following examples and comparative examples, unless otherwise specified, all raw materials can be obtained by commercial purchase or conventional methods.
[0039] Example 1
[0040] A method for preparing a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material (Co SAs-NC) comprises the following steps:
[0041] 0.5 g of hexadecyltrimethylammonium bromide was weighed and added to a mixed organic solvent consisting of 5 mL of n-butanol and 25 mL of n-heptane to obtain a mixed solution. 0.1701 g of 1-carboxymethylpyrazole-4-carboxylic acid ligand was dissolved in 2.5 mL of water and then added dropwise to the mixed solution. Then 0.2085 g of zinc acetate dihydrate and 0.0125 g of cobalt acetate tetrahydrate were dissolved in 2.5 mL of water and then added dropwise to the mixed solution. The mixture was stirred and reacted at room temperature for 3 h. After the reaction was completed, 0.2206 g of precursor Co was obtained after centrifugation, washing and drying. 0.05 Zn 0.95 -MOF, yield 81.86%;
[0042] The precursor Co 0.05 Zn 0.95 -MOF was placed in a tubular furnace with a heating rate of 5°C / min. After calcination at 900°C for 2h in a nitrogen atmosphere, it was cooled to room temperature to obtain a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material, denoted as Co SAs-NC.
[0043] Example 2
[0044] A method for preparing MOF-derived two-dimensional cobalt-nitrogen doped carbon material (Co NPs-NC) comprises the following steps:
[0045] 0.5 g of hexadecyltrimethylammonium bromide was weighed and added to a mixed organic solvent consisting of 5 mL of n-butanol and 25 mL of n-heptane to obtain a mixed solution. 0.1701 g of 1-carboxymethylpyrazole-4-carboxylic acid ligand was dissolved in 2.5 mL of water and then added dropwise to the mixed solution. Then 0.1976 g of zinc acetate dihydrate and 0.0249 g of cobalt acetate tetrahydrate were dissolved in 2.5 mL of water and then added dropwise to the mixed solution. The mixture was stirred and reacted at room temperature for 3 h. After the reaction was completed, 0.2173 g of precursor Co was obtained after centrifugation, washing and drying. 0.1 Zn 0.9 -MOF, yield 80.63%;
[0046] The precursor Co 0.1 Zn 0.9-MOF was placed in a tubular furnace with a heating rate of 5°C / min. After calcination at 900°C for 2h in a nitrogen atmosphere, it was cooled to room temperature to obtain MOF-derived two-dimensional cobalt-nitrogen co-doped carbon material, denoted as Co NPs-NC.
[0047] Comparative Example 1
[0048] A method for preparing a MOF-derived two-dimensional nitrogen-doped carbon material (NC) comprises the following steps:
[0049] Weigh 0.5 g of hexadecyltrimethylammonium bromide and add it to a mixed organic solvent consisting of 5 mL of n-butanol and 25 mL of n-heptane to obtain a mixed solution, dissolve 0.17 g of 1-carboxymethylpyrazole-4-carboxylic acid ligand in 2.5 mL of water and then drop it into the mixed solution, then dissolve 0.2195 g of zinc acetate dihydrate in 2.5 mL of water and then drop it into the mixed solution, stir and react at room temperature for 3 h, after the reaction is completed, centrifuge, wash and dry to obtain 0.2238 g of precursor Zn-MOF, with a yield of 83.04%;
[0050] The precursor Zn-MOF was placed in a tubular furnace with a heating rate of 5°C / min. After calcination at 900°C for 2h in a nitrogen atmosphere, it was cooled to room temperature to obtain a nitrogen-doped MOF-derived carbon material, recorded as NC.
[0051] Test Example 1
[0052] The powder X-ray diffraction patterns of NC, Co SAs-NC and Co NPs-NC materials prepared in Comparative Example 1 and Examples 1-2 are as follows: Figure 1 As shown in Figure 2, the peak of Co element was found in Co NPs-NC materials, but not in Co SAs-NC. Figure 2 From the comparison of the X-ray photoelectron spectra of Co 2p of Co SAs-NC and Co NPs-NC materials, it can be seen that there is an additional spectral peak belonging to the Co element in the Co NPs-NC material, while there is no such peak in the Co SAs-NC, indicating that the Co species is dispersed at the atomic level in the Co SAs-NC material. Figure 3 3 is a scanning electron microscope image of the Co SAs-NC material prepared in Example 1 before and after calcination, and its good two-dimensional lamellar structure can be seen.
[0053] Test Example 2
[0054] 3 mg of the materials prepared in Examples 1-2 and Comparative Example 1 and commercial Pt / C were added to a mixed solution consisting of 575 μL of ethanol and 25 μL of 5 wt% Nafion, and then ultrasonically treated to uniformly disperse the catalyst in the solution to obtain a catalyst slurry.
[0055] Use a pipette to draw 2 μL of catalyst slurry each time (four times in total) and drop it on the rotating disk electrode. After the catalyst on the electrode is dried, a working electrode is obtained. A three-electrode system consisting of a silver / silver chloride electrode (reference electrode), a graphite electrode (auxiliary electrode), and a catalyst-loaded rotating disk electrode (working electrode) is used to measure a linear sweep voltammetric curve at 1600 rpm in an oxygen-saturated 0.1 M KOH solution. Figure 4 As shown in the figure, for the NC material prepared in Comparative Example 1, its half-wave potential is only 0.814V, which is lower than the half-wave potential of commercial platinum carbon, 0.845V. For CoSAs-NC and Co NPs-NC containing Co active species, their half-wave potentials are 0.886V and 0.854V, respectively, exceeding commercial platinum carbon. The more Co content, the lower its catalytic activity, indicating that the Co SAs-NC prepared in Example 1 has excellent electrocatalytic oxygen reduction activity.
[0056] The stability of Co SAs-NC materials and Pt / C was tested. Figure 5 As shown in the figure, the current density of Co SAs-NC material decreased by 8.11% after running for 10 h, while the current density of Pt / C decayed by 19.12%, indicating that under the same conditions, CoSAs-NC material has better stability than commercial Pt / C.
[0057] Test Example 3
[0058] Based on the excellent electrocatalytic oxygen reduction performance of the Co SAs-NC material prepared in Example 1, it was prepared with commercial Pt / C into catalyst slurry according to the method in Test Example 2, and then dropped onto carbon paper to make the cathode of the zinc-air battery. The zinc sheet was used as the anode and a 6M KOH solution was used as the electrolyte solution to assemble the zinc-air battery.
[0059] The discharge performance of zinc-air batteries assembled with Co SAs-NC materials and commercial Pt / C was tested respectively. The discharge curves and power density curves are shown in Figure 2. Figure 6 The peak power density of the zinc-air battery assembled with commercial Pt / C is 89mW.cm -2 The peak power density of the zinc-air battery assembled with Co SAs-NC material is significantly improved, reaching 134 mW.cm -2 . It shows that under the same conditions, the zinc-air battery assembled with Co SAs-NC material has better discharge performance.
[0060] In order to study the practical application of zinc-air batteries assembled with Co SAs-NC materials, their positive and negative electrodes were connected to LED lights, respectively. Figure 7As shown, the zinc-air battery assembled based on Co SAs-NC materials can easily light up LED lights, indicating its feasibility in practical applications.
[0061] Test Example 4
[0062] In order to further expand the application range of the prepared catalyst, a flexible zinc-air battery with certain portability and bendability was assembled. The conductive gel prepared with N,N-methylenebisacrylamide as the solid electrolyte, the carbon paper loaded with the catalyst as the cathode of the flexible zinc-air battery, and the zinc sheet as the anode, and the conductive gel was sandwiched between the two to assemble into a flexible zinc-air battery.
[0063] The discharge performance of flexible zinc-air batteries assembled with Co SAs-NC materials and commercial Pt / C was tested respectively. The discharge curves and power density curves are shown in Figure 2. Figure 8 The peak power density of the zinc-air battery assembled with commercial Pt / C is 12.4 mW.cm -2 The peak power density of the zinc-air battery assembled with Co SAs-NC material is significantly improved to 16 mW.cm -2 Under the same conditions, the flexible zinc-air battery assembled with Co SAs-NC material has better discharge performance.
[0064] In order to study the practical application of flexible zinc-air batteries assembled with Co SAs-NC materials, their positive and negative electrodes were connected to LED lights, respectively. Fig. 9 As shown, the flexible zinc-air battery assembled based on Co SAs-NC material can not only easily light up the LED lamp, but also can still light up the LED lamp even after being bent to different degrees, indicating that it has good bendability and practicality.
[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material, characterized in that: The following steps are involved: (1) dissolving a surfactant in a mixed organic solvent to obtain a solution A; The metal salt and 1-carboxymethylpyrazole-4-carboxylic acid were dissolved in water to obtain solution B and solution C respectively. Solution B and solution C were successively dropped into solution A and stirred at room temperature for reaction. After the reaction was completed, the precursor Co was obtained after centrifugation, washing and drying. x Zn 1-x -MOF; (2) The precursor Co x Zn 1-x -MOF was calcined under an inert atmosphere to obtain MOF-derived two-dimensional cobalt-nitrogen-doped carbon material.
2. The method for preparing the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (2), the calcination temperature is 800-1000° C., the calcination time is 2-4 hours, the heating rate is 4-6° C. / min, and the inert atmosphere is nitrogen.
3. The method for preparing the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (1), the stirring reaction time is 2 to 4 hours.
4. The method for preparing the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (1), the molar ratio of 1-carboxymethylpyrazole-4-carboxylic acid, metal salt and surfactant is 1:[1-2]:[1-3].
5. The method for preparing the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (1), the metal salt includes a Zn salt and a Co salt; wherein the Zn salt is zinc acetate dihydrate, the Co salt is cobalt acetate tetrahydrate, and the molar ratio of Co ions to total metal ions is (0-0.1]:
1.
6. The method for preparing the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (1), the surfactant is at least one of hexadecyltrimethylammonium bromide, sodium dodecyl sulfate and sodium hexadecyl sulfate.
7. The method for preparing a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: In step (1), the mixed organic solvent includes a hydrophilic solvent and an oil phase solvent; wherein the hydrophilic solvent is n-propanol and / or n-butanol, and the oil phase solvent is n-heptane and / or cyclohexane; and the volume ratio of water, the hydrophilic solvent and the oil phase solvent is 1:1:[4-6].
8. The method for preparing a MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 1, characterized in that: The precursor Co x Zn 1-x -The value of x in MOF is 0 <x≤0.1。 9. A MOF-derived two-dimensional cobalt-nitrogen-doped carbon material, characterized in that: A MOF-derived two-dimensional cobalt-nitrogen-doped carbon material prepared by the method described in any one of claims 1 to 8.
10. Use of the MOF-derived two-dimensional cobalt-nitrogen-doped carbon material according to claim 9 in the positive electrode material of zinc-air batteries.