Electrode felt of flow battery and preparation method of electrode felt
By performing low-temperature carbonization, water vapor etching and impregnation and activation of the carbon fiber felt, the problem of insufficient hydrophilicity and conductivity of the liquid flow battery electrode felt is solved, and the battery energy efficiency and production are improved Efficiency, achieving more efficient electrochemical activity and specific surface area.
Patent Information
- Application Number
- CN202411106551.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
AI Technical Summary
The electrode felt of the liquid flow battery has problems such as poor hydrophilicity, insufficient conductivity, poor electrocatalyticity and electrochemical reversibility, resulting in low energy conversion efficiency of all vanadium flow batteries, low production technology efficiency and poor process connection.
By performing low-temperature carbonization and water vapor etching on the carbon fiber felt, the Au-CNTs@MOF precursor solution is impregnated, and dried, activated and in-situ reduction are carried out to form Au-CNTs@MOF, improving the conductivity and electrochemistry of the electrodes. active.
It significantly improves the hydrophilicity and electrochemical reversibility of the liquid flow electrode felt, increases the specific surface area and electrocatalyticity, improves the battery energy efficiency to 90% @80mA/cm2, shortens the process flow, and improves the production efficiency.
Smart Images

Figure CN119008990A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrode felts, and in particular to a liquid flow battery electrode felt and a preparation method thereof. Background Art
[0002] All-vanadium redox flow batteries (VRFBs) are large-capacity energy storage batteries, mainly composed of an infusion pump, a storage tank, and a stack. The stack is mainly composed of a current collector, a bipolar plate, an electrode, and a diaphragm. Flow battery electrode felt is a key component of all-vanadium flow batteries, and its performance directly affects the energy efficiency of flow batteries. Flow battery electrode felt generally has problems such as poor hydrophilicity, insufficient conductivity, poor electrocatalysis, and poor electrochemical reversibility, which directly affect the energy conversion efficiency of all-vanadium flow batteries.
[0003] The preparation method of flow battery electrode felt mainly includes oxidizing the carbon fiber felt to increase the oxygen-containing functional groups to improve the hydrophilicity of the flow electrode felt; or increasing the conductivity of the electrode felt by compounding with graphene, carbon nanotubes, etc.; or loading metal bismuth and metal iridium on the surface of the carbon fiber felt to increase the electrochemical activity of the electrode;
[0004] At present, the production of flow battery electrode felt mainly includes carbonization / graphitization, activation, and post-treatment. These three processes are handled separately and do not achieve efficient coordination. The shortcomings of existing production technology are mainly manifested in: 1) Insufficient activation effect leads to low battery energy efficiency, which is specifically manifested in poor hydrophilicity, insufficient conductivity, poor electrocatalytic properties and other problems. 2) The existing technology for producing flow battery electrode felt has low production efficiency and poor process connection. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a liquid flow battery electrode felt and a preparation method thereof, which can effectively solve the above-mentioned problems of the prior art.
[0006] Technical Solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] The present invention provides a liquid flow battery electrode felt, which is prepared by subjecting the carbon fiber felt to low-temperature carbonization treatment and water vapor etching treatment in sequence, and then immersing it in an Au-CNTs@MOF precursor solution, and then drying, activating and in-situ reducing the Au-CNTs@MOF precursor solution; the Au-CNTs@MOF precursor solution comprises metal chloride, carbon nanotubes and an acid solution.
[0009] Furthermore, the low-temperature carbonization treatment process is as follows: the carbon fiber felt is carbonized and graphitized in a continuous carbonization graphitization furnace, with nitrogen as the protective gas, the graphitization temperature is 800-1600° C., and the winding speed is 0.45-0.5 m / min.
[0010] Furthermore, the carbon fiber felt before low-temperature carbonization has a bulk density of 0.14-0.16 g / cm 2 , surface density tolerance ≤7.5%, thickness tolerance ≤7.5%.
[0011] Furthermore, the water vapor etching treatment process is as follows: the low-temperature carbonized carbon fiber felt is etched on the surface of the carbon fiber felt in a water vapor (desalted water) atmosphere using a continuous atmosphere furnace; wherein the furnace temperature is 700-1000°C, the water vapor pressure is 2-8Bar, and the treatment time is 15-60min.
[0012] Furthermore, the metal chloride is at least one or more of AuCl3, MnCl or AgCl; the carbon nanotubes are carboxylated carbon nanotubes or amino carbon nanotubes; and the acid solution is hydrochloric acid.
[0013] Furthermore, the Au-CNTs@MOF precursor solution includes 0.1-0.2 mol / L metal chloride, 0.01-0.1 g / mL carbon nanotubes and 2-5 mol / L acid solution.
[0014] Preferably, the metal chloride is AuCl3;
[0015] Preferably, 100 mL of AuCl3 (or MnCl2 or AgCl) is added to every 0.1 g of carboxylated carbon nanotubes (or amino carbon nanotubes), and an appropriate amount of hydrochloric acid is added to adjust the pH to 2-4;
[0016] Preferably, the acid solution is hydrochloric acid.
[0017] Furthermore, the preparation method of the Au-CNTs@MOF precursor solution is as follows:
[0018] Weigh the corresponding weight of carbon nanotubes and suspend them in a metal chloride solution, adjust the pH to 2-4 by adding hydrochloric acid, fully disperse them by ultrasonic vibration for 3-5 hours, and place them in a water bath at a constant temperature of 70-90° C. for 6-10 hours to prepare an Au-CNTs@MOF precursor solution.
[0019] Preferably, the preparation method of the Au-CNTs@MOF precursor solution is as follows:
[0020] 1) Prepare a solution of AuCl3 (or MnCl2 or AgCl) and hydrochloric acid with the above concentrations;
[0021] 2) Weigh the corresponding weight of carboxylated carbon nanotubes (or amino carbon nanotubes) and suspend them in a solution containing AuCl3 (or MnCl2 or Agcl), adjust the pH to 2-4 by adding hydrochloric acid, fully disperse them by ultrasonic vibration for 4 hours, place them in a water bath at 80°C for 8 hours to prepare the required solution, i.e., Au-CNTs@MOF precursor solution.
[0022] Furthermore, the activation and in-situ reduction treatment process is as follows:
[0023] The dried carbon fiber felt is placed in a tubular furnace, NH3 gas is introduced, and the reaction is carried out at 300-500℃ for 20-40h. The metal ions in the metal chloride on the surface of the carbon fiber are reduced to nanoparticles and further form coordination bonds with carbon nanotubes to generate Au-CNTs@MOF in situ on the surface of the carbon fiber.
[0024] Preferably, the activation and in-situ reduction treatment process is as follows: the dried carbon fiber felt is placed in a tubular furnace, 1L / min NH3 gas is introduced, and the reaction is carried out at 400°C for 30 hours. The metal ions in AuCl3 (or MnCl2 or AgCl) on the surface of the carbon fiber are reduced to nanoparticles and further form coordination bonds with carboxylated carbon nanotubes (or amino carbon nanotubes) to generate Au-CNTs@MOF in situ on the surface of the carbon fiber.
[0025] A method for preparing a flow battery electrode felt comprises the following steps:
[0026] 1) Low temperature carbonization: Carbonization and graphitization of carbon fiber felt in a continuous carbonization and graphitization furnace;
[0027] 2) Water vapor etching: The low-temperature carbonized carbon fiber felt is etched on the surface of the carbon fiber felt in a continuous atmosphere furnace under a water vapor (desalted water) atmosphere;
[0028] 3) Prepare Au-CNTs@MOF precursor solution: weigh the corresponding weight of carbon nanotubes and suspend them in a metal chloride solution, adjust the pH to 2-4 by adding hydrochloric acid, fully disperse them by ultrasonic vibration for 3-5 hours, and place them in a water bath at 70-90° C. for 6-10 hours to prepare Au-CNTs@MOF precursor solution;
[0029] 4) Impregnation: The carbon fiber felt subjected to the hydrophilic treatment in step 2) is immersed in the Au-CNTs@MOF precursor solution for full adsorption, and then dried;
[0030] 5) Activation and in-situ reduction: Place the carbon fiber felt dried in step 4) in a tubular furnace, introduce NH3, and react at 300-500°C for 20-40 hours.
[0031] Beneficial Effects
[0032] Compared with the known public technology, the technical solution provided by the present invention has the following beneficial effects:
[0033] (1) The specific surface area is increased by etching the surface of the carbon fiber felt, thereby improving the hydrophilicity.
[0034] (2) The redox activity and electrochemical reversibility of the flow electrode felt are increased.
[0035] (3) Untreated carbon fiber electrodes cannot be charged and discharged normally. The energy efficiency of treated carbon fiber electrodes is about 90% @ 80mA / cm 2 , activating and growing gold nanoparticles in situ at the same time, shortening the process flow and improving production efficiency.
[0036] (4) The present invention can improve the conductivity and specific surface area of the liquid flow electrode felt by innovatively introducing Au-CNTs@MOF and in-situ growing Au-CNTs@MOF on carbon fiber. At the same time, since Au-CNTs@MOF has strong electrochemical catalysis and abundant active sites, it can increase the redox activity of the liquid flow electrode felt. Chloroauric acid is replaced by Au-CNTs@MOF, which has the advantages of better electrocatalysis, larger specific surface area, better reaction activity and stability.
[0037] (5) During the high-temperature activation process of the carbon fiber felt, not only are N atoms introduced to improve the electrocatalytic property of the electrode, but Au-CNTs@MOF is also grown in situ on the carbon fiber surface, shortening the process and improving production efficiency.
[0038] (6) Conventional process flow: carbon fiber felt - impregnation with metal ion solution - reduction to metal nanoparticles - metal particles and organic ligands form MOF - activation. The process flow of the present invention: carbon fiber felt - impregnation with metal ion solution - activation, while metal ions are reduced to metal nanoparticles and form MOF with organic ligands, improving efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 This is a microscopic morphology of the carbon fiber felt in Example 1;
[0041] Figure 2 This is a microscopic morphology diagram after water vapor treatment in Example 1;
[0042] Figure 3 This is the microscopic morphology of the electrode felt loaded with Au-CNTs@MOF in Example 1. DETAILED DESCRIPTION
[0043] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] The present invention will be further described below in conjunction with the embodiments.
[0045] The raw material manufacturers and models used in the embodiments and comparative examples are as follows:
[0046] PAN-based pre-oxidized felt, Hangzhou Weiken New Material Technology Co., Ltd.;
[0047] Carboxylated carbon nanotubes, carboxylated multi-walled carbon nanotube powder from Guangdong Innovation Materials (Shenzhen) Co., Ltd.;
[0048] Aminated carbon nanotubes, aminated multi-walled carbon nanotube powder from Guangdong Innovation Materials (Shenzhen) Co., Ltd.;
[0049] (I) Embodiment
[0050] Embodiment 1:
[0051] A flow battery electrode felt, the preparation steps of which are as follows:
[0052] ① Low temperature carbonization. Select a bulk density of 0.15g / cm 2 PAN-based pre-oxidized felt with a thickness of 5.0 mm and a thickness tolerance of ≤7.5% was carbonized and graphitized in a continuous carbonization and graphitization furnace. Under the condition of nitrogen as the protective gas, the graphitization temperature was 1200°C and the winding speed was 0.45 m / min to obtain low-temperature carbonized PAN-based carbon felt. The advantage of low-temperature carbonization of PAN-based carbon felt is that the water vapor etching effect in the next step is more obvious.
[0053] ② Water vapor etching. Place the PAN-based carbon felt that has been carbonized at low temperature in the previous step in a continuous atmosphere furnace with a furnace temperature of 700°C, a water vapor pressure of 6 Bar, and a water vapor flow rate of 0.1 m 3 / h, and the winding speed is controlled to ensure that the treatment time in the water vapor atmosphere reaches 30 minutes. At this time, the surface of the PAN-based carbon felt is etched to increase the specific surface area.
[0054] ③ Prepare Au-CNTs@MOF precursor solution. For every 0.1g of carboxylated carbon nanotubes, prepare 100mL of 0.1mol / L AuCl3, add appropriate amount of hydrochloric acid to adjust the pH to 2, stir and ultrasonically vibrate for 4 hours to fully disperse, place in a water bath at 80℃ for 8 hours to make the required solution, which is the Au-CNTs@MOF precursor solution.
[0055] ④ Impregnation: Immerse the PAN-based carbon felt treated in step ② in the Au-CNTs@MOF precursor solution to fully absorb the liquid, take it out after it is completely wetted, and dry it in a forced air drying oven at 80° C. for 1 hour for use.
[0056] ⑤ Activation and in-situ reduction. The dried carbon fiber felt is placed in a tube furnace, 1L / min of NH3 gas is introduced, and the reaction is carried out at 400℃ for 30h. The metal ions in AuCl3 on the carbon fiber surface are reduced to nanoparticles and further form coordination bonds with carboxylated carbon nanotubes to generate Au-CNTs@MOF on the carbon fiber surface in situ. At the same time, NH3 can also directly react with the carbon fiber body to embed polar and electrochemically active N atoms in the CC bond.
[0057] Through the above steps, a 4 mm thick carbon fiber felt electrode with Au-CNTs@MOF in situ loaded on the surface was prepared.
[0058] Comparative Example 1:
[0059] The only difference from Example 1 is that the low-temperature carbonization treatment in step ① is not performed, and the PAN-based preoxidized felt is directly treated in steps ②-⑤.
[0060] Comparative Example 2:
[0061] The only difference from Example 1 is that step ② treatment is not performed, and the PAN-based carbon felt that has been low-temperature carbonized in step ① is directly treated with steps ③-⑤.
[0062] Comparative Example 3:
[0063] The only difference from Example 1 is that steps ③ and ④ are not performed, and the carbon fiber felt treated in step ② is directly treated in step ⑤.
[0064] Comparative Example 4:
[0065] The only difference from Example 1 is that the precursor solution is a PDA solution, and its specific preparation method is as follows:
[0066] First, prepare an appropriate amount of 10mM / L Tris-HCL buffer: weigh 1.2114g of tris(hydroxymethyl)aminomethane hydrochloride using an electronic balance, dissolve it in 1000ml of deionized water using a magnetic stirrer, take 250ml of this solution after it is completely dissolved, and use a two-point calibrated pH meter to test the pH value of the solution, then use a pipette to drip dilute hydrochloric acid into the solution drop by drop while stirring the solution until the pH meter reads 8.5, and the required Tris-HCL buffer is successfully prepared. Weigh 18.9g of dopamine hydrochloride and dissolve it in 1000ml of Tris-HCL buffer. After stirring for 30min, the solution turns brown, and a dopamine solution with a concentration of 0.1mol / L is obtained.
[0067] Comparative Example 5:
[0068] The only difference from Example 1 is that step ⑤ is not performed.
[0069] (II) Performance test
[0070] Energy efficiency: The test method is "NB_T 42081-2016 All-vanadium liquid flow battery single cell performance test method";
[0071] Resistivity: measured by a four-probe resistivity tester;
[0072] Specific surface area: BET nitrogen adsorption method;
[0073]
[0074]
[0075] In Comparative Example 1, since Comparative Example 1 did not perform the graphitization step, the resistivity of the electrode felt was very high and exceeded the instrument range;
[0076] In Comparative Example 2, since the electrode felt in Comparative Example 2 was not subjected to surface etching, the surface area was very small and the adsorption effect of the precursor solution was poor due to the hydrophobicity of the graphite fiber;
[0077] In Comparative Example 3, since Comparative Example 3 was not impregnated with Au-CNTs@MOF precursor solution, Au particles with strong catalytic activity were missing from the fiber surface, and the obtained electrode felt had poor catalytic activity and low battery energy efficiency;
[0078] In Comparative Example 4, Au-CNTs@MOF has a better catalytic activity than PDA or other common surface modifiers because of the large number of low-coordination index crystal faces that can strongly bind to the catalytic molecules;
[0079] In Comparative Example 5, since the electrode felt was not activated and AuCl3 in the Au-CNTs@MOF precursor solution impregnated on the surface was not reduced, the electrode felt had no catalytic activity, and the battery gained and lost electrons normally, so it could not be charged and discharged normally;
[0080] In the present invention, the energy efficiency of the whole battery is improved by 3% compared with the untreated electrode at a current density of 80 mA / cm 2 The energy efficiency is about 90%. The resistivity is significantly reduced, from 58mΩ·cm to 24mΩ·cm. The specific surface area is significantly increased, from 2.5m 2 / g increased to 883m 2 / g.
[0081] The battery energy efficiency of the liquid flow battery electrode felt prepared by the present invention is greatly improved, the resistivity is significantly reduced, and the specific surface area is significantly increased.
[0082] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present invention.
Claims
1. A flow battery electrode felt, characterized in that: The carbon fiber felt is subjected to low-temperature carbonization treatment and water vapor etching treatment in sequence, and then immersed in Au-CNTs@MOF precursor solution, and then prepared by drying, activating and in-situ reduction; the Au-CNTs@MOF precursor solution includes metal chloride, carbon nanotubes and acid solution.
2. A flow battery electrode felt according to claim 1, characterized in that: The low-temperature carbonization treatment process is as follows: carbonizing and graphitizing the carbon fiber felt in a continuous carbonization graphitization furnace, with nitrogen as the protective gas, the graphitization temperature is 800-1600° C., and the winding speed is 0.45-0.5 m / min.
3. A flow battery electrode felt according to claim 2, characterized in that: The carbon fiber felt before low-temperature carbonization has a bulk density of 0.14-0.16 g / cm 2 , surface density tolerance ≤7.5%, thickness tolerance ≤7.5%.
4. The electrode felt for a liquid flow battery according to claim 1, characterized in that: The water vapor etching treatment process is as follows: the low-temperature carbonized carbon fiber felt is etched on the surface of the carbon fiber felt in a water vapor atmosphere using a continuous atmosphere furnace; wherein the furnace temperature is 700-1000° C., the water vapor pressure is 2-8 Bar, and the treatment time is 15-60 min.
5. The electrode felt for a liquid flow battery according to claim 1, characterized in that: The metal chloride is at least one or more of AuCl3, MnCl2 or AgCl; the carbon nanotube is carboxylated carbon nanotube or amino carbon nanotube; and the acid solution is hydrochloric acid.
6. A flow battery electrode felt according to claim 5, characterized in that: The Au-CNTs@MOF precursor solution includes 0.1-0.2 mol / L metal chloride, 0.01-0.1 g / mL carbon nanotubes and 2-5 mol / L hydrochloric acid.
7. A flow battery electrode felt according to claim 6, characterized in that: The preparation method of the Au-CNTs@MOF precursor solution is as follows: Weigh the corresponding weight of carbon nanotubes and suspend them in a metal chloride solution, adjust the pH to 2-4 by adding hydrochloric acid, fully disperse them by ultrasonic vibration for 3-5 hours, and place them in a water bath at a constant temperature of 70-90° C. for 6-10 hours to prepare an Au-CNTs@MOF precursor solution.
8. The electrode felt for a liquid flow battery according to claim 1, characterized in that: The activation and in-situ reduction treatment process is as follows: The dried carbon fiber felt is placed in a tubular furnace, NH3 gas is introduced, and the reaction is carried out at 300-500℃ for 20-40h. The metal ions in the metal chloride on the surface of the carbon fiber are reduced to nanoparticles and further form coordination bonds with carbon nanotubes to generate Au-CNTs@MOF in situ on the surface of the carbon fiber.
9. A method for preparing a flow battery electrode felt according to any one of claims 1 to 8, characterized in that: It includes the following steps: 1) Low temperature carbonization: Carbonization and graphitization of carbon fiber felt in a continuous carbonization and graphitization furnace; 2) Water vapor etching: The low-temperature carbonized carbon fiber felt is etched on the surface of the carbon fiber felt in a continuous atmosphere furnace under a water vapor (desalted water) atmosphere; 3) Prepare Au-CNTs@MOF precursor solution: weigh the corresponding weight of carbon nanotubes and suspend them in a metal chloride solution, adjust the pH to 2-4 by adding hydrochloric acid, fully disperse them by ultrasonic vibration for 3-5 hours, and place them in a water bath at 70-90° C. for 6-10 hours to prepare Au-CNTs@MOF precursor solution; 4) Impregnation: The carbon fiber felt subjected to the hydrophilic treatment in step 2) is immersed in the Au-CNTs@MOF precursor solution for full adsorption, and then dried; 5) Activation and in-situ reduction: Place the carbon fiber felt dried in step 4) in a tubular furnace, introduce NH3, and react at 300-500°C for 20-40 hours.
Citation Information
Cited By
Flow battery electrode with hierarchical pore structure constructed by copper-MOF in-situ etching and preparation method of flow battery electrode
CN122177853A