- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
During the assembly process of sodium ion battery, the lithium ion battery assembly solution is not applicable, resulting in high failure efficiency and lack of effective methods to improve assembly stability.
A method is proposed to reduce assembly failure efficiency by adjusting the key parameters in the assembly process of sodium ion buckle battery, especially the key factor index σ. The index σ is 20*((s/h-0.9)/0.9)^2+((f/r^2-10)/10)^2. By adjusting the battery case thickness, sealing pressure and other parameters, σ≤ is controlled 0.15 or lower to reduce failure efficiency.
It significantly reduces the failure efficiency of the sodium ion buckle battery assembly process, improves assembly stability and test stability, and provides guiding significance for assembly stability evaluation and prediction.
Smart Images

Figure BDA0004983567150000051 
Figure BDA0004983567150000061 
Figure BDA0004983567150000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and specifically to a method for improving battery assembly stability by adjusting key parameters in the sodium ion button battery assembly process. Background Art
[0002] Sodium-ion batteries are rich in raw materials and cheap, and have excellent low-temperature performance and cycle characteristics. They are conducive to the sustainable development of large-scale energy storage and can be used as a supplement to other batteries under specific requirements of low temperature and long cycle. At present, the electrochemical performance test of sodium-ion battery raw materials is completely based on lithium-ion batteries. However, due to the differences in lithium sheets, sodium sheets, and positive and negative electrode raw material sheets involved in the assembly of button batteries, the assembly scheme of lithium-ion button batteries in actual operation is not completely applicable to the assembly of sodium-ion button batteries, resulting in a high failure rate of sodium-ion button battery assembly. At present, there is a lack of effective methods to control the failure rate in the assembly process of sodium-ion button batteries. The improvement of stability is often tentatively or blindly adjusted based on experience, which makes the effect of improving the stability of battery assembly insignificant and time-consuming and labor-intensive.
[0003] To this end, this application is filed. Summary of the invention
[0004] In view of the above problems in the prior art, the present invention studies the key factors affecting assembly failure during the assembly process of sodium ion button batteries based on the characteristics of sodium ion batteries, and proposes a method for improving the assembly stability of sodium ion button batteries, which can significantly reduce the failure rate caused by the assembly process.
[0005] In a first aspect, the present invention provides a method for improving the assembly stability of sodium ion button cells by reducing a key factor index σ.
[0006] Among them, the key factor index σ is:
[0007] σ=20*((s / h-0.9) / 0.9)^2+((f / r^2-10) / 10)^2
[0008] Wherein, s is the total thickness of the sodium ion button battery excluding the battery shell, in mm; h is the total thickness of the battery shell, in mm; r is the radius of the battery shell, in mm; f is the sealing pressure of the sodium ion button battery, in kg.
[0009] As some preferred solutions, the above key factor index σ≤0.15, or further σ≤0.1, or further σ≤0.01, can control the total failure rate to a lower level.
[0010] As some preferred solutions, the sodium ion button battery includes positive and negative electrode shells, a positive electrode sheet, a negative electrode sheet, a separator, an electrolyte, a gasket and a spring.
[0011] As some more preferred solutions, when the total thickness of the battery shell h≤1.6mm, the thickness of the spring is 0.
[0012] As some preferred schemes, the assembly steps of the sodium ion button battery include: placing the positive electrode sheet, the negative electrode sheet, the diaphragm, the gasket, and the spring sheet into a shell in the order of battery stacking, adding electrolyte, and then covering another shell, and then applying pressure to the covered battery for packaging.
[0013] In a second aspect, the present invention also provides an application of a key factor indicator σ in the evaluation and prediction of the assembly stability of sodium ion button batteries.
[0014] Compared with the prior art, the present invention has at least the following beneficial effects:
[0015] The present invention, through the study and comprehensive consideration of key parameters in the assembly process of sodium ion button batteries, proposes for the first time a key factor indicator σ that is directly related to the total failure rate of sodium ion button battery assembly. The key factor indicator σ is reduced by adjusting and controlling the design parameters, thereby improving the assembly and test stability of sodium ion button batteries, which has important guiding significance for the evaluation and prediction of battery assembly stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0017] Figure 1 This is a graph showing the relationship between the total failure rate and f / (r*r) when s / h is fixed in the present invention.
[0018] Figure 2 This is a graph showing the relationship between the total failure rate and s / h when 10 / (r*r) is fixed.
[0019] Figure 3 It is a scatter plot of the relationship between the key factor index σ of the present invention and the total failure rate. DETAILED DESCRIPTION
[0020] The embodiments of the present invention are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0021] Button cell is a small cylindrical battery, its diameter is usually a few millimeters to more than ten millimeters, and its height is relatively small. Button cell is small in size, easy to carry and install, and is widely used in rapid detection, clocks, small electronic devices, calculators, remote controls, smart cards, RFID tags, sensors, monitoring equipment, etc.
[0022] The structure of button batteries usually includes positive and negative electrode shells, positive electrode sheets, negative electrode sheets, diaphragms, electrolytes, gaskets and springs. During assembly, the positive electrode sheets, negative electrode sheets, diaphragms, gaskets and springs are placed into one shell in the order of assembly, and then the electrolyte is added. Then, the other shell is closed, and the closed battery needs to be packaged under a certain pressure to ensure the sealing and structural integrity of the battery.
[0023] The applicant found that in the above process, the battery often fails to assemble due to the influence of multiple factors. The first is the battery material characteristics factor. The differences between sodium-ion batteries and lithium-ion batteries in the types of positive electrode materials and negative electrode sheets (lithium sheets, sodium sheets) lead to large differences in the thickness, pressure resistance, permeability and other aspects of the battery materials, resulting in assembly defects; the second is the structural design factor. The dimensions of button batteries, such as diameter and thickness, including absolute and relative dimensions, lead to obvious deviations in the pressure bearing capacity and deformation resistance of the battery; the third is the process condition factor, including packaging (sealing) pressure, injection pressure, etc., which leads to differences in the wettability of the battery, packaging reliability and other aspects. Moreover, the above-mentioned influencing factors do not have only independent effects on the assembly stability results, but also have mutual influence correlations between the above-mentioned factors. For example, although thickening the battery shell size is beneficial to improving the pressure-bearing capacity and increasing the sealing pressure to promote packaging reliability, it will lead to a reduction in the internal effective space, which will affect the electrolyte capacity and easily affect the wettability, leading to an increase in failure rate. For another example, increasing the sealing pressure is beneficial to ensuring the reliability of the package and promoting electrolyte infiltration, but it may also cause battery deformation or active material peeling and failure due to excessive pressure, which also leads to an increase in failure rate.
[0024] With regard to the many interrelated influences between the above factors, the applicant has successfully screened out the parameters that have a key correlation effect on the early failure rate and the late failure rate (failure rate in the cycle test) during the assembly process of the sodium ion button battery through a large number of experiments, and obtained the contribution degree between the parameters to the total failure rate, and obtained the key factor index σ that can be used to control and evaluate the stability of the sodium ion button battery assembly, specifically:
[0025] σ=20*((s / h-0.9) / 0.9)^2+((f / r^2-10) / 10)^2
[0026] Wherein, s is the total thickness of the sodium ion button battery excluding the battery shell (i.e., the total thickness of the negative electrode sheet, diaphragm, positive electrode sheet, gasket and spring), in mm; h is the total thickness of the battery shell (i.e., the sum of the thickness of the positive electrode shell and the negative electrode shell), in mm; r is the radius of the battery shell, in mm; f is the sealing pressure of the sodium ion button battery, in kg;
[0027] The applicant has found that the smaller the above-mentioned key factor index σ is, the lower the failure rate of the sodium ion button battery after assembly is, and the better the stability and reliability of assembly and testing is.
[0028] After analysis, the applicant believes that the above key factor index σ comprehensively reflects the key influencing factors in the assembly process of sodium ion button batteries, the correlation between key influencing factors, and the contribution rate of key influencing factors and their correlation, and therefore has guiding significance for guiding the assembly method of sodium ion button batteries. Among them, s / h reflects the thickness of the non-shell part of the battery relative to the shell part, takes into account the balance of thickness matching and force of the sodium ion battery, and participates in the key factor index control with the central magnification contribution rate, f / r^2 reflects the main influence of the battery force on the battery shell area, and participates in the key factor index control with the central magnification contribution rate, and at the same time, the amplified contribution rates of the two aspects are superimposed due to the correlation effect, thereby obtaining σ.
[0029] As some further solutions, we found that by controlling the above-mentioned key factor indicator σ below 0.15, the total failure rate of assembly can be basically controlled below 20%; by controlling the above-mentioned key factor indicator σ below 0.1, the total failure rate of assembly can be basically controlled below 15%; by controlling the above-mentioned key factor indicator σ below 0.01, the total failure rate of assembly can be basically controlled below 10%.
[0030] Since the key factor index σ of the present invention has correlation and consistency with the total failure rate, the key factor index σ can also be used to evaluate and predict the assembly stability of sodium ion button batteries. The smaller the key factor index σ is, the better the stability of the battery after assembly is expected to be.
[0031] The present invention is further described and verified by specific examples below. In the examples, based on the raw materials of the positive electrode of the sodium ion battery, a series of sodium ion button batteries are prepared by taking CR2032 battery shell as an example.
[0032] Example 1
[0033] Preparation of positive electrode sheet: weigh 5g of materials with a total weight of 8:1:1 ratio of sodium ion battery positive electrode raw material: polyvinylidene fluoride: conductive agent superp, that is, weigh 4.0g of sodium ion battery positive electrode raw material, 0.5g of polyvinylidene fluoride, and 0.5g of conductive agent superp. p was put into a mortar and ground for 15 minutes, and then put into a mixer; 0.5g of the weighed polyvinylidene fluoride was put into a 10g N-methylpyrrolidone solution and dispersed at a speed of 200r / min for 1h to obtain a binder solution, and put into the mixer; the mixer parameters were set to centrifuge at 1000r / min for 10min, 1500r / min for 10min, and 1000r / min for 10min, and the operation was repeated twice to obtain a positive electrode material slurry; the above-mentioned positive electrode material slurry was coated on an aluminum foil with a coating thickness of about 250um; the aluminum foil coated with the slurry was dried at 90°C for 2h, and then the dried aluminum foil was cut into a positive electrode sheet with a size of φ12 by a cutting machine, the mass of the electrode sheet was weighed, and then the electrode sheet was placed in a self-sealing bag and dried in a vacuum drying oven at 110°C for 12h to obtain a dried positive electrode sheet.
[0034] Assemble button cells: This is done in a glove box with a water and oxygen content of <0.01ppm. Take positive and negative battery shells of model CR2032. The total thickness of the battery shell is 3.2mm and the radius is 10mm. Place the negative electrode shell flat on the table; clamp a negative electrode metal sodium sheet with a size of φ14, tear off its double-sided protective film and place it at the center of the negative electrode shell; clamp a glass fiber diaphragm with a model of GF / D and a size of φ16, and place it on the negative electrode metal sodium sheet; use a pipette to take a sodium perchlorate electrolyte of 185±5um, and evenly drip it on the diaphragm to make it infiltrated; clamp the positive electrode sheet prepared in the above steps, and place it with its coated surface facing down to the diaphragm; clamp a metal gasket and place it above the positive electrode sheet; clamp a metal shrapnel and place it above the gasket, and then cover the positive electrode shell; the total thickness of the negative electrode metal sodium sheet, glass fiber diaphragm, positive electrode sheet, metal gasket, and metal shrapnel is 2.9mm; place the assembled battery in a sealing machine, adjust the sealing machine pressure to 800kg, and the pressure holding time to 5s, and obtain a complete button battery after sealing.
[0035] Embodiments 2 to 47
[0036] The same method as in Example 1 was used, while changing the relevant parameters in the battery assembly process, and the parameter changes were listed in Table 1. When the total thickness of the battery shell h≤1.6 mm, no spring sheet was placed, and the spring sheet thickness was considered to be 0.
[0037] Table 1
[0038]
[0039]
[0040]
[0041] For the above embodiment, we first observed the change between the total failure rate and f / (r*r) under the condition that s / h is fixed at about 0.9, as shown in Figure 1 As shown in the figure, it can be seen that when the thickness is fixed, as the ratio of the sealing pressure to the square of the radius f / (r*r) gradually increases, the total failure rate shows a trend of first decreasing and then increasing. The change in this trend is related to the impact of factors such as the edge packaging, contact conditions, internal material stress damage, structural deformation, micro short circuit or open circuit of the sodium ion battery when the sealing pressure is too large or too small. It can be seen that when the thickness is fixed, f / (r*r) has a central amplification effect on the total failure rate.
[0042] At the same time, we also observed the changes between the total failure rate and s / h under the condition that the sealing pressure is fixed at 10 / (r*r), as shown in Figure 2 As shown in the figure, it can be seen that when the sealing pressure is fixed, s / h also has a central amplification trend on the total failure rate. This is related to the influence of the redundant space inside the battery on the contact or extrusion of the positive and negative electrodes and the diaphragm and gasket parts, as well as its influence on wetting, deformation, micro short circuit or open circuit.
[0043] Combined with the above effects, and further combined with Examples 1 to 47, we can see that the key factor index σ, σ = 20*((s / h-0.9) / 0.9)^2+((f / r^2-10) / 10)^2, has a correlation with the total failure rate. As σ decreases, the total failure rate follows the general trend of continuous decrease. Figure 3 As shown, the scatter plot of the relationship between the key factor index σ of the present invention and the total failure rate of Examples 1 to 47 also fully demonstrates and proves this correlation. It should be noted that although there are deviations in individual examples in the embodiments, it does not affect the correlation judgment between the key factor index σ and the total failure rate in the overall trend. The proposal and control of the key factor index σ is of guiding significance for improving the assembly stability of sodium ion button batteries.
[0044] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.
Claims
1. A method for improving the assembly stability of sodium ion button cells by reducing the key factor index σ. in, The key factor index σ is: σ=20*((s / h-0.9) / 0.9)^2+((f / r^2-10) / 10)^2 Wherein, s is the total thickness of the sodium ion button battery excluding the battery shell, in mm; h is the total thickness of the battery shell, in mm; r is the radius of the battery shell, in mm; f is the sealing pressure of the sodium ion button battery, in kg.
2. The method for improving the assembly stability of sodium ion button cells according to claim 1, characterized in that: Control the key factor index σ≤0.15, or further σ≤0.1, or further σ≤0.
01.
3. The method for improving the assembly stability of sodium ion button cells according to claim 1, characterized in that: The sodium ion button battery comprises a positive and negative electrode shell, a positive electrode sheet, a negative electrode sheet, a diaphragm, an electrolyte, a gasket and a spring.
4. The method for improving the assembly stability of sodium ion button cells according to claim 3, characterized in that: When the total thickness of the battery shell is h≤1.6 mm, the thickness of the spring is 0.
5. The method for improving the assembly stability of sodium ion button cells according to claim 1, characterized in that: The assembly steps of the sodium ion button battery include: placing the positive electrode sheet, the negative electrode sheet, the diaphragm, the gasket, and the spring sheet into a shell in the order of battery stacking, adding electrolyte, and then covering another shell, and then applying pressure to the covered battery for packaging.
6. Application of the key factor indicator σ described in claim 1 in the assessment and prediction of the assembly stability of sodium ion button batteries.