Polymer gel electrolyte capable of stably circulating at high rate and lithium metal battery based on polymer gel electrolyte
By polymerizing polymer gel electrolytes with crosslinking networks using epoxy ethers and acrylate-containing monomers at room temperature, the problem of poor cycling stability of lithium metal batteries at high magnification is solved, and a more uniform electrolyte distribution is achieved and higher electrochemical stability windows, extend battery life and improve safety performance.
Patent Information
- Application Number
- CN202411306495.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-22
AI Technical Summary
Existing lithium metal batteries have poor cycling stability at high magnifications, and polymer gel electrolytes are unevenly polymerized at high temperatures, resulting in a short battery cycle life, and the oxidation stability of ether-based polymers is limited to voltages below 4V.
Polymerized at room temperature by epoxy ether monomer and acrylate-containing crosslinkable monomer to form a crosslinked polymer network, improve the uniformity and electrochemical stability window of electrolytes, and use carbonate solvents as plasticization The agent and electrolyte salt form polymer gel electrolyte on the battery separator by in situ polymerization.
It improves the cycle stability and electrochemical performance of lithium metal batteries at high magnifications, extends the service life of the battery, reduces the battery impedance, and enhances the safety performance of the battery.
Smart Images

Figure CN119009103A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of lithium metal batteries, and in particular relates to a polymer gel electrolyte with stable circulation at high rate, a lithium metal battery and a preparation method thereof. Background Art
[0002] Rechargeable lithium metal batteries are not only clean and environmentally friendly, but their battery systems also have the advantages of high energy density, long cycle life, low self-discharge, no memory effect and low dependence on temperature. They have been widely used in electric bicycles, electric vehicles, energy storage and other fields.
[0003] Lithium metal batteries based on liquid electrolytes have safety hazards such as easy leakage and flammable organic solvents. Solid electrolytes have problems such as low ionic conductivity at room temperature and poor contact with positive and negative electrode materials, resulting in large interface impedance. Therefore, the development of solid electrolyte materials with high ionic conductivity and high stability is the key to the field of solid-state lithium batteries. The polymer gel electrolyte combines the advantages of liquid electrolytes and solid polymer electrolytes. The elastic gel fits tightly with the electrode, which not only strengthens the contact with the electrode, but also accommodates the volume change of the lithium negative electrode. In addition, the polymer network formed by it helps lithium ion transmission, promotes the migration of lithium ions, and helps to form a more stable solid electrolyte phase interface film, inhibiting the growth of lithium dendrites. At the same time, the polymer gel electrolyte contains some unpolymerized precursor liquid, which can provide better ion conduction and better electrochemical performance than solid electrolytes. In addition, the reaction conditions of polymer electrolytes are mild and easy to form films.
[0004] At present, common polymer gel electrolyte systems often need to be polymerized at high temperatures because the initiator can only work properly at high temperatures, such as polyethylene glycol diacrylate (PEGDA), vinylene carbonate (VC), etc., which generally polymerize at 60°C to 80°C. However, since the heat conduction rates in different phases of the electrolyte are different, the uniformity of the polymerization will also be different, and the uniform distribution of the polymer gel electrolyte on the diaphragm cannot be guaranteed, which affects the cycle life of the battery. Although room temperature polymerization can polymerize more evenly, its degree of polymerization curing is generally not as good as high-temperature polymerization, and more liquid components are retained. In addition, the oxidation stability of common ether-based polymer electrolytes is mostly limited to voltages below 4V, and the cycle stability at high current density is low. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a polymer gel electrolyte with stable circulation at high rate and a preparation method of a lithium metal battery based thereon, wherein epoxy ether monomers and acrylate-containing crosslinkable monomers are polymerized at room temperature to form a polymer gel electrolyte, and the crosslinkable acrylate-containing monomers improve the degree of polymerization by polymerizing to form a crosslinked polymer network while ensuring more uniform room temperature polymerization, thereby improving the electrochemical stability window and charge and discharge cycle performance while ensuring good contact between the electrolyte / electrode, thereby improving the service life of the battery and the cycle stability at high rate.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention firstly discloses a polymer gel electrolyte with stable circulation at high rate. The polymer gel electrolyte is synthesized by in-situ polymerization at room temperature using a mixed solution of a first ether monomer capable of ring-opening polymerization, a second cross-linkable monomer containing acrylate, a carbonate solvent (also serving as a plasticizer), an initiator and an electrolyte salt as an electrolyte prepolymer precursor solution.
[0008] Furthermore, the raw materials of the electrolyte prepolymer precursor solution are composed of 5% to 50% of a first ring-opening polymerizable ether monomer, 2% to 50% of a second cross-linkable acrylate monomer, 10% to 40% of an electrolyte salt, 0.05% to 1% of an initiator, and the remainder is a carbonate solvent.
[0009] Furthermore, the first ether monomer capable of ring-opening polymerization is selected from at least one of 1,3-dioxolane and 1,3-dioxane. Preferably, the first ether monomer capable of ring-opening polymerization is 1,3-dioxolane.
[0010] Further, the acrylate-containing crosslinkable second monomer is selected from at least one of pentaerythritol triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, ethoxypentaerythritol tetraacrylate and dipentaerythritol hexaacrylate. Preferably, the acrylate-containing crosslinkable second monomer is pentaerythritol tetraacrylate.
[0011] Further, the carbonate solvent is selected from at least one of fluoroethylene carbonate, vinylene carbonate, vinyl ethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate and chloroethylene carbonate. Preferably, the carbonate solvent is fluoroethylene carbonate.
[0012] Further, the electrolyte salt is selected from at least one of lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium trifluoromethylsulfonate, lithium bis(trifluoromethylsulfonylimide) and lithium bis(fluorosulfonylimide).
[0013] Furthermore, the initiator is aluminum trifluoromethanesulfonate.
[0014] The method for preparing the polymer gel electrolyte of the present invention comprises the following steps:
[0015] Add the first ether monomer capable of ring-opening polymerization and the second cross-linkable monomer containing acrylate to a carbonate solvent and stir for 10 to 30 minutes; then add the electrolyte salt and stir for 1 to 12 hours to uniformly disperse the electrolyte salt in the solvent; finally add the initiator and stir in an ice bath for 5 to 30 minutes (stirring in an ice bath can effectively avoid premature polymerization) to form a uniformly dispersed electrolyte prepolymer precursor solution;
[0016] After the electrolyte prepolymer precursor liquid is taken out from the ice bath, it is immediately injected into the separator between the positive and negative electrodes of the battery in an environment with a protective atmosphere and an oxygen content and a water content of less than 1 ppm, and in-situ polymerized at room temperature to form a polymer gel electrolyte.
[0017] The present invention further discloses a lithium metal battery, the lithium metal battery comprising a positive electrode sheet, a negative electrode sheet and a polymer gel electrolyte, wherein the polymer gel electrolyte is formed by in-situ polymerization on a separator between the positive electrode sheet and the negative electrode sheet. The specific preparation method may be:
[0018] (1) In an environment with a protective atmosphere and an oxygen content and a water content of less than 1 ppm, an electrolyte prepolymer precursor solution is injected into the separator between the positive and negative electrodes, and a battery is assembled.
[0019] The injection volume is 30 to 120 μL.
[0020] (2) The assembled battery is placed at room temperature for in-situ polymerization.
[0021] The electrolyte prepolymer precursor solution of the present invention can undergo polymerization reaction in a wide temperature range of 0°C to 70°C, and room temperature is most preferred because the battery performance obtained when polymerized at room temperature is optimal. Room temperature here means that no heating or freezing operations are performed, and the reaction is carried out directly at room temperature (18°C to 28°C).
[0022] The polymerization time is 30 minutes to 24 hours.
[0023] Furthermore: the positive electrode material is a ternary material LiNi x Co y Mn zO2 (x + y + z = 1), lithium cobalt oxide LiCoO2 or lithium iron phosphate LiFePO4; the negative electrode material is lithium metal; the separator is selected from one of polyethylene, polypropylene, polyacrylonitrile, poly (vinylidene fluoride-hexafluoroethylene), polymethyl methacrylate, polyimide, polyetherimide, cellulose, aramid and non-woven bacterial cellulose separator. Preferably, the separator is a non-woven bacterial cellulose separator, which has excellent liquid absorption rate and can ensure the uniform distribution of the electrolyte prepolymer precursor solution.
[0024] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0025] 1. In order to alleviate the problems of poor mechanical properties, poor cycle stability and low electrochemical stability window of the polymer system of a single ether monomer, the polymer gel electrolyte provided by the present invention selects a cross-linkable acrylate monomer as the second monomer to participate in room temperature polymerization. While ensuring that the room temperature polymerization is more uniform, the degree of polymerization is improved by forming a cross-linked polymer network through polymerization. The introduction of COC and C=O groups improves the effective coordination-dissociation efficiency between lithium ions and chains, thereby promoting their migration ability, increasing the lithium ion migration number, and effectively reducing the interface internal resistance between the positive and negative electrodes and the separator, thereby improving the electrochemical performance of the battery, ensuring good contact between the electrolyte / electrode, and at the same time improving the electrochemical stability window and charge and discharge cycle performance, thereby increasing the service life of the battery.
[0026] 2. The polymer gel electrolyte provided by the present invention uses fluoroethylene carbonate as the carbonate solvent that also serves as a plasticizer to form a SEI film with a tight structure and excellent performance on the surface of the lithium metal negative electrode, thereby reducing the battery impedance while increasing the battery specific capacity and improving the battery cycle stability.
[0027] 3. When the polymer gel electrolyte of the present invention is used in a battery, a non-woven bacterial cellulose membrane is selected as the supporting material between the positive and negative electrodes, which has a strong liquid absorption capacity and mechanical strength. The battery system constituted exists in the form of a gel, which maintains excellent mechanical strength of the membrane while maintaining good interface contact, thereby improving the safety performance of the battery.
[0028] 4. The polymer gel electrolyte provided by the present invention has a significant effect on improving the electrochemical performance and cycle life of lithium metal batteries at high rates, and its preparation method is convenient and can utilize existing battery production processes and production equipment without increasing equipment investment, and has good industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a SEM image of the surface of the non-woven bacterial cellulose membrane in Example 1.
[0030] Figure 2This is a SEM image of the surface of the polymer gel electrolyte membrane prepared in Example 1.
[0031] Figure 3 1 and 2 are impedance diagrams of the polymer gel electrolyte membranes prepared in Example 1, Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3.
[0032] Figure 4 This is the electrochemical window diagram of the polymer gel electrolyte membrane prepared in Example 1.
[0033] Figure 5 This is a cycle performance diagram of a lithium metal battery assembled using the prepared polymer gel electrolyte membrane in Example 1 at 2C.
[0034] Figure 6 This is a charge and discharge curve of a lithium metal battery assembled using the prepared polymer gel electrolyte membrane in Example 1 at 2C.
[0035] Figure 7 This is a graph showing the cycling performance of a lithium metal battery assembled using the prepared polymer gel electrolyte membrane in Example 1 at 5C.
[0036] Figure 8 This is a cycle performance diagram of a lithium metal battery assembled using the prepared polymer gel electrolyte membrane in Example 2 at 0.5C.
[0037] Fig. 9 The graph is a cycle performance diagram of lithium metal batteries assembled using the prepared polymer gel electrolyte membranes in Comparative Examples 1, 2 and 3 at 0.5C.
[0038] Fig.10 This is a cycle performance diagram of a lithium metal battery assembled using the prepared polymer gel electrolyte membrane in Comparative Example 2 at 2C.
[0039] Fig.11 Optical image of a soft-pack battery assembled using the prepared polymer gel electrolyte membrane. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The following embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following embodiments.
[0041] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0042] Example 1
[0043] This embodiment provides a method for preparing a polymer gel electrolyte, and assembles a lithium metal battery based on the polymer gel electrolyte, comprising the following steps:
[0044] (1) After 0.4 g of 1,3-dioxolane (DOL), 0.4 g of pentaerythritol tetraacrylate (PETEA), and 1.6 g of fluoroethylene carbonate (FEC) were mixed and stirred for 30 min, 0.68 g of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was added and the mixture was stirred for 2 h to fully dissolve the lithium salt, 0.015 g of aluminum trifluoromethanesulfonate (Al(OTf)3) was added, and the mixture was stirred in an ice bath at 0°C for 10 min to obtain a prepolymer precursor solution.
[0045] (2) Using a lithium iron phosphate positive electrode sheet as the positive electrode, a metal lithium sheet as the negative electrode, and a non-woven bacterial cellulose separator (d = 16 mm), 80 μL of prepolymer precursor solution was injected, and an experimental cell was assembled in an argon glove box, and then allowed to stand at 25°C for 12 hours to obtain a polymer gel electrolyte lithium metal battery. The electrochemical performance test was carried out at 25°C.
[0046] The preparation method of the lithium iron phosphate positive electrode sheet is as follows: the lithium iron phosphate positive electrode material is fully mixed with acetylene black and polyvinylidene fluoride (PVDF) in a ratio of 8:1:1 (mass ratio), NMP (1-methyl-2-pyrrolidone) is added to a solid content of 25%, and after stirring for 8 hours, it is evenly coated on an aluminum foil with a coating thickness of 75 μm, and dried at 80°C, rolled and cut into a positive electrode sheet with a diameter of 12 mm, and vacuum dried for use.
[0047] Figure 1 The SEM image of the original non-woven bacterial cellulose membrane surface shows that the average pore size of the non-woven bacterial cellulose membrane is 1 μm, and the maximum pore size exceeds 2 μm.
[0048] Figure 2 The SEM image of the surface of the prepared polymer gel electrolyte membrane shows that after the in-situ polymerization reaction, the polymer is effectively filled in the bacterial cellulose membrane, the surface roughness decreases, the interface impedance between the electrolyte and the electrode is effectively reduced, and the lithium ion conductivity is improved.
[0049] Figure 3 The impedance diagram of the prepared polymer gel electrolyte membrane. It can be seen that the bulk impedance of the electrolyte membrane measured by the blocking electrode method is 5.7Ω, and the ionic conductivity is calculated to be 4.37×10 -4 S / cm, which is greater than the polymer electrolytes currently widely used.
[0050] Figure 4The electrochemical window diagram of the prepared polymer gel electrolyte membrane shows that the oxidation decomposition voltage of the electrolyte membrane is as high as 5V, proving that it can be adapted to positive electrode materials with higher working voltages.
[0051] Figure 5 The cycle performance diagram of the lithium metal battery assembled with the prepared polymer gel electrolyte membrane is shown in FIG. Figure 6 The charge and discharge curve of the lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, the cycle conditions are: 25℃, 2C (1C = 170mAh·g -1 ). It can be seen that the discharge capacity after 1600 cycles is 132.36 mAh g -1 , the cycle retention rate is as high as 98.6% and the Coulombic efficiency is close to 100%.
[0052] Figure 7 The cycling performance diagram of the lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, the cycling conditions are: 25℃, 5C (C=170mAh·g -1 ). It can be seen that the discharge capacity after 1600 cycles is 98.22 mAh g -1 , the cycle retention rate is as high as 82.5% and the Coulombic efficiency is close to 100%.
[0053] Example 2
[0054] This embodiment provides a method for preparing a polymer gel electrolyte, and assembles a lithium metal battery based on the polymer gel electrolyte, comprising the following steps:
[0055] (1) After 0.75 g of 1,3-dioxane (DOX), 0.38 g of pentaerythritol tetraacrylate (PETEA), and 1.5 g of fluoroethylene carbonate (FEC) were mixed and stirred for 30 min, 0.7 g of lithium bis(fluorosulfonyl)imide (LiFSI) was added and the mixture was stirred for 2 h to fully dissolve the lithium salt, 0.015 g of aluminum trifluoromethanesulfonate (Al(OTf)3) was added, and the mixture was stirred in an ice bath at 0°C for 10 min to obtain a prepolymer precursor solution.
[0056] (2) Using a lithium iron phosphate positive electrode sheet as the positive electrode, a metal lithium sheet as the negative electrode, and a non-woven bacterial cellulose separator (d = 16 mm), 80 μL of prepolymer precursor solution was injected, and an experimental cell was assembled in an argon glove box, and then allowed to stand at 25°C for 24 hours to obtain a polymer gel electrolyte lithium metal battery. The electrochemical performance test was carried out at 25°C.
[0057] The preparation method of the lithium iron phosphate positive electrode sheet is the same as that in Example 1 and will not be described again here.
[0058] Figure 3 The impedance diagram of the prepared polymer gel electrolyte membrane. It can be seen that the bulk impedance of the electrolyte membrane measured by the blocking electrode method is 4.04Ω, and the ionic conductivity is calculated to be 6.16×10 -4 S / cm, which is greater than the polymer electrolytes currently widely used.
[0059] Figure 8 The figure shows the cycle performance of a lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, and the cycle conditions are: 25°C, 0.5C (1C = 170mAh g -1 ). It can be seen that the first cycle discharge capacity is 141.8 mAh g -1 After 200 cycles, the discharge capacity is 98.5 mAh g -1 , the cycle retention rate is 74.6% and the Coulombic efficiency is about 99%.
[0060] Comparative Example 1
[0061] In this comparative example, a polymer gel electrolyte was prepared and a lithium metal battery was assembled in the same manner as in Example 1, except that pentaerythritol tetraacrylate (PETEA) was not added during the preparation of the prepolymer precursor solution, stirring was continued at room temperature for 30 minutes instead of stirring in an ice bath at 0°C for 10 minutes, and after the experimental battery was assembled, it was heated in a blast drying oven at 70°C for 8 hours for in-situ thermal polymerization to obtain a polymer gel electrolyte lithium metal battery. The rest is the same as in Example 1 and will not be repeated here.
[0062] Figure 3 The impedance diagram of the prepared polymer gel electrolyte membrane. It can be seen that the bulk impedance of the electrolyte membrane measured by the blocking electrode method is 6.8Ω, and the ionic conductivity is calculated to be 3.66×10 -4 S / cm.
[0063] Fig. 9 The figure shows the cycle performance of a lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, and the cycle conditions are: 25°C, 0.5C (1C = 170mAh g -1 ). It can be seen that the maximum discharge capacity during the charge and discharge cycle is 148.2 mAh g -1 (201st cycle), after 300 cycles, the discharge capacity is 137.8 mAh g -1, the cycle retention rate is 92.98%. When the cycle conditions are changed to 25℃, 2C, the prepared polymer gel electrolyte lithium metal battery cannot be cycled normally.
[0064] Comparative Example 2
[0065] In this comparative example, a polymer gel electrolyte was prepared and a lithium metal battery was assembled in the same manner as in Example 1, except that 1,3-dioxolane (DOL) was not added during the preparation of the prepolymer precursor solution, stirring was continued at room temperature for 30 minutes instead of stirring in an ice bath at 0°C for 10 minutes, and after the experimental battery was assembled, it was heated in a blast drying oven at 70°C for 8 hours for in-situ thermal polymerization to obtain a polymer gel electrolyte lithium metal battery. The rest is the same as in Example 1 and will not be repeated here.
[0066] Figure 3 The impedance diagram of the prepared polymer gel electrolyte membrane. It can be seen that the bulk impedance of the electrolyte membrane measured by the blocking electrode method is 9.23Ω, and the ionic conductivity is calculated to be 2.7×10 -4 S / cm.
[0067] Fig. 9 The figure shows the cycle performance of a lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, and the cycle conditions are: 25°C, 0.5C (1C = 170mAh g -1 ). It can be seen that the maximum discharge capacity during the charge and discharge cycle is 132.4 mAh g -1 (103rd cycle), after 300 cycles, the discharge capacity is 131.6 mAh g -1 , the cycle retention rate is as high as 99.4%.
[0068] Fig.10 The figure shows the cycle performance of a lithium metal battery assembled with the prepared polymer gel electrolyte membrane at 2C. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, and the prepared polymer gel electrolyte lithium metal battery is activated for the first three cycles at 0.1C, and the first cycle discharge capacity is 145.56mAh·g -1 After activation, the cycle condition was 2C, and the discharge capacity after 150 cycles was only 24.37 mAh g -1 .
[0069] The cycle performance of Comparative Examples 1 and 2 at high rates, compared with Example 1, proves that the polymer gel electrolyte provided by the present invention effectively improves the charge and discharge cycle performance of the polymer gel electrolyte lithium metal battery at high rates.
[0070] Comparative Example 3
[0071] In this comparative example, a polymer gel electrolyte was prepared and a lithium metal battery was assembled in the same manner as in Example 1, with the only difference being that 0.8 g of ethylene carbonate (EC) and 0.8 g of diethyl carbonate (DEC) were added instead of adding fluoroethylene carbonate (FEC) during the preparation of the prepolymer precursor solution. The rest was the same as in Example 1 and will not be described again.
[0072] Figure 3 The impedance diagram of the prepared polymer gel electrolyte membrane. It can be seen that the bulk impedance of the electrolyte membrane measured by the blocking electrode method is 5.17Ω, and the ionic conductivity is calculated to be 4.78×10 -4 S / cm.
[0073] Fig. 9 The figure shows the cycle performance of a lithium metal battery assembled with the prepared polymer gel electrolyte membrane. The positive electrode is lithium iron phosphate (LFP), the negative electrode is lithium metal, the battery operating voltage is 2.8-3.6V, and the cycle conditions are: 25°C, 0.5C (1C = 170mAh g -1 ). It can be seen that the first cycle discharge capacity is 153.7 mAh g -1 After 150 cycles, the discharge capacity is 72.2 mAh g -1 The cycle retention rate is 47.00%. When the cycle conditions are changed to 25℃, 2C, the prepared polymer gel electrolyte lithium metal battery cannot be cycled normally.
[0074] Comparative Example 4
[0075] In this comparative example, a polymer gel electrolyte was prepared and a lithium metal battery was assembled in the same manner as in Example 1, except that aluminum trifluoromethanesulfonate (Al(OTf)3) was not added during the preparation of the prepolymer precursor solution, ice bath stirring was not performed, and after the experimental battery was assembled, it was heated in a 70°C forced air drying oven for 12 hours for in-situ thermal polymerization to obtain a polymer gel electrolyte lithium metal battery. The rest is the same as in Example 1 and will not be repeated here.
[0076] Although no initiator was added to the comparative example, polymerization reaction could still occur at 70°C to generate a transparent polymer gel electrolyte. The prepared polymer gel electrolyte lithium metal battery could light up the light-emitting diode, but could not undergo normal battery cycling.
[0077] Example 3
[0078] This embodiment provides a method for preparing a polymer gel electrolyte soft-pack battery, comprising the following steps:
[0079] (1) After 0.4 g of 1,3-dioxolane (DOL), 0.4 g of pentaerythritol tetraacrylate (PETEA), and 1.6 g of fluoroethylene carbonate (FEC) were mixed and stirred for 30 min, 0.68 g of lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) was added and the mixture was stirred for 2 h to fully dissolve the lithium salt, 0.015 g of aluminum trifluoromethanesulfonate (Al(OTf)3) was added, and the mixture was stirred in an ice bath at 0°C for 10 min to obtain a prepolymer precursor solution.
[0080] (2) Cut the non-woven bacterial cellulose membrane into sheets (size: 46 mm × 60 mm), and assemble two sheets of non-woven bacterial cellulose membrane, two sheets of graphite negative electrode sheets (size: 42 mm × 56 mm) and one sheet of ternary material positive electrode sheet (size: 40 mm × 54 mm) into a soft-pack battery cell.
[0081] The preparation method of the ternary material positive electrode sheet is as follows: 0.9 Co 0.05 Mn 0.05 O2), acetylene black and polyvinylidene fluoride (weight average molecular weight 600,000) are ground in a mass ratio of 90:5:5, dispersed in an organic solvent of N-methylpyrrolidone (solid content: 40%) and stirred for 12 hours to obtain a uniform slurry. Then the slurry is coated on an aluminum foil with a coating thickness of 150 μm, placed in an 80°C blast oven for drying for 12 hours, and then the slurry is continuously coated on the other side of the aluminum foil with a coating thickness of 150 μm, placed in an 80°C blast oven for drying for 12 hours, and a double-sided coated positive electrode material is obtained and rolled and cut into sheets (size: 40 mm × 54 mm).
[0082] The preparation method of the graphite negative electrode sheet is as follows: the graphite negative electrode material, acetylene black and sodium alginate are ground in a mass ratio of 90:5:5, dispersed in deionized water (solid content: 20%) and stirred for 12 hours to obtain a uniform slurry. Then the slurry is scraped on the copper foil with a coating thickness of 150μm, placed in an 80℃ forced air oven and dried for 12 hours to obtain a single-sided coated graphite negative electrode material, which is rolled and cut into sheets (size: 42mm×56mm).
[0083] (3) The assembled soft-pack battery cell was encapsulated with an aluminum-plastic film, and 0.8 g of the prepolymer precursor solution obtained in step (1) was injected and then sealed. The cell was allowed to stand at 25° C. for 2 h, and the soft-pack battery was turned over every 30 min to allow the prepolymer precursor solution to fully infiltrate the non-woven bacterial cellulose membrane. The cell was then allowed to stand at room temperature of 25° C. for 24 h to allow the prepolymer precursor solution to polymerize completely, thereby obtaining a solid-state soft-pack battery. The electrochemical performance of the cell was tested at 25° C.
[0084] Fig.11 Optical image of a soft-pack battery assembled using the prepared polymer gel electrolyte membrane.
[0085] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A polymer gel electrolyte with stable cycling at high rates, characterized in that: The polymer gel electrolyte is synthesized by in-situ polymerization using a mixed solution of a first ring-opening polymerizable ether monomer, a second cross-linkable acrylate monomer, a carbonate solvent, an initiator and an electrolyte salt as an electrolyte prepolymer precursor solution.
2. The polymer gel electrolyte according to claim 1, characterized in that: The raw materials of the electrolyte prepolymer precursor solution are composed of the following in percentage by mass: The invention comprises 5% to 50% of a first ring-opening polymerizable ether monomer, 2% to 50% of a second cross-linkable acrylic ester monomer, 10% to 40% of an electrolyte salt, 0.05% to 1% of an initiator, and the balance is a carbonate solvent.
3. The polymer gel electrolyte according to claim 1 or 2, characterized in that: The first ring-opening polymerizable ether monomer is selected from at least one of 1,3-dioxolane and 1,3-dioxane.
4. The polymer gel electrolyte according to claim 1 or 2, characterized in that: The acrylate-containing crosslinkable second monomer is at least one selected from pentaerythritol triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, ethoxypentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.
5. The polymer gel electrolyte according to claim 1 or 2, characterized in that: The carbonate solvent is selected from at least one of fluoroethylene carbonate, vinylene carbonate, vinylethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate and chloroethylene carbonate.
6. The polymer gel electrolyte according to claim 1 or 2, characterized in that: The electrolyte salt is at least one selected from the group consisting of lithium perchlorate, lithium hexafluorophosphate, lithium bis(oxalatoborate), lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethanesulfonyl imide) and lithium bis(fluorosulfonyl imide).
7. The polymer gel electrolyte according to claim 1 or 2, characterized in that: The initiator is aluminum trifluoromethanesulfonate.
8. A method for preparing a polymer gel electrolyte according to any one of claims 1 to 7, characterized in that: The following steps are involved: Adding a first ether monomer capable of ring-opening polymerization and a second cross-linkable acrylate monomer to a carbonate solvent and stirring for 10 to 30 minutes; then adding an electrolyte salt and stirring for 1 to 12 hours to uniformly disperse the electrolyte salt in the solvent; finally adding an initiator and stirring in an ice bath for 5 to 30 minutes to form a uniformly dispersed electrolyte prepolymer precursor solution; The electrolyte prepolymer precursor liquid is injected into the separator between the positive and negative electrodes of the battery in an environment with a protective atmosphere and an oxygen content and a water content both less than 1 ppm, and in-situ polymerized at room temperature to form a polymer gel electrolyte.
9. A lithium metal battery, characterized in that: The lithium metal battery includes a positive electrode sheet, a negative electrode sheet, and a polymer gel electrolyte, wherein the polymer gel electrolyte is formed by in-situ polymerization on a separator between the positive electrode sheet and the negative electrode sheet.
10. The lithium metal battery according to claim 9, characterized in that: The membrane is selected from one of polyethylene, polypropylene, polyacrylonitrile, poly(vinylidene fluoride-hexafluoroethylene), polymethyl methacrylate, polyimide, polyetherimide, cellulose, aramid and non-woven bacterial cellulose membranes.
Citation Information
Cited By
Composite coating modified negative electrode, all-solid-state battery and preparation method of all-solid-state battery
CN119695155A
Lithium battery polymer solid electrolyte membrane capable of rapidly polymerizing at room temperature as well as preparation method and application of lithium battery polymer solid electrolyte membrane
CN120376739A