High-stability gel composite solid electrolyte as well as preparation method and application thereof

By adopting high-stability gel composite solid electrolyte in lithium metal batteries, using diluents and ultra-thin solid electrolyte membrane technology, the problems of side reactions of metal lithium negative electrodes and dendrites are solved, and the Coulomb efficiency and cycle life of the battery are improved. And reduce the cost and polarization risk of electrolyte.

CN119009104APending Publication Date: 2024-11-22XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411383799.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The metal lithium negative electrode in existing lithium-ion batteries has low utilization efficiency and short life due to side reactions and dendrite growth, high cost of high-salt liquid electrolyte and reduced ionic conductivity.

Method used

Using high-stability gel composite solid electrolyte, an ultra-thin solid electrolyte membrane combined with polymer backbone and nano-active inorganic filler is used to combine diluents to reduce lithium salt concentration, reduce side reactions and improve ionic conductivity. The preparation method includes casting The electrolyte membrane was prepared by rolling pressing method and immersed in the diluent to form a high-stability local diluted electrolyte.

Benefits of technology

The Coulomb efficiency and cycle life of lithium metal batteries have been significantly improved, the internal polarization and cost of the battery are reduced, and the safe and reliable operation of the metal lithium negative electrode is achieved. The Coulomb efficiency reaches 99.2%, and the cycle life reaches 1,000 hours.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009104A_ABST
    Figure CN119009104A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electrochemical energy storage, and particularly relates to a high-stability gel composite solid electrolyte as well as a preparation method and application thereof. The gel composite solid electrolyte comprises an electrolyte and a solid electrolyte film, the solid electrolyte film is infiltrated in the electrolyte, the electrolyte comprises an electrolyte matrix and a diluent, the electrolyte matrix comprises a solvent, a lithium salt and an additive, the concentration of the lithium salt is 4-6 mol / L, and the additive is 0.001-30 wt.% of the electrolyte matrix; the solid electrolyte film is prepared by mixing the polymer skeleton and the nano active inorganic filler. According to the invention, the solvation effect of the high-concentration lithium salt is utilized to reduce free side reactions between the solvent and the metal lithium and the electrolyte, so that a stable solid electrolyte membrane is formed on the surface of the metal lithium, the formation of dendritic crystals is inhibited, the battery has better coulombic efficiency and longer cycle life, the thickness of the solid electrolyte is controllable, the internal polarization of the battery is reduced, and the service life of the battery is prolonged. And the safety and the reliability of the battery are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrochemical energy storage, and in particular relates to a high-stability gel composite solid electrolyte and a preparation method and application thereof. Background Art

[0002] With the continuous progress of society, the energy used by humans is also increasing day by day. Efficient energy storage and conversion is the driving force of social progress, and the emergence and use of batteries enable people to use energy more efficiently and conveniently. Compared with other batteries, lithium-ion batteries are favored by various industries due to their high specific energy, small size, maintenance-free, and environmentally friendly. As the actual energy density of lithium-ion batteries (especially graphite negative electrodes) gradually approaches its theoretical limit, more efficient electrode materials are urgently needed to meet the needs of the development of emerging high-end energy storage devices. Lithium metal batteries with lithium metal as the negative electrode, including lithium-sulfur batteries, lithium-oxygen batteries and lithium-oxide batteries, show extremely high theoretical energy density. Therefore, lithium metal batteries with lithium metal as the negative electrode will become the next generation of energy storage batteries.

[0003] Due to the extremely high reactivity of metallic lithium, when conventional lithium-ion battery electrolytes are used, serious side reactions occur between metallic lithium and the electrolyte, causing the active substances to be irreversibly consumed, resulting in low utilization efficiency of metallic lithium negative electrodes, and dendrite growth and volume expansion effects of lithium negative electrodes during the charge and discharge process, which seriously affect the battery utilization and service life during its actual operation, limiting the practical application of metallic lithium. Recently, semi-solid gel electrolytes have been widely accepted by researchers as an effective strategy to achieve stable cycling of metallic lithium negative electrodes. This type of electrolyte combines the mechanical properties of polymer solid electrolytes with the advantages of high ionic conductivity of liquid electrolytes. Among them, high-salt liquid electrolytes exhibit certain ionic liquid properties and other unconventional excellent properties because most of their solvents are solvated by lithium salts and there is little free solvent. High-salt concentration electrolytes have important advantages in inhibiting dendrite growth and improving the Coulombic efficiency and cycle life of batteries. One disadvantage of this type of electrolyte is that it is relatively expensive. Due to the use of more lithium salts, the overall cost of the electrolyte increases. Moreover, as the concentration of salt increases, the viscosity of the electrolyte increases and the ionic conductivity decreases. To this end, the present invention provides a high-stability gel composite solid electrolyte for lithium metal batteries and a preparation method and application thereof. Summary of the invention

[0004] The purpose of the present invention is to provide a high-stability gel composite solid electrolyte and its preparation method and application. The electrolyte has high ionic conductivity and good stability, and the electrolyte is applied to lithium metal batteries to reduce the side reaction between lithium metal and electrolyte, inhibit dendrite growth, and improve the coulombic efficiency and cycle life of the battery.

[0005] The present invention solves the above technical problems through the following technical solutions.

[0006] The first object of the present invention is to provide a high-stability gel composite solid electrolyte, wherein the solid electrolyte comprises an electrolyte and a solid electrolyte film, wherein the solid electrolyte film is immersed in the electrolyte, wherein the electrolyte comprises an electrolyte matrix and a diluent, wherein the electrolyte matrix comprises a solvent, a lithium salt and an additive, wherein the concentration of the lithium salt is 4 to 6 mol / L, and the additive is 0.001 to 30 wt.% of the total mass of the electrolyte matrix; the solid electrolyte film is prepared by mixing a polymer skeleton and a nano-active inorganic filler through casting and rolling.

[0007] Furthermore, the lithium salt is at least one of lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide) and lithium difluorooxalatoborate.

[0008] Furthermore, the diluent is at least one of toluene, o-xylene, m-xylene and p-xylene.

[0009] Furthermore, the additives are lithium nitrate and fluoroethylene carbonate.

[0010] Furthermore, lithium nitrate accounts for 0.001 to 10 wt.% of the total mass of the electrolyte matrix; fluoroethylene carbonate accounts for 0.001 to 20 wt.% of the total mass of the electrolyte matrix.

[0011] Furthermore, the solvent is a mixture of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane, and the molar ratio of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane is 0-1:1:1.

[0012] Furthermore, the preparation method of the solid electrolyte membrane is as follows:

[0013] The polymer skeleton and nano-active inorganic filler are added to solvent B, the electrolyte membrane solution is evenly dispersed by stirring, and a solid electrolyte membrane is prepared by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 20 to 200 μm; the mass ratio of the polymer skeleton and the nano-active inorganic filler is 90:10.

[0014] Furthermore, the polymer skeleton is one or more of vinylidene fluoride, polyethylene oxide, polymethyl methacrylate, and polyacrylonitrile; the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , Li 1.3 Al 0.3 Ge 1.7 (PO 4 ) 3or Li 7 La 3 Zr 2 O 12 ; Solvent B is N,N-dimethylformamide.

[0015] The second object of the present invention is to provide a method for preparing the above-mentioned high-stability gel composite solid electrolyte, comprising the following steps:

[0016] Adding lithium salt and additives to a solvent to obtain an electrolyte matrix; adding a diluent to the electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L, and mixing evenly to obtain an electrolyte; and immersing a solid electrolyte membrane in the electrolyte to obtain a high-stability gel composite solid electrolyte.

[0017] The third object of the present invention is to provide the application of the above-mentioned high-stability gel composite solid electrolyte in lithium batteries.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] (1) The present invention adopts a high-stability gel composite solid electrolyte, which comprises a high-stability local dilution electrolyte and a high-stability ultra-thin polymer-based gel composite solid electrolyte of an ultra-thin solid electrolyte membrane, wherein the high-stability local dilution electrolyte utilizes the solvation effect of high-concentration lithium salts to reduce the free-existing solvent, reduce the side reaction between metal lithium and the electrolyte, form a stable solid electrolyte membrane on the surface of metal lithium, inhibit the formation of dendrites, and utilize toluene, o-xylene, p-xylene, and m-xylene as diluents to improve the ionic conductivity of the high-salt concentration electrolyte and reduce the overall cost of the electrolyte. The diluent used in the present invention is stable in nature, easy to obtain, and inexpensive, and can make the battery have better coulomb efficiency and cycle life. On the other hand, the thickness of the ultra-thin solid electrolyte can be controlled to reduce the internal polarization of the battery and improve the safety and reliability of the battery. The system has significant advantages such as low cost, stable quality of the obtained electrolyte, high coulomb efficiency and cycle life of metal lithium batteries, and is expected to be widely used in commercial secondary battery energy storage systems.

[0020] (2) The present invention also discloses a method for preparing a highly stable localized dilute electrolyte and an ultrathin polymer-based solid electrolyte membrane. The preparation method has a simple process, readily available raw materials, and is easy to industrialize.

[0021] (3) The present invention also discloses the application of a high-stability local dilution high-salt electrolyte in a metal lithium battery. The electrolyte combines a high-salt concentration electrolyte matrix with different diluents, utilizes the fewer side reactions between the high-salt concentration electrolyte and metal lithium, improves the coulombic efficiency and cycle life of the lithium metal battery, utilizes the diluent to improve the ionic conductivity of the electrolyte, and reduces the cost of the electrolyte. The prepared lithium metal battery not only has high coulombic efficiency but also has a long cycle life. The coulombic efficiency of the battery can reach 99.2%, and the cycle life can reach 1000h.

[0022] (4) The present invention also discloses the application of an ultra-thin polymer-based solid electrolyte membrane in a metal lithium battery. The electrolyte membrane combines different polymers and inorganic fillers, and utilizes its relatively high mechanical strength and sufficient ionic conductivity to achieve safe and reliable operation of the metal lithium negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a graph of the interface morphology of the metal lithium negative electrode after cycling of the gel composite solid electrolyte in Example 1 of the present invention.

[0024] Figure 2 This is a graph of the metal lithium negative electrode cycle coulombic efficiency of the gel composite solid electrolyte of Example 1-2 of the present invention, wherein: Figure 2 Herein, a is Example 1, and b is Example 2. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] It should be noted that the professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, the various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0027] On the one hand, the present invention provides a high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and a solid electrolyte film, the solid electrolyte film being immersed in the electrolyte, the electrolyte comprising an electrolyte matrix and a diluent, the electrolyte matrix comprising a solvent, a lithium salt and an additive, the concentration of the lithium salt being 4 to 6 mol / L, and the additive being 0.001 to 30 wt.% of the total mass of the electrolyte matrix; the solid electrolyte film being prepared by mixing a polymer skeleton and a nano-active inorganic filler through casting and rolling.

[0028] The purpose of the present invention is to design an ultra-thin polymer-based gel composite solid electrolyte: a highly stable local dilute electrolyte utilizes the solvation effect of a high-concentration lithium salt to reduce the free-existing solvent, reduce the side reaction between metal lithium and the electrolyte, form a stable solid electrolyte film on the surface of metal lithium, and inhibit the formation of dendrites. By continuously optimizing the electrolyte system and using a diluent to improve the lithium ion conductivity of the high-salt concentration electrolyte system, adapt the ultra-thin polymer-based solid electrolyte, and reduce the cost of the electrolyte, it is of great significance to improve the cycle life and coulomb efficiency of lithium metal batteries and accelerate the practical application of lithium metal batteries. On the other hand, the thickness of the ultra-thin solid electrolyte can be controlled to reduce the internal polarization of the battery and improve the safety and reliability of the battery. The system has significant advantages such as low cost, stable quality of the obtained electrolyte, high coulomb efficiency and cycle life of metal lithium batteries, and is expected to be widely used in commercial secondary battery energy storage systems.

[0029] In a specific embodiment, the lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide and lithium difluorooxalatoborate.

[0030] In a specific embodiment, the diluent is at least one of toluene, o-xylene, m-xylene, and p-xylene. In the present invention, the purpose of the diluent is to improve the ionic conductivity of the high salt concentration electrolyte and reduce the overall cost of the electrolyte. The diluent used is stable in nature, easy to obtain, and low in price, which can make the battery have better coulombic efficiency and cycle life.

[0031] In a specific embodiment, the additive is lithium nitrate and fluoroethylene carbonate. In the present invention, the additive can form an interface film on the surface of the lithium negative electrode that passivates the active surface of the negative electrode and protects the lithium negative electrode, thereby improving the cycle performance of the battery.

[0032] In a specific embodiment, lithium nitrate accounts for 0.001-10 wt.% of the total mass of the electrolyte matrix; when the additive is fluoroethylene carbonate, fluoroethylene carbonate accounts for 0.001-20 wt.% of the total mass of the electrolyte matrix.

[0033] In a specific embodiment, the solvent is a mixture of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane, and the molar ratio of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane is 0-1: 1: 1. In the present invention, the solvent is used to increase the solubility of the lithium salt, and the diethyl carbonate in the solvent has good antioxidant properties and high solubility for lithium salts, and ethylene glycol dimethyl ether and 1,3-dioxolane are stable to the metal lithium negative electrode.

[0034] In a specific embodiment, the preparation method of the solid electrolyte membrane is as follows:

[0035] The polymer skeleton and nano-active inorganic filler are added to solvent B, the electrolyte membrane solution is evenly dispersed by stirring, and a solid electrolyte membrane is prepared by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 20 to 200 μm; the mass ratio of the polymer skeleton and the nano-active inorganic filler is 90:10.

[0036] The electrolyte membrane used in the present invention combines different polymers and inorganic fillers, and uses its relatively high mechanical strength and sufficient ionic conductivity to achieve safe and reliable operation of the metal lithium negative electrode. The thickness of the ultra-thin solid electrolyte can be controlled to reduce the internal polarization of the battery and improve the safety and reliability of the battery. The system has significant advantages such as low cost, stable quality of the obtained electrolyte, high coulombic efficiency and cycle life of metal lithium batteries, and is expected to be widely used in commercial secondary battery energy storage systems.

[0037] In a specific embodiment, the polymer backbone is one or more of vinylidene fluoride, polyethylene oxide, polymethyl methacrylate, and polyacrylonitrile; the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , Li 1.3 Al 0.3 Ge 1.7 (PO 4 ) 3 or Li 7 La 3 Zr 2 O 12 Solvent B is N,N-dimethylformamide. In the present invention, the amount of N,N-dimethylformamide is determined according to the viscosity of the electrolyte membrane solution, and the purpose is to form an electrolyte membrane solution with good castability. In the casting combined with the roller pressing method to prepare the solid electrolyte membrane, therefore, the amount of dimethylformamide is not limited, as long as it can form a good castability.

[0038] On the other hand, the present invention provides a method for preparing the above-mentioned high-stability gel composite solid electrolyte, comprising the following steps:

[0039] Add lithium salt and additives to the solvent to obtain an electrolyte matrix; add a diluent to the electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L, mix evenly to obtain an electrolyte; immerse the solid electrolyte membrane in the electrolyte to obtain a high-stability gel composite solid electrolyte. The preparation method is simple in process, the raw materials are easily available, and it is easy to realize industrialization.

[0040] The present invention also provides the application of the high-stability gel composite solid electrolyte in a lithium battery. The electrolyte combines a high-salt concentration electrolyte matrix with different diluents, utilizes the fewer side reactions between the high-salt concentration electrolyte and metallic lithium, improves the coulomb efficiency and cycle life of the lithium metal battery, utilizes the diluent to improve the ionic conductivity of the electrolyte, and reduces the cost of the electrolyte. The prepared lithium metal battery not only has high coulomb efficiency but also has a long cycle life. The coulomb efficiency of the battery can reach 99.2%, and the cycle life reaches 1000h.

[0041] The invention is further described below through specific examples.

[0042] Example 1

[0043] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, and the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent.

[0044] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), the concentration of LiFSI is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0045] The diluent toluene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0046] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0047] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , and then added into N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity was 5Pa·s, to obtain an electrolyte membrane solution, and an ultra-thin solid electrolyte membrane was prepared by a tape casting combined with a roller pressing method; the thickness of the ultra-thin solid electrolyte membrane was 50μm.

[0048] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0049] S1. Add LiFSI and LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0050] S2. Add diluent toluene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0051] Example 2

[0052] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, and the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent;

[0053] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), the concentration of LiFSI is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0054] The diluent o-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0055] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0056] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the ultra-thin solid electrolyte membrane is 50μm.

[0057] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0058] S1. Add LiFSI and LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0059] S2. Add diluent o-xylene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0060] Example 3

[0061] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent,

[0062] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), the concentration of LiFSI is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0063] The diluent m-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0064] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0065] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the ultra-thin solid electrolyte membrane is 50μm.

[0066] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0067] S1. Add LiFSI and LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0068] S2. Add diluent m-xylene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0069] Example 4

[0070] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent,

[0071] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), the concentration of LiFSI is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0072] The diluent p-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0073] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0074] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the ultra-thin solid electrolyte membrane is 50μm.

[0075] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0076] S1. Add LiFSI and LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0077] S2. Add diluent p-xylene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high-stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high-stability gel composite solid electrolyte.

[0078] Example 5

[0079] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent,

[0080] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI) and lithium difluorooxalatoborate (LiDFOB), the molar ratio of LiFSI and LiDFOB is 1:1, the total concentration of LiFSI and LiDFOB is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0081] The diluent toluene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0082] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0083] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the ultra-thin solid electrolyte membrane is 50μm.

[0084] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0085] S1. Add LiFSI, LiDFOB, LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0086] S2. Add diluent toluene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0087] Example 6

[0088] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent,

[0089] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI) and lithium difluorooxalatoborate (LiDFOB), the molar ratio of LiFSI and LiDFOB is 1:1, the total concentration of LiFSI and LiDFOB is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0090] The diluent o-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0091] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0092] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 50μm.

[0093] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0094] S1. Add LiFSI, LiDFOB, LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0095] S2. Add diluent o-xylene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0096] Example 7

[0097] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent,

[0098] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI) and lithium difluorooxalatoborate (LiDFOB), the molar ratio of LiFSI and LiDFOB is 1:1, the total concentration of LiFSI and LiDFOB is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte matrix, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte matrix.

[0099] The diluent m-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0100] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0101] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3 , then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 50μm.

[0102] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0103] S1. Add LiFSI, LiDFOB, LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0104] S2. Add diluent toluene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high stability gel composite solid electrolyte.

[0105] Example 8

[0106] A high-stability gel composite solid electrolyte, the solid electrolyte comprising an electrolyte and an ultra-thin solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, and the electrolyte comprises a high-salt concentration electrolyte matrix and a diluent;

[0107] The high salt concentration electrolyte matrix includes a solvent formed by mixing 1,3-dioxolane (DOL) and ethylene glycol dimethyl ether (DME) in a molar ratio of 1:1, the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI) and lithium difluorooxalatoborate (LiDFOB), the molar ratio of LiFSI and LiDFOB is 1:1, the total concentration of LiFSI and LiDFOB is 5 mol / L, and the additive is lithium nitrate (LiNO 3 ) and fluoroethylene carbonate (FEC), LiNO 3 It is 3wt.% of the total mass of the high salt concentration electrolyte, and FEC is 10wt.% of the total mass of the high salt concentration electrolyte.

[0108] The diluent p-xylene is added to the high salt concentration electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L.

[0109] The preparation method of the ultra-thin solid electrolyte membrane is as follows:

[0110] The polymer skeleton and the nano-active inorganic filler are mixed in a mass ratio of 90:10, the polymer skeleton is formed by mixing vinylidene fluoride and polyethylene oxide in a mass ratio of 1:1, and the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO 4 ) 3, then added to N,N-dimethylformamide, then added to N,N-dimethylformamide, stirred and dispersed until the overall electrolyte slurry viscosity is 5Pa·s, to obtain an electrolyte membrane solution, and prepared an ultra-thin solid electrolyte membrane by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 50μm.

[0111] The method for preparing the above-mentioned high-stability gel composite solid electrolyte comprises the following steps:

[0112] S1. Add LiFSI, LiDFOB, LiNO to the mixed solvent of DOL and DME. 3 and FEC to obtain a high salt concentration electrolyte matrix;

[0113] S2. Add diluent p-xylene to the high salt concentration electrolyte matrix, mix well, dilute the concentration of lithium salt to 1 mol / L, and obtain a high-stability local diluted electrolyte; immerse the solid electrolyte membrane in the electrolyte for 12 hours to obtain a high-stability gel composite solid electrolyte.

[0114] The gel composite solid electrolyte prepared by the method of the present invention was tested for ion conductivity, the gel electrolyte was applied to a lithium metal negative electrode battery for coulombic efficiency test, and the gel electrolyte was applied to a lithium metal battery for cycle stability test. The test conditions were:

[0115] The prepared gel electrolyte was tested with a conductivity meter to determine the ionic conductivity of the electrolyte. A lithium-copper half-cell was used to test the coulombic efficiency (lithium metal was used for the negative electrode and copper foil was used for the positive electrode). The coulombic efficiency of metallic lithium was calculated using the capacity ratio of lithium deposited and removed on the copper foil. Constant current charging and discharging was used with a voltage range of 0-1V and a current density of 1.0mA / cm 2 , deposition capacity 2.0mAh / cm 2 , and tested the coulombic efficiency of the metal lithium anode using the electrolyte. 0.8 Co 0.1 Mn 0.1 O 2 As the positive electrode, metallic lithium is the negative electrode, the liquid electrolyte is a lithium salt, and the lithium salt is at least one of lithium hexafluorophosphate, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide and lithium difluorooxalate borate. In the present invention, the lithium salt is consistent with the lithium salt used in the electrolyte membrane (gel electrolyte), and the lithium salt concentration of the liquid electrolyte is 1 mol / L. The electrolytes of the above embodiments are respectively used to assemble the test cells according to the conventional battery preparation method. The battery is charged and discharged at a rate of 0.5C in the voltage range of 3-4.9V, and the capacity retention rate. The results of ionic conductivity, coulomb efficiency and capacity retention rate are shown in Table 1.

[0116] Table 1 Gel composite solid electrolyte performance test results

[0117]

[0118]

[0119] As can be seen from Table 1, the coulombic efficiency of metal lithium deposition and extraction in the gel composite solid electrolytes of Examples 1-8 of the present invention is higher than 98%, and the metal lithium full batteries using the electrolyte of the present invention all show excellent cycle stability, and can still show a capacity retention rate of more than 85% after 500 cycles.

[0120] Figure 1 This is a graph showing the interface morphology of the metal lithium negative electrode after cycling of the gel composite solid electrolyte in Example 1 of the present invention. Figure 1 As shown, the electrolyte circulation presents a uniform morphology, reduces the side reaction between metallic lithium and the electrolyte, forms a stable solid electrolyte film on the surface of metallic lithium, inhibits the formation of dendrites, and the resulting electrolyte has stable quality.

[0121] Figure 2 This is a graph of the metal lithium negative electrode cycle coulombic efficiency of the gel composite solid electrolyte of Example 1-2 of the present invention, Figure 2 (a) is Example 1, and (b) is Example 2. Figure 2 As shown, at a current density of 0.5 mA / cm 2 and 1.0mA / cm 2 When the coulombic efficiency of metal lithium deposition and extraction in the gel composite solid electrolyte of Examples 1-2 is 99.5% and 99.2% respectively, the coulombic efficiency of the lithium metal battery is improved.

[0122] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0123] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A high-stability gel composite solid electrolyte, characterized in that: The solid electrolyte includes an electrolyte and a solid electrolyte film, the solid electrolyte film is immersed in the electrolyte, the electrolyte includes an electrolyte matrix and a diluent, the electrolyte matrix includes a solvent, a lithium salt and an additive, the concentration of the lithium salt is 4 to 6 mol / L, and the additive is 0.001 to 30 wt.% of the total mass of the electrolyte matrix; the solid electrolyte film is prepared by mixing a polymer skeleton and a nano-active inorganic filler through casting and rolling.

2. The high-stability gel composite solid electrolyte according to claim 1, characterized in that: The lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide and lithium difluorooxalatoborate.

3. The high-stability gel composite solid electrolyte according to claim 1, characterized in that: The diluent is at least one of toluene, o-xylene, m-xylene and p-xylene.

4. The high-stability gel composite solid electrolyte according to claim 1, characterized in that: The additives are lithium nitrate and fluoroethylene carbonate.

5. The high-stability gel composite solid electrolyte according to claim 4, characterized in that: The lithium nitrate accounts for 0.001 to 10 wt.% of the total mass of the electrolyte matrix; the fluoroethylene carbonate accounts for 0.001 to 20 wt.% of the total mass of the electrolyte matrix.

6. The high-stability gel composite solid electrolyte according to claim 1, characterized in that: The solvent is a mixture of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane, and the molar ratio of diethyl carbonate, ethylene glycol dimethyl ether and 1,3-dioxolane is 0-1:1:

1.

7. The high-stability gel composite solid electrolyte according to claim 1, characterized in that: The preparation method of the solid electrolyte membrane is as follows: The polymer skeleton and nano-active inorganic filler are added to solvent B, the electrolyte membrane solution is evenly dispersed by stirring, and a solid electrolyte membrane is prepared by a casting combined with a roller pressing method; the thickness of the solid electrolyte membrane is 20 to 200 μm; the mass ratio of the polymer skeleton and the nano-active inorganic filler is 90:

10.

8. The high-stability gel composite solid electrolyte according to claim 7, characterized in that: The polymer skeleton is one or more of vinylidene fluoride, polyethylene oxide, polymethyl methacrylate, and polyacrylonitrile; the nano-active inorganic filler is Li 1.3 Al 0.3 Ti 1.7 (PO4)3、Li 1.3 Al 0.3 Ge 1.7 (PO4)3 or Li7La3Zr2O 12 ; Solvent B is N,N-dimethylformamide.

9. A method for preparing a high-stability gel composite solid electrolyte according to any one of claims 1 to 8, characterized in that: The following steps are involved: Adding lithium salt and additives to a solvent to obtain an electrolyte matrix; adding a diluent to the electrolyte matrix to dilute the concentration of the lithium salt to 1 mol / L, and mixing evenly to obtain an electrolyte; and immersing a solid electrolyte membrane in the electrolyte to obtain a high-stability gel composite solid electrolyte.

10. Use of the high-stability gel composite solid electrolyte according to any one of claims 1 to 8 in a lithium battery.