Surface modified aluminum oxide diaphragm as well as preparation method and application thereof
By grafting sulfonic acid groups on the surface of the alumina separator to form a stable SEI film, the problem of the insolidity of the SEI film in lithium metal batteries is solved, and the discharge capacity and life of the battery are improved.
Patent Information
- Application Number
- CN202411126240.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The solid electrolyte interface (SEI) film in lithium metal batteries is not strong enough, resulting in insufficient discharge capacity and short service life of the battery.
By grafting sulfonic acid groups on the surface of the alumina separator, forming a sulfonic acid molecular layer, promoting the decomposition of lithium nitrate in the electrolyte, and generating a stable SEI film rich in Li3N nanocrystals, improving the interface ion conductivity and inhibiting lithium dendrites. Grow.
It significantly improves the deep charging and discharge capacity and cycle life of lithium metal batteries, and achieves uniform and rapid deposition of lithium ions and interface stability.
Smart Images

Figure CN119009373A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery separators, and more specifically to a surface-modified aluminum oxide separator and a preparation method and application thereof. Background Art
[0002] With the development of portable electronic devices and electric vehicles, the demand for energy storage devices has grown rapidly. Lithium metal has a high theoretical capacity (3860 mAh g -1 ), low redox potential (-3.04 V, relative to standard hydrogen electrode) and low density (0.534 g·cm -3 ) characteristics, and is considered an ideal battery negative electrode material. However, the growth of lithium dendrites and the consumption of electrolyte during the cycle seriously affect the capacity and life of lithium metal batteries. Lithium metal reacts with the electrolyte during the battery cycle to form a solid electrolyte interface (SEI) film, which can partially protect the lithium metal. However, due to the volume change of the lithium negative electrode, the SEI film repeatedly ruptures and regenerates, consuming lithium and electrolyte, resulting in a decrease in coulombic efficiency and accelerating the growth of lithium dendrites.
[0003] At present, designing functional diaphragms to solve the above-mentioned interface problems is an efficient and convenient solution that helps control costs and is easy to integrate into existing commercial production lines. A more common modification method is to enhance the mechanical strength of the diaphragm by coating alumina particles on the surface of the polyethylene diaphragm. However, this modification method often results in insufficient discharge capacity of the lithium metal battery because the alumina particles cannot effectively induce the lithium metal anode to form a strong SEI, thereby further shortening the battery life. Summary of the invention
[0004] The present invention provides a surface modified alumina diaphragm and a preparation method and application thereof, which are used to solve the problem in the prior art that SEI in lithium metal batteries is not strong enough, resulting in weak battery discharge capacity and short service life.
[0005] In a first aspect, the present invention provides a surface-modified aluminum oxide membrane, comprising an aluminum oxide membrane and sulfonic acid groups compounded on the surface of the aluminum oxide membrane.
[0006] As a possible implementation manner, the sulfonic acid group is grafted onto the surface of the alumina membrane through ionic bonding with the alumina.
[0007] In a second aspect, the present invention provides a method for preparing a surface-modified alumina diaphragm as described in any possible implementation of the first aspect, comprising the following steps: immersing the alumina diaphragm in a sulfonic acid solution to obtain a crude product; wherein the solvent of the sulfonic acid solution is a polar organic solvent; and washing and drying the crude product in sequence to obtain the surface-modified alumina diaphragm. The sulfonate in the sulfonic acid solution undergoes an ionic bonding reaction with the alumina, and finally the sulfonate molecules are successfully grafted onto the surface of the alumina. The dried diaphragm should be flat and curl-free.
[0008] As a possible implementation method, the soaking conditions are: temperature 25-30°C, time greater than 12h; and / or, the washing includes: washing with deionized water several times and then rinsing with methanol; and / or, the drying conditions are: drying at 50°C.
[0009] The solvent of the sulfonic acid solution should preferably be a highly polar solvent that can dissolve the sulfonic acid molecules and should not have side reactions with the alumina diaphragm. The concentration of the sulfonic acid solution should be a concentration that allows the sulfonic acid molecules to be completely grafted. Too high a concentration may cause the surface of the alumina diaphragm to adsorb too many additional sulfonic acid molecules, increasing the difficulty of subsequent cleaning. Too low a concentration may cause insufficient grafting on the surface of the alumina diaphragm. The appropriate concentration of the sulfonic acid solution can be determined based on the actual situation of the alumina diaphragm, and the present invention does not make specific limitations. For example, the sulfonic acid is 1,2-ethanedisulfonic acid; the polar organic solvent is methanol; and the concentration of the sulfonic acid solution is 5 mg / mL.
[0010] As a possible implementation, the alumina diaphragm is composed of α-alumina and polyethylene and has a single-sided alumina coating.
[0011] In a third aspect, the present invention provides an application of a surface-modified alumina diaphragm described in any possible implementation of the first aspect or a surface-modified alumina diaphragm prepared by the preparation method described in any possible implementation of the second aspect in a lithium metal battery.
[0012] In a fourth aspect, the present invention provides a lithium metal battery, wherein the diaphragm is the surface-modified alumina diaphragm described in any possible implementation of the first aspect or the surface-modified alumina diaphragm prepared by the preparation method described in any possible implementation of the second aspect.
[0013] As a possible implementation, the electrolyte includes a nitrate component.
[0014] The present invention proposes a surface-modified alumina diaphragm, which grafts a sulfonic acid molecule layer onto the oxide surface through ionic bonding between sulfonic acid molecules and metal oxide particles on the diaphragm surface, making the surface highly polar. The high dipole moment of the sulfonic acid group promotes the breaking of the NO bond, catalyzes the decomposition of lithium nitrate in the electrolyte, and generates a stable SEI film rich in Li3N nanocrystals; the SEI film significantly improves the interfacial ion conductivity and effectively inhibits the growth of lithium dendrites, thereby achieving a long life cycle of lithium metal batteries.
[0015] The invention provides a method for preparing a surface-modified aluminum oxide diaphragm, which has low raw material acquisition cost and a simple and efficient preparation process.
[0016] When a surface-modified alumina diaphragm provided by the present invention is applied to a lithium metal battery, on the one hand, under the influence of a uniform sulfonate molecular layer, the lithium deposition form in the lithium metal battery is spherical, and no dendrite-shaped lithium metal is generated; on the other hand, when encountering an electrolyte to which a salt containing a NO bond is added, the sulfonate radical has a catalytic effect on NO, effectively improving its decomposition efficiency and depth, and being able to quickly produce a large amount of lithium nitride nanocrystals at the lithium metal anode interface to protect the interface, and finally realizing the sulfonic acid molecular layer catalyzing the salt containing NO in the electrolyte to form a stable SEI film rich in Li3N, and under the influence of highly conductive and highly stable Li3N nanocrystals, uniform and rapid deposition of lithium ions can be achieved. Experimental results show that compared with ordinary diaphragms, the diaphragm of the present invention can effectively improve the deep charge and discharge capacity of lithium metal batteries and extend the battery cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0018] Figure 1 This is an XRD diagram of the surface of the diaphragm II provided in an embodiment of the present invention.
[0019] Figure 2 SEM images of diaphragm I, diaphragm II and diaphragm III provided in the embodiments of the present invention, wherein from left to right are the results of diaphragm I, diaphragm II and diaphragm III respectively.
[0020] Figure 3 Infrared spectra of membranes I, II and III provided in the embodiments of the present invention, wherein -PP represents the result of membrane I, -AL2O3 represents the result of membrane II, and -AL2O3-EDA represents the result of membrane III.
[0021] Figure 4 This is a diagram of the contact angle measurement results of membrane I, membrane II and membrane III provided in an embodiment of the present invention, wherein from left to right are the results of membrane I, membrane II and membrane III respectively.
[0022] Figure 5 2mA·cm provided in the embodiment of the present invention -2 Coulomb efficiency test results at current density.
[0023] Figure 6 5mA·cm provided in the embodiment of the present invention -2 Voltage-time behavior at current density of .
[0024] Figure 7 The cycle performance curve at a current density of 1C provided by an embodiment of the present invention.
[0025] Figure 8 This is a diagram of the working mechanism of the diaphragm III provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] In order to solve the problems of weak discharge capacity and short battery life of lithium metal batteries in the prior art, an embodiment of the present invention provides a surface-modified aluminum oxide diaphragm and a preparation method and application thereof.
[0028] The embodiment of the present invention provides a preparation experiment of a surface-modified aluminum oxide membrane and a common aluminum oxide membrane, and performs structural observation and analysis experiments on them, which verifies that the surface-modified aluminum oxide membrane provided by the present invention has more excellent structure and physical properties.
[0029] Furthermore, the present invention has conducted comparative test experiments on electrochemical performance, which verified that the surface-modified alumina separator provided by the present invention has better coulombic efficiency, cycle performance, interface stability, and higher capacity retention rate and cycle stability.
[0030] The technical solution of the present invention will be further described below in conjunction with specific embodiments.
[0031] Example 1
[0032] This embodiment provides a preparation experiment of a polyethylene diaphragm.
[0033] The polyethylene membrane (16 μm polypropylene) was cut into a button battery membrane with a diameter of 20 mm, immersed in 20 mL of anhydrous methanol, soaked at 30°C for 12 h, taken out, washed several times with deionized water and anhydrous methanol respectively, and placed in a forced air drying oven at 40°C to dry, thereby obtaining membrane I.
[0034] Example 2
[0035] This embodiment provides an experiment for preparing an aluminum oxide diaphragm.
[0036] The α-alumina particles, PVDF binder particles and NMP solvent were mixed evenly and stirred in a mass ratio of 9:1:10. After the PVDF was dissolved, the mixture was coated on a 16 μm thick polypropylene diaphragm with a thickness of 4 μm. After drying in an environment of 40°C, it was taken out and cut into button battery diaphragms with a diameter of 20 mm. The membranes were immersed in 20 mL of anhydrous methanol, soaked at 30°C for 12 h, taken out, washed several times with deionized water and anhydrous methanol respectively, and dried in a forced air drying oven at 40°C to obtain diaphragm II.
[0037] Example 3
[0038] This embodiment provides a preparation experiment of a surface-modified aluminum oxide diaphragm.
[0039] The alumina diaphragm (16 μm polypropylene + 4 μm alumina) was cut into a button battery diaphragm with a diameter of 20 mm, immersed in 20 mL of a 5 mg / mL methanol solution of 1,2-ethanedisulfonic acid, soaked at 30°C for 12 h, taken out, washed several times with deionized water and anhydrous methanol, and dried in a forced air drying oven at 40°C to obtain diaphragm III.
[0040] Experimental Example 1
[0041] This experimental example provides a diaphragm structure observation and analysis experiment.
[0042] The surface of the diaphragm II prepared in Example 2 was analyzed by X-ray diffraction, and the following results were obtained: Figure 1 The XRD pattern shown in Figure 1 It can be seen that the surface of diaphragm II is aluminum oxide.
[0043] Scanning electron microscope analysis was performed on the diaphragms I, II and III prepared in Example 1, Example 2 and Example 3, respectively, and the following results were obtained: Figure 2 The SEM picture shown. Figure 2 It can be seen that there is no obvious change in the alumina particles before and after self-installation, and the structural morphology remains intact.
[0044] The infrared spectrum of membranes I to III was analyzed respectively, and the following results were obtained: Figure 3 The infrared spectrum shown in Figure 1 is Figure 3 It can be seen that 1032cm -1 There is S=O asymmetric stretching vibration at 1122-1245cm -1 The symmetric stretching vibration of SO2 in the range indicated the successful self-assembly of 1,2-ethanedisulfonic acid on the surface of alumina particles.
[0045] The contact angles of membranes I, II and III were measured respectively, and the results were as follows: Figure 4 The results shown. Figure 4 It can be seen that after coating the hydrophilic alumina particles on the surface of the PP diaphragm, the interfacial wettability is significantly enhanced, and the significant increase in the contact angle of the interface after self-assembly further confirms the successful construction of the self-assembled monolayer.
[0046] Experimental Example 2
[0047] This experimental example provides a test experiment for the electrochemical performance of the diaphragm.
[0048] Assembly and testing of Li / Cu half-cell: Soak the cut copper foil in dilute hydrochloric acid for 3 minutes to remove excess impurities, then wash the copper foil with deionized water and anhydrous ethanol in turn and put it in a forced air drying oven to dry. The dried copper foil is used as the current collector, and DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives is used as the electrolyte. The diaphragm to be tested is used as the diaphragm. The Li / Cu half-cell to be tested is assembled in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). The Xinwei battery test system is used to test the Li / Cu half-cell at a voltage of 0.1-1V at 0.03mA·cm -2 Electrochemical activation was performed at a current density of 2 mA cm -2 A constant current charge and discharge test was carried out with a current density of , and the coulombic efficiency was calculated based on the amount of lithium metal deposited and stripped.
[0049] Assembly and testing of Li / Li symmetric cells: Both electrodes are clean Li foils, and the other components and operating steps are the same as those of Li / Cu half-cells to obtain the Li / Li symmetric cell to be tested. -2 ; 5mAh·cm -2 The (polarization) overpotential is measured by constant current charge and discharge, and the stability of the battery interface is measured by comparing the overpotential.
[0050] Assembly and testing of Li / LiFePO4 full battery: LiFePO4 powder, acetylene black, PVDF and NMP were uniformly mixed in a mass ratio of 9:0.6:0.4:50 to form a slurry. The slurry was evenly coated on the surface of aluminum foil using an applicator, and dried in a vacuum oven at 60°C. Finally, it was pressed under a pressure of 15Mpa to obtain a LiFePO4 positive electrode sheet. DOL / DME (1:1w / w) with 1M LiTFSI and 1wt% LiNO3 as additives was used as the electrolyte, and the diaphragm to be tested was used as the diaphragm. The Li / LiFePO4 full battery to be tested was assembled in an argon glove box (H2O < 0.01ppm, O2 < 0.01ppm). After activating and cycling for 3 cycles at a charge and discharge rate of 0.2C, a charge and discharge test at a rate of 1C was performed. The charge and discharge voltage range was 2.5-3.8V, and its capacity retention rate was tested.
[0051] In this experimental example, the membranes I, II and III prepared in Examples 1 to 3 were used as the tested membranes, and the coulombic efficiency of the Li / Cu half-cells assembled therefrom was tested. Figure 5 2mA·cm shown -2 Coulombic efficiency at a current density of , where Li / Cu represents the result of separator I, Li / Al2O3 / Cu represents the result of separator II, and Li / AL2O3-EDA / Cu represents the result of separator III. Figure 5 It can be seen that compared with the alumina separator not modified by the molecular layer, the lithium metal battery using the alumina separator modified by sulfonic acid molecules has a higher conductivity at 2 mA cm -2 It has higher coulombic efficiency and better cycle performance at a current density of 2.
[0052] In this experimental example, the membranes I, II and III prepared in Examples 1 to 3 were used as the tested membranes, and the interface stability of the Li / Li symmetric battery assembled therefrom was tested. The results are as follows: Figure 6 5mA·cm shown -2 The voltage-time situation under the current density of , where Li / Li represents the result of separator I, Li / Al2O3 / Li represents the result of separator II, and Li / AL2O3-EDA / Li represents the result of separator III. Figure 6 It can be seen that the diaphragm III is at 5 mA·cm -2 At current densities of , the constructed SEI is more stable and has better interface stability.
[0053] In this experimental example, the diaphragms I, II and III prepared in Examples 1 to 3 were used as the diaphragms to be tested, and the capacity retention rate of the Li / LiFePO4 full battery assembled therefrom was tested. The results are as follows: Figure 7 The cycling performance curve at a current density of 1C is shown in FIG. Figure 7It can be seen that the Li / LiFePO4 full battery using separator III has higher capacity retention and cycle stability.
[0054] This experimental example provides Figure 8 The working mechanism diagram of diaphragm III is shown in the figure. Figure 8 It can be seen that the densely arranged long-range ordered sulfonic acid group molecular layer on the alumina coating membrane provides a strong dipole moment, which can effectively promote the rapid and deep decomposition of LiNO3, thereby forming a SEI rich in Li3N nanocrystals. Under the influence of highly lithium-conductive and highly stable Li3N nanocrystals, the uniform and rapid deposition of lithium ions can be achieved, thereby effectively improving the deep charge and discharge capabilities of the battery and extending the battery cycle life.
[0055] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0056] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A surface-modified alumina diaphragm, characterized in that: The invention comprises an aluminum oxide membrane and a sulfonic acid group compounded on the surface of the aluminum oxide membrane.
2. The surface-modified alumina diaphragm according to claim 1, characterized in that: The sulfonic acid group is grafted onto the surface of the aluminum oxide membrane through ionic bonding with the aluminum oxide.
3. A method for preparing a surface-modified alumina diaphragm according to any one of claims 1 to 2, characterized in that: The following steps are involved: The alumina diaphragm is immersed in a sulfonic acid solution to obtain a crude product; wherein the solvent of the sulfonic acid solution is a polar organic solvent; The crude product is sequentially washed and dried to obtain the surface-modified alumina diaphragm.
4. The preparation method according to claim 3, characterized in that: The soaking conditions are: temperature 25-30°C, duration greater than 12h; And / or, the washing comprises: washing with deionized water for several times and then rinsing with methanol; And / or, the drying condition is: drying at 50°C.
5. The preparation method according to claim 3, characterized in that: The sulfonic acid is 1,2-ethanedisulfonic acid; And / or, the polar organic solvent is methanol; And / or, the concentration of the sulfonic acid solution is 5 mg / mL.
6. The preparation method according to claim 3, characterized in that: The alumina diaphragm is composed of α-alumina and polyethylene and has a single-sided alumina coating.
7. Use of the surface-modified alumina diaphragm according to any one of claims 1 to 2 or the surface-modified alumina diaphragm prepared by the preparation method according to any one of claims 3 to 6 in lithium metal batteries.
8. A lithium metal battery, characterized in that: The diaphragm is the surface-modified aluminum oxide diaphragm described in any one of claims 1 to 2 or the surface-modified aluminum oxide diaphragm prepared by the preparation method described in any one of claims 3 to 6.
9. The lithium metal battery according to claim 8, characterized in that Its electrolyte includes the component nitrate.
Citation Information
Patent Citations
Self-assembled monomolecular layer modified aluminum oxide diaphragm and preparation and application thereof
CN112133867A
Diaphragm slurry, battery diaphragm, preparation method and lithium battery
CN115579583A
Cited By
Preparation method of sulfo-functionalized boehmite and coating diaphragm of sulfo-functionalized boehmite
CN122326028A