Double-sided perovskite solar cell based on multilayer structure transparent electrode and preparation method of double-sided perovskite solar cell

By using multi-layer structure transparent electrodes in double-sided perovskite solar cells, the problem of large resistance under low temperature conditions is solved, the photoelectric conversion efficiency and stability of perovskite solar cells are improved, and efficient photovoltaic power generation efficiency is achieved.

CN119012722AActive Publication Date: 2024-11-22GUANGZHOU INST OF ENERGY CONVERSION CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310561407.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-17
Publication Date
2024-11-22
Estimated Expiration
2043-05-17

AI Technical Summary

Technical Problem

The existing double-sided perovskite solar cells have a problem of large resistance in the preparation of transparent thin film electrodes under low temperature conditions, especially in the production of large-area solar cells, which affects the series resistance and performance of the battery.

Method used

A multi-layer structure transparent electrode is adopted, including a transparent conductive layer, an electron transport layer, a perovskite structure photoactive layer, a hole transport layer, a buffer layer and a transparent top electrode. The transparent top electrode structure is a metal ion doped oxide layer/organic Small molecule modification layer/ultra-thin metal layer/metal ion-doped oxide layer is prepared by ultraviolet ozone treatment, magnetron sputtering and other processes to optimize the thickness of the metal ion-doped oxide layer and the use of organic small molecule modification layer. To improve the conductivity and transmittance of the electrode.

Benefits of technology

The photoelectric conversion efficiency of perovskite solar cells is significantly improved, the photoelectric conversion efficiency under single-sided light reaches 20.3%, and the double-sided equivalent conversion efficiency reaches 26.5%, and the battery stability and transparent electrode performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012722A_ABST
    Figure CN119012722A_ABST
Patent Text Reader

Abstract

The invention discloses a double-sided perovskite solar cell based on a multilayer structure transparent electrode and a preparation method of the double-sided perovskite solar cell. The perovskite solar cell is sequentially composed of a transparent conductive layer, an electron transport layer, a perovskite structure optical active layer, a hole transport layer, a buffer layer and a transparent top electrode from bottom to top, and the transparent top electrode structurally comprises a metal ion doped oxide I layer, an organic small molecule modification layer, an ultrathin metal layer and a metal ion doped oxide I layer. And a metal ion doped oxide I layer is arranged at the top of the buffer layer. The multi-layer structure transparent top electrode obtained by the invention has excellent conductivity and transmittance, the photoelectric conversion efficiency of the perovskite solar cell can be greatly improved, the perovskite cell can absorb sunlight from two sides due to the high transmittance of the transparent electrode, the photoelectric conversion efficiency is further improved, and the photoelectric conversion efficiency of the perovskite solar cell is improved. The method has positive significance in further improvement of photovoltaic power generation efficiency and research and development of photovoltaic building integration in the future.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solar cells, and in particular to a double-sided perovskite solar cell based on a multi-layer structure transparent electrode and a preparation method thereof. Background Art

[0002] Double-sided perovskite solar cells not only have the advantages of simple process, low production cost, flexible and portable devices, and high photoelectric conversion efficiency, but also have the characteristics of double-sided light absorption, which further improves the photoelectric conversion efficiency and has attracted widespread attention from researchers around the world. In addition, many domestic companies have begun to develop and prepare double-sided perovskite solar cells, which has become an important direction for the development of the photovoltaic field. The transparent electrode of double-sided perovskite solar cells must have both high conductivity and high transmittance, so that it can collect light on both sides without affecting the performance of the cell. The most commonly used transparent thin film electrodes such as ITO, FTO, AZO, etc. have the problem of high resistance under low temperature conditions, resulting in large series resistance of solar cells, especially when preparing large-area solar cells. Summary of the invention

[0003] The purpose of the present invention is to provide a double-sided perovskite solar cell based on a multi-layer structure transparent electrode and a preparation method thereof. The present invention can greatly improve the photoelectric conversion efficiency of the perovskite solar cell by virtue of the transparent top electrode multi-layer structure having excellent conductivity and transmittance. The high transmittance of the transparent electrode enables the perovskite cell to absorb sunlight on both sides, further improving the photoelectric conversion efficiency, which has positive significance for further improving the research and development of photovoltaic power generation efficiency and photovoltaic building integration in the future.

[0004] The present invention is achieved through the following technical solutions:

[0005] A double-sided perovskite solar cell based on a multi-layer transparent electrode structure is composed of a transparent conductive layer, an electron transport layer, a perovskite structure photoactive layer, a hole transport layer, a buffer layer and a transparent top electrode from bottom to top. The transparent top electrode structure is a metal ion-doped oxide I layer / organic small molecule modification layer / ultra-thin metal layer / metal ion-doped oxide Ⅰ layer, and a metal ion-doped oxide Ⅰ layer is arranged on the top of the buffer layer.

[0006] Preferably, the organic small molecule modification layer material is an organic small molecule that produces coordination effects with metal ions.

[0007] More preferably, the organic small molecule modification layer material is selected from one or two of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, 6,6'-dicyano-2,2'-bipyridine and 1,10-phenanthroline-4,7-dicarboxylic acid.

[0008] Preferably, in the metal ion-doped oxide I layer / organic small molecule modification layer / ultra-thin metal layer / metal ion-doped oxide Ⅰ layer structure, the thickness of the metal ion-doped oxide Ⅰ layer is 40-60 nm, and the thickness of the metal ion-doped oxide Ⅰ layer is 50-60 nm.

[0009] Preferably, the buffer layer is a metal oxide layer, and the metal oxide is MoO3 or NiO x , the thickness of the buffer layer is 10-30nm.

[0010] The thickness of the electron transport layer is 25-35 nm, the thickness of the organic-inorganic perovskite structure photoactive layer is 640-660 nm, and the thickness of the hole transport layer is 70-90 nm.

[0011] Preferably, in the structure of metal ion-doped oxide layer I / organic small molecule modified layer / ultra-thin metal layer / metal ion-doped oxide layer Ⅰ, the metal material of the ultra-thin metal layer is selected from one of silver, aluminum, gold and copper, and the metal ion-doped oxide in the metal ion-doped oxide layer I or the metal ion-doped oxide layer Ⅰ is selected from one of indium-doped tin oxide, aluminum-doped zinc oxide and indium-doped zinc oxide.

[0012] The transparent conductive layer is glass or flexible plastic, the material of the transparent conductive layer is fluorine-doped tin oxide (FTO) or indium-doped tin oxide (ITO), and the material of the perovskite structure photoactive layer can be selected from MAPbI3, FAPbI3, MAPbBr3, FAPbBr3 or (FAPbI3) 0.95 (MAPbBr) 0.05 One of, but not limited to these materials; the material of the hole transport layer is selected from one of polythiophene, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, CuSCN, WO3 and MoO3, but not limited to these materials.

[0013] The thickness of the metal ion doped oxide layer I / metal ion doped oxide layer Ⅰ of the metal ion doped oxide layer I / organic small molecule modified layer / ultra-thin metal layer / metal ion doped oxide layer Ⅰ is adjustable, and the transmittance of the multi-layer structure transparent electrode changes with the thickness of the metal ion doped oxide layer. The thickness of the organic small molecule modified layer is 3-5nm, and the thickness of the ultra-thin metal layer is 8-10nm.

[0014] The present invention also protects a method for preparing the above-mentioned double-sided perovskite solar cell based on a multi-layer structure transparent electrode, comprising the following steps:

[0015] (1) treating the pretreated transparent conductive layer with ultraviolet ozone;

[0016] (2) preparing a tin oxide nanofilm on the surface of the transparent conductive layer after the ultraviolet ozone treatment in step (1) to obtain a nano tin oxide electron transport layer;

[0017] (3) preparing a perovskite structure photoactive layer on the nano-tin oxide electron transport layer obtained in step (2);

[0018] (4) preparing a hole transport layer on the perovskite structure photoactive layer obtained in step (3);

[0019] (5) depositing a buffer layer on the hole transport layer obtained in step (4) by thermal evaporation;

[0020] (6) preparing a metal ion-doped oxide layer I from the buffer layer obtained in step (5) by a magnetron sputtering method, preparing an organic small molecule modification layer on the metal ion-doped oxide layer I by a spin coating process, and then preparing an ultrathin metal layer and a metal ion-doped oxide layer Ⅰ by a magnetron sputtering method on the organic small molecule modification layer.

[0021] Preferably, step (6) is prepared by the following steps:

[0022] a. Preparation of metal ion-doped oxide layer I: using metal ion-doped oxide target material, substrate temperature is room temperature, sputtering pressure is controlled at 0.2-0.3 Pa, sputtering power is 40-60 W, sputtering time is 10-15 minutes, and metal ion-doped oxide layer I is prepared on the buffer layer obtained in step (5);

[0023] b. Preparation of an organic small molecule modification layer: a 0.1-0.5 mg / mL organic small molecule solution is spin-coated on the metal ion-doped oxide I layer at a rotation speed of 3000-4000 rpm;

[0024] c. Preparation of ultra-thin metal layer: using metal target material, sputtering pressure controlled at 0.2-0.3Pa, sputtering power at 20-30W, sputtering time at 1-2 minutes, to prepare ultra-thin metal layer on the organic small molecule modified layer;

[0025] d. Preparation of metal ion-doped oxide layer ⅠⅠ: metal ion-doped oxide target material is used, the substrate temperature is room temperature, the sputtering pressure is controlled at 0.2-0.3Pa, the sputtering power is 40-60W, the sputtering time is 10-15 minutes, and the metal ion-doped oxide layer ⅠⅠ is prepared on the ultra-thin metal layer.

[0026] Further preferably, the metal ion-doped oxide target in step a or d is selected from one of indium-doped tin oxide, aluminum-doped zinc oxide and indium-doped zinc oxide, and the metal target in step c is selected from one of silver, aluminum, gold and copper.

[0027] Preferably, step (5) adopts thermal evaporation method with a vacuum degree of 2×10 -4 -4×10 -4 Pa, the evaporation rate is

[0028] The present invention also protects the application of the double-sided perovskite solar cell based on the multi-layer structure transparent electrode in photovoltaic building integration. The double-sided perovskite solar cell is made into a double-sided solar cell panel, and the double-sided solar cell panel is integrated into the appearance of the building, capturing incident sunlight on the front side and absorbing indoor light and reflected light on the back side, thereby realizing photovoltaic building integration.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The use of an organic small molecule modification layer can inhibit the isolated island growth of metal at a low thickness threshold, forming an ultra-thin and continuous metal film, and obtaining an ultra-thin metal with excellent conductive properties, so that the metal ion-doped oxide / organic small molecule modification layer / ultra-thin metal layer / metal ion-doped oxide transparent electrode has a low surface square resistance.

[0031] 2. Using the structure of metal ion-doped oxide / metal / metal ion-doped oxide and the anti-reflection effect of the metal ion-doped oxide layer, the transmittance of the metal ion-doped oxide / organic small molecule modification layer / ultra-thin metal layer / metal ion-doped oxide transparent electrode can be improved, and direct contact between the metal electrode and the battery can be avoided, thereby improving the stability of the perovskite solar cell.

[0032] 3. The multi-layer transparent top electrode obtained by the present invention has excellent conductivity and transmittance, which can greatly improve the photoelectric conversion efficiency of perovskite solar cells. The photoelectric conversion efficiency under single-sided illumination reaches 20.3%. When the bottom is illuminated single-sidedly and the top is given 0.2 and 0.5 unit light intensity, the double-sided equivalent conversion efficiency of the double-sided perovskite solar cell reaches 23.3% and 26.5% respectively, which is the highest among the single-section double-sided perovskite solar cells reported so far. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic structural diagram of a double-sided perovskite solar cell of the present invention;

[0034] Figure 2 This is a scanning electron microscope image of a continuous ultra-thin metal formed after using an organic small molecule modification layer in Example 1;

[0035] Figure 3 This is a scanning electron microscope image of a discontinuous ultra-thin metal without an organic small molecule modification layer for comparative example 3;

[0036] Figure 4 The solar cells prepared in Example 1 and Comparative Examples 1 and 2 of the present invention are subjected to a light source of a solar simulator (standard light source) with a light intensity of 100 mW / cm 2 The JV curve below, where J is the photocurrent density and V is the photovoltage;

[0037] Figure 5 The solar cell prepared in Example 1 of the present invention has a front light intensity of 100 mW / cm 2 Under irradiation, the light intensity given to the back of the battery is 20mW / cm 2 and 50mW / cm 2 JV curve under light intensity of, where J is the photocurrent density and V is the photovoltage;

[0038] Explanation of the accompanying drawings: 1. Transparent conductive layer; 2. Nano-tin oxide electron transport layer; 3. Perovskite structure photoactive layer; 4. Hole transport layer; 5. Buffer layer; 6. Transparent top electrode; 6-1. Metal ion-doped oxide layer I; 6-2. Organic small molecule modification layer / ultra-thin metal layer; 6-3. Metal ion-doped oxide layer Ⅰ. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below with reference to the examples. These examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples where specific conditions are not specified are generally based on conventional conditions in the art or conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are considered to be raw materials and reagents that can be obtained through commercial channels such as conventional markets.

[0040] like Figure 1 As shown, a double-sided perovskite solar cell based on a multi-layer transparent electrode is composed of a transparent conductive layer 1, an electron transport layer, a perovskite structure photoactive layer 3, a hole transport layer 4, a buffer layer 5 and a transparent top electrode 6 from bottom to top. The structure of the transparent top electrode 6 is specifically metal ion doped oxide layer I / organic small molecule modification layer / ultra-thin metal layer / metal ion doped oxide layer Ⅰ, a metal ion doped oxide layer Ⅰ 6-1 is arranged on the top of the buffer layer 5, and an organic small molecule modification layer / ultra-thin metal layer 6-2 and a metal ion doped oxide layer Ⅰ 6-3 are arranged on the top of the metal ion doped oxide layer Ⅰ 6-1.

[0041] In the following embodiments, the preferred electron transport layer is preferably a nano-tin oxide electron transport layer 2 .

[0042] In the following embodiments, the transparent conductive layer 1 is preferably glass or flexible plastic, the material of the transparent conductive layer 1 is fluorine-doped tin oxide (FTO) or indium-doped tin oxide (ITO), and the material of the perovskite structure photoactive layer 3 is selected from MAPbI3, FAPbI3, MAPbBr3, FAPbBr3 or (FAPbI3) 0.95 (MAPbBr) 0.05 One of the following; the material of the hole transport layer 4 is selected from one of polythiophene, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, CuSCN, WO3 and MoO3.

[0043] In the following embodiments, preferably, the thickness of the nano-tin oxide electron transport layer 2 is 25-35nm, the thickness of the perovskite structure photoactive layer 3 is 640-660nm, and the thickness of the hole transport layer 4 is 70-90nm. The thickness of the buffer layer 5 is 10-30nm, and in the transparent top electrode 6 metal ion doped oxide I layer / organic small molecule modification layer / ultra-thin metal layer / metal ion doped oxide Ⅰ layer structure, the thickness of the metal ion doped oxide Ⅰ layer 6-1 is 40-60nm, the thickness of the metal ion doped oxide Ⅰ layer 6-3 is 50-60nm, the thickness of the organic small molecule modification layer is 3-5nm, and the thickness of the ultra-thin metal layer is 8-10nm.

[0044] Example 1

[0045] A method for preparing a double-sided perovskite solar cell based on a multi-layer structure transparent electrode comprises the following steps:

[0046] (1) Ultrasonic cleaning of FTO glass was performed for 20 minutes with deionized water, anhydrous ethanol, and isopropanol, respectively, and then dried with high-purity nitrogen;

[0047] (2) treating the cleaned FTO glass sheet with UV ozone to improve the wettability of the FTO surface and increase the work function of the transparent conductive film;

[0048] (3) Spin coating a layer of tin oxide nanocrystalline film on the surface of FTO as an electron transport layer, the thickness of the electron transport layer is 30 nm, the concentration of the nano tin oxide solution is 15%, the spin coating speed is 3000 rpm, and heat treatment is performed at 150° C. for 30 minutes;

[0049] (4) Spin-coat a layer of (FAPbI3) on the tin oxide nanocrystalline film 0.95 (MAPbBr) 0.05The perovskite active layer, with a thickness of 650 nm, was prepared by dissolving a 1.4 M mixture of metal lead salts and organic cations (with additional additions of 0.5 M MACl and 0.13 M PbI2) in a solvent combination of DMF:DMSO (4:1 by volume). The precursor solution was stirred for one hour at 3000 rpm before use.

[0050] (5) dynamically spin-coating ethyl acetate antisolvent on the perovskite film at a rotation speed of 4000 rpm and performing a heat treatment at 100° C. for 60 minutes;

[0051] (6) spin coating a layer of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene as a hole transport layer material on the perovskite film, with a thickness of 80 nm and a spin coating speed of 4000 rpm, wherein the hole transport layer material solution is 72.3 mg of 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 28.8 μL of tert-butylpyridine, and 17.5 μL of acetonitrile solution containing 520 mg / mL bis(trifluoromethanesulfonylimide) lithium in 1 mL of chlorobenzene;

[0052] (7) depositing a layer of MoO3 on the hole transport layer with a thickness of 20 nm;

[0053] (8) sputtering an ITO metal ion-doped oxide layer on the MoO3 by a magnetron sputtering method, with a vacuum degree of 0.3 Pa, 70 sccm of Ar gas, and a sputtering power of 60 W; by controlling the deposition time, the thickness of the ITO metal ion-doped oxide layer I is 40 nm;

[0054] (9) Spin coating an organic small molecule layer on ITO with a thickness of 4 nm, using a BCP solution with a concentration of 0.5 mg / mL, the solvent is isopropanol, and the rotation speed is 3500 rpm;

[0055] (10) depositing a continuous ultra-thin silver layer with a thickness of 9 nm on the organic small molecule layer by magnetron sputtering, with a vacuum degree of 0.3 Pa, 60 sccm of Ar gas, and a sputtering power of 20 W;

[0056] (11) A top ITO layer was deposited on the ultra-thin silver layer by a magnetron sputtering method with a vacuum degree of 0.3 Pa, 70 sccm of Ar gas, and a sputtering power of 60 W, so that the thickness of the ITO metal ion-doped oxide ⅠⅠ layer was 55 nm, thereby obtaining a double-sided perovskite solar cell.

[0057] The double-sided perovskite solar cell based on multilayer transparent electrode prepared by the above method achieved an optimal power conversion efficiency of 20.3% under the condition of single-sided illumination at the bottom. When the single-sided illumination at the bottom was given 0.2 units of illumination intensity at the top, the double-sided equivalent conversion efficiency of the double-sided perovskite solar cell reached 23.3%. When the single-sided illumination at the bottom was given 0.5 units of illumination intensity at the top, the double-sided equivalent conversion efficiency of the double-sided perovskite solar cell reached 26.5%. The JV curves of the double-sided perovskite solar cell under different albedo are shown in Figure 1. Figure 5 shown.

[0058] Comparative Example 1

[0059] Same as Example 1, except that:

[0060] A pure ITO transparent electrode with a thickness of 300 nm was prepared on the buffer layer by magnetron sputtering. The efficiency of the perovskite solar cell based on this top electrode is 16.7%. The JV curve of the perovskite solar cell with ITO electrode is shown in Figure 2. Figure 4 The device’s J SC 22.41 mA cm -2 , V OC It is 1.09V, FF is 69.1%, and PCE is 16.8%.

[0061] Comparative Example 2

[0062] Same as Example 1, except that:

[0063] The Au electrode is directly deposited on the hole transport layer with a thickness of 70 nm. The efficiency of the perovskite solar cell based on this top electrode is 20.4%. The JV curve of the perovskite solar cell with Au electrode is shown in Figure 4 The device’s J SC 24.72 mA cm -2 , V OC It is 1.109V, FF is 75.6%, and PCE is 20.7%.

[0064] Comparative Example 3

[0065] Same as Example 1, except that:

[0066] Without using BCP organic small molecule layer, ITO / Ag / ITO electrode was prepared on the buffer layer by magnetron sputtering. The surface scanning electron microscope image is as follows Figure 3 As shown, compared with the ITO / BCP-Ag / ITO electrode in Example 1, the Ag layer in the electrode without using BCP organic small molecules is discontinuous, the surface resistance is larger, and the transmittance is lower.

[0067] Example 2

[0068] Same as Example 1, except that:

[0069] The material of the buffer layer is NiO. x The perovskite solar cell prepared by this method has an efficiency of 16.2%.

[0070] Example 3

[0071] Same as Example 1, except that:

[0072] The thickness of the buffer layer is 10 nm. The efficiency of the perovskite solar cell prepared by this method is 15.3%.

[0073] Example 4

[0074] Same as Example 1, except that:

[0075] The thickness of the buffer layer is 30nm. The efficiency of the perovskite solar cell prepared by this method is 19.5%.

[0076] Example 5

[0077] Same as Example 1, except that:

[0078] The organic small molecule modified layer material is DCP. The efficiency of the perovskite solar cell prepared by this method is 18.2%.

[0079] Example 6

[0080] Same as Example 1, except that:

[0081] The organic small molecule modified layer material is PDC. The efficiency of the perovskite solar cell prepared by this method is 18.6%.

[0082] Example 7

[0083] Same as Example 1, except that:

[0084] The thickness of the metal ion doped oxide I layer is 40nm, and the thickness of the metal ion doped oxide II layer is 50nm. The efficiency of the perovskite solar cell prepared by this method is 19.1%.

[0085] Example 8

[0086] Same as Example 1, except that:

[0087] The thickness of the metal ion doped oxide I layer is 40nm, and the thickness of the metal ion doped oxide II layer is 60nm. The efficiency of the perovskite solar cell prepared by this method is 19%.

[0088] Example 9

[0089] Same as Example 1, except that:

[0090] The sputtering power of the metal ion doped oxide layer I / metal ion doped oxide layer II is 50 W. The efficiency of the perovskite solar cell prepared by this method is 18.5%.

[0091] Example 10

[0092] Same as Example 1, except that:

[0093] The sputtering power of the metal ion doped oxide layer I / metal ion doped oxide layer II is 40 W. The efficiency of the perovskite solar cell prepared by this method is 18.3%.

[0094] Embodiment 11

[0095] Same as Example 1, except that:

[0096] The perovskite active layer is MAPbI3. The efficiency of the perovskite solar cell prepared by this method is 17.6%.

[0097] Example 12

[0098] Same as Example 1, except that:

[0099] The perovskite active layer is FAPbI3. The efficiency of the perovskite solar cell prepared by this method is 18.2%.

[0100] Example 13

[0101] Same as Example 1, except that:

[0102] The material of the metal ion doped oxide layer I / metal ion doped oxide layer II is AZO. The efficiency of the perovskite solar cell prepared by this method is 18.6%.

[0103] Embodiment 14

[0104] Same as Example 1, except that:

[0105] The material of the metal ion doped oxide layer I / metal ion doped oxide layer Ⅰ is IZO. The efficiency of the perovskite solar cell prepared by this method is 18.1%.

[0106] Embodiment 15

[0107] Same as Example 1, except that:

[0108] The concentration of the organic small molecule modification layer solution is 0.3 mg / mL. The efficiency of the perovskite solar cell prepared by this method is 19.3%.

[0109] Example 16

[0110] Same as Example 1, except that:

[0111] The concentration of the organic small molecule modification layer solution is 0.1 mg / mL. The efficiency of the perovskite solar cell prepared by this method is 19.1%.

[0112] Embodiment 17

[0113] Same as Example 1, except that:

[0114] The ultra-thin metal layer is made of Au. The efficiency of the perovskite solar cell prepared by this method is 19.5%.

[0115] Embodiment 18

[0116] Same as Example 1, except that:

[0117] The ultra-thin metal layer is made of Cu. The efficiency of the perovskite solar cell prepared by this method is 18.9%.

[0118] Embodiment 19

[0119] Same as Example 1, except that:

[0120] The thickness of the nano-tin oxide electron transport layer is 25nm, the thickness of the perovskite structure photoactive layer is 640nm, and the thickness of the hole transport layer is 70nm. The buffer layer material is MoO3, the thickness of the buffer layer is 10nm, and the thermal evaporation method is used, and the vacuum degree is 2×10 -4 Pa, the evaporation rate is

[0121] The metal ion doped oxide layer I / organic small molecule modified layer / ultra-thin metal layer / metal ion doped oxide layer Ⅰ is prepared by the following steps:

[0122] a. Preparation of metal ion-doped oxide layer I: using metal ion-doped oxide target material, substrate temperature is room temperature, sputtering pressure is controlled at 0.2 Pa, sputtering power is 40 W, sputtering time is 15 minutes, and metal ion-doped oxide layer I is prepared on the buffer layer. The metal ion-doped oxide target material is aluminum-doped zinc oxide, and the thickness of the metal ion-doped oxide layer I is 40 nm;

[0123] b. Preparation of organic small molecule modification layer: a BCP solution with a concentration of 0.3 mg / mL is used to prepare an organic small molecule modification layer on the metal ion-doped oxide layer I by spin coating, the rotation speed is 3000 rpm, and the thickness of the organic small molecule modification layer is 3 nm;

[0124] c. Preparation of ultra-thin metal layer: using metal target material, sputtering pressure controlled at 0.3Pa, sputtering power of 30W, sputtering time of 1 minute, preparing ultra-thin metal layer on the organic small molecule modified layer, the metal target material is silver, and the thickness of ultra-thin metal layer is 8nm;

[0125] d. Preparation of metal ion-doped oxide layer ⅠⅠ: Using metal ion-doped oxide target, the substrate temperature is room temperature, the sputtering gas pressure is controlled at 0.2 Pa, the sputtering power is 40 W, and the sputtering time is 15 minutes. The metal ion-doped oxide layer ⅠⅠ is prepared on the ultra-thin metal layer. The metal ion-doped oxide target is aluminum-doped zinc oxide, and the thickness of the metal ion-doped oxide layer ⅠⅠ is 50 nm.

[0126] Embodiment 20

[0127] Same as Example 1, except that:

[0128] The thickness of the nano-tin oxide electron transport layer is 35nm, the thickness of the perovskite structure photoactive layer is 660nm, and the thickness of the hole transport layer is 90nm. The buffer layer material is NiO x The thickness of the buffer layer is 30 nm, and the vacuum degree is 4×10 -4 Pa, the evaporation rate is

[0129] The metal ion doped oxide layer I / organic small molecule modified layer / ultra-thin metal layer / metal ion doped oxide layer Ⅰ is prepared by the following steps:

[0130] a. Preparation of metal ion-doped oxide layer I: using metal ion-doped oxide target material, substrate temperature is room temperature, sputtering pressure is controlled at 0.3 Pa, sputtering power is 60 W, sputtering time is 10 minutes, and metal ion-doped oxide layer I is prepared on the buffer layer. The metal ion-doped oxide target material is indium-doped tin oxide, and the thickness of the metal ion-doped oxide layer I is 60 nm;

[0131] b. Preparation of organic small molecule modification layer: a BCP solution with a concentration of 0.1 mg / mL is used to prepare an organic small molecule modification layer on the metal ion-doped oxide layer I by spin coating, the rotation speed is 4000 rpm, and the thickness of the organic small molecule modification layer is 5 nm;

[0132] c. Preparation of ultra-thin metal layer: using metal target material, sputtering pressure controlled at 0.2Pa, sputtering power of 20W, sputtering time of 2 minutes, preparing ultra-thin metal layer on the organic small molecule modified layer, the metal target material is aluminum, and the thickness of the ultra-thin metal layer is 10nm;

[0133] d. Preparation of metal ion-doped oxide layer ⅠⅠ: Using metal ion-doped oxide target, the substrate temperature is room temperature, the sputtering gas pressure is controlled at 0.3 Pa, the sputtering power is 60 W, and the sputtering time is 10 minutes. A metal ion-doped oxide layer ⅠⅠ is prepared on the ultra-thin metal layer. The metal ion-doped oxide target is indium-doped tin oxide, and the thickness of the metal ion-doped oxide layer ⅠⅠ is 60 nm.

[0134] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A double-sided perovskite solar cell based on a multi-layer transparent electrode, characterized in that: From bottom to top, it is composed of a transparent conductive layer, an electron transport layer, a perovskite structure photoactive layer, a hole transport layer, a buffer layer and a transparent top electrode. The transparent top electrode structure is a metal ion-doped oxide layer I / organic small molecule modification layer / ultra-thin metal layer / metal ion-doped oxide layer Ⅰ, and a metal ion-doped oxide layer Ⅰ is arranged on the top of the buffer layer.

2. The double-sided perovskite solar cell according to claim 1, characterized in that: The organic small molecule modification layer material is an organic small molecule that produces coordination effect with metal ions.

3. The double-sided perovskite solar cell according to claim 2, characterized in that: The organic small molecule modification layer material is selected from one or two of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, 6,6'-dicyano-2,2'-bipyridine and 1,10-phenanthroline-4,7-dicarboxylic acid.

4. The perovskite solar cell according to claim 1 or 2, characterized in that: In the structure of metal ion doped oxide layer I / organic small molecule modification layer / ultra-thin metal layer / metal ion doped oxide layer II, the thickness of the metal ion doped oxide layer I is 40-60nm, and the thickness of the metal ion doped oxide layer II is 50-60nm.

5. The perovskite solar cell according to claim 1 or 2, characterized in that: The buffer layer is a metal oxide layer, and the metal oxide is MoO3 or NiO x , the thickness of the buffer layer is 10-30nm.

6. The perovskite solar cell according to claim 1 or 2, characterized in that: In the structure of metal ion doped oxide layer I / organic small molecule modified layer / ultra-thin metal layer / metal ion doped oxide Ⅰ layer, the metal material of the ultra-thin metal layer is selected from one of silver, aluminum, gold and copper, and the metal ion doped oxide in the metal ion doped oxide layer I or the metal ion doped oxide Ⅰ layer is selected from one of indium-doped tin oxide, aluminum-doped zinc oxide and indium-doped zinc oxide.

7. The method for preparing a double-sided perovskite solar cell based on a multi-layer structure transparent electrode according to claim 1, characterized in that: The steps include: (1) treating the pretreated transparent conductive layer with ultraviolet ozone; (2) preparing a tin oxide nanofilm on the surface of the transparent conductive layer after the ultraviolet ozone treatment in step (1) to obtain a nano tin oxide electron transport layer; (3) preparing a perovskite structure photoactive layer on the nano-tin oxide electron transport layer obtained in step (2); (4) preparing a hole transport layer on the perovskite structure photoactive layer obtained in step (3); (5) depositing a buffer layer on the hole transport layer obtained in step (4) by thermal evaporation; (6) Using a magnetron sputtering method to prepare a metal ion-doped oxide layer I on the buffer layer obtained in step (5), preparing an organic small molecule modification layer on the metal ion-doped oxide layer I by a spin coating process, and then using a magnetron sputtering method to prepare an ultra-thin metal layer and a metal ion-doped oxide layer ⅠⅠ on the organic small molecule modification layer, respectively, to obtain the double-sided perovskite solar cell.

8. The preparation method according to claim 7, characterized in that: Step (6) is specifically prepared by the following steps: a. Preparation of metal ion-doped oxide layer I: using metal ion-doped oxide target material, substrate temperature is room temperature, sputtering pressure is controlled at 0.2-0.3 Pa, sputtering power is 40-60 W, sputtering time is 10-15 minutes, and metal ion-doped oxide layer I is prepared on the buffer layer obtained in step (5); b. Preparation of an organic small molecule modification layer: a 0.1-0.5 mg / mL organic small molecule solution is spin-coated on the metal ion-doped oxide I layer at a rotation speed of 3000-4000 rpm; c. Preparation of ultra-thin metal layer: using metal target material, sputtering pressure controlled at 0.2-0.3Pa, sputtering power at 20-30W, sputtering time at 1-2 minutes, to prepare ultra-thin metal layer on the organic small molecule modified layer; d. Preparation of metal ion-doped oxide layer ⅠⅠ: metal ion-doped oxide target material is used, the substrate temperature is room temperature, the sputtering pressure is controlled at 0.2-0.3Pa, the sputtering power is 40-60W, the sputtering time is 10-15 minutes, and the metal ion-doped oxide layer ⅠⅠ is prepared on the ultra-thin metal layer.

9. The preparation method according to claim 8, characterized in that: In step a or d, the metal ion-doped oxide target is selected from one of indium-doped tin oxide, aluminum-doped zinc oxide and indium-doped zinc oxide, and in step c, the metal target is selected from one of silver, aluminum, gold and copper.

10. Application of the double-sided perovskite solar cell based on multi-layer structure transparent electrode in photovoltaic building integration according to claim 1, characterized in that: The bifacial perovskite solar cells are made into bifacial solar panels, which are integrated into the exterior of a building, with the front side capturing incident sunlight and the back side absorbing indoor light and reflected light.

Citation Information

Patent Citations

  • Double-buffer-layer perovskite solar cell manufacturing method

    CN109326718A

  • Perovskite solar cell and rapid preparation method thereof

    CN115768222A

  • Organic electroluminescence device

    CN1564641A