Zinc oxide nanoparticle electron transport layer, preparation method thereof and flexible wearable electronic equipment

The electron transport layer of zinc oxide nanoparticles was prepared by chemical precipitation method and modified by amino acid surface, which solved the oxygen vacancies defects and grain size problems in the electron transport layer film of zinc oxide nanoparticles, improved the charge transfer efficiency and device stability, and was suitable for Flexible wearable devices and organic solar cells.

CN119012723APending Publication Date: 2024-11-22HUBEI CHINA TOBACCO INDUSTRY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411091562.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There are a large number of oxygen vacancies defects in the existing zinc oxide nanoparticle electron transport layer film, which limits the charge transfer efficiency and device stability, and the large grain size leads to holes, affecting electron mobility and stability.

Method used

The electron transport layer of zinc oxide nanoparticles was prepared by chemical precipitation method, and the surface defect density was reduced through amino acid surface modification, and the charge extraction capacity was optimized, including coating the ZnO-NPs solution onto the substrate, then spin coating the amino acid surface modification solution and annealing.

Benefits of technology

It effectively reduces the surface defect density of zinc oxide nanoparticles, improves charge transmission and collection efficiency, enhances the energy conversion efficiency and stability of the device, and reduces leakage current. It is suitable for flexible wearable electronic devices and organic solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004986725240000011
    Figure HDA0004986725240000011
  • Figure HDA0004986725240000012
    Figure HDA0004986725240000012
  • Figure HDA0004986725240000021
    Figure HDA0004986725240000021
Patent Text Reader

Abstract

The invention provides a preparation method of a zinc oxide nanoparticle electron transport layer, which comprises the following steps: A) coating a ZnO-NPs solution on a substrate to obtain a ZnO-NPs electron transport layer film; and B) spin-coating the ZnO-NPs electron transport layer film with the amino acid surface modification solution, and annealing to obtain the ZnO-NPs electron transport layer. According to the amino acid surface modified ZnO-NPs, the surface defects of ZnO-NPs can be reduced, charge recombination is effectively reduced, the charge transmission and collection efficiency is improved, the leakage current of a device is reduced, and carrier recombination can be better inhibited, so that the energy conversion efficiency (PCE) of an organic solar cell device is improved, and the stability of the device is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a zinc oxide nanoparticle electron transport layer and a preparation method thereof, a flexible wearable electronic device and a firmware in a cigarette filter rod. Background Art

[0002] In the field of optoelectronic technology, the electron transport layer is a key functional layer, and its performance directly affects the energy conversion efficiency and stability of solar cells. At present, there are many kinds of electron transport layer materials, including metal materials, oxide semiconductor materials, inorganic composite materials, and polymer dielectric materials. Among them, oxide semiconductor materials are particularly favored because of their high transmittance in the visible light region, high reflectivity to infrared light, and low resistance. They are considered to be ideal choices for building high-quality electron transport layers. Taking ZnO as an example, its optical bandgap is about 3.2eV, and it has extremely high transparency to visible light. It is also rich in resources, non-toxic, and low in cost. These advantages have made zinc oxide quickly become the focus of electron transport layer research and application in the past decade, especially in the optoelectronic field, showing broad application potential.

[0003] At present, there are various methods for preparing zinc oxide thin films, including electron beam vacuum evaporation, magnetron sputtering, chemical vapor deposition, sol-gel method and chemical precipitation method, etc. Among them, chemical precipitation method has become an attractive preparation method due to its advantages of low cost, simple process, good uniformity of thin film formation, low preparation temperature and easy and precise doping.

[0004] However, the presence of a large number of oxygen vacancy defects in the electron transport layer film of zinc oxide nanoparticles (ZnO-NPs) prepared by chemical precipitation not only limits the effective charge transport and collection efficiency, but also may lead to energy level mismatch between the ZnO-NPs film and the photoactive layer due to the formation of Schottky contact. In addition, compared with the ZnO film obtained by the sol-gel method, the larger grain size of ZnO-NPs may increase the interstitial area between nanoparticles, resulting in the appearance of holes in the film, which is not only not conducive to improving the electron mobility, but also may make the active layer more susceptible to corrosion by water and oxygen, resulting in reduced stability of the device.

[0005] With the vigorous development of flexible wearable electronic devices and the Internet of Things, people have an increasing demand for high-performance electron transport layers that can be prepared at low temperature and low cost. Therefore, a simple and efficient method for preparing zinc oxide electron transport layer films is urgently needed. Summary of the invention

[0006] In view of this, the technical problem to be solved by the present invention is to provide a method for preparing a zinc oxide nanoparticle electron transport layer. The zinc oxide nanoparticle electron transport layer prepared by the present invention retains the original photoelectric properties of the zinc oxide nanoparticles, reduces its surface defect density, maintains high transmittance, and optimizes the charge extraction capability.

[0007] The present invention provides a method for preparing a zinc oxide nanoparticle electron transport layer, comprising:

[0008] A) coating a ZnO-NPs solution onto a substrate to obtain a ZnO-NPs electron transport layer film;

[0009] B) Spin-coat the amino acid surface modification solution onto the ZnO-NPs electron transport layer film and anneal to obtain the result.

[0010] Preferably, the method for preparing the ZnO-NPs solution comprises:

[0011] i) heating and mixing the zinc salt and the solvent to obtain a zinc salt solution;

[0012] ii) adding the precipitant solution dropwise to the zinc salt solution, heating and stirring, and cooling to obtain a precipitate;

[0013] iii) dispersing the precipitate into the dispersion liquid to obtain a ZnO-NPs solution.

[0014] Preferably, the zinc salt in step i) is one or more of zinc acetate, zinc nitrate, and zinc chloride; the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, and water; and the heating temperature is 25 to 100°C.

[0015] Preferably, the precipitant in step ii)

[0016] One of potassium hydroxide, sodium hydroxide, and sodium bicarbonate; the solvent of the precipitant solution is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, and water; the concentration of the precipitant solution is 0.1-100 mg / mL; the temperature of the heating and stirring is 25° C., and the time is 30 min; the dropping speed is 10 mL / min.

[0017] Preferably, the dispersion in step iii) is one or more of methanol, ethanol, isopropanol, water, chloroform, and chlorobenzene;

[0018] The concentration of the ZnO-NPs solution is 0.1-100 mg / mL.

[0019] Preferably, in step A), the substrate is selected from ITO glass, crystalline silicon wafer, quartz wafer, PET, PEN or PI.

[0020] Preferably, in step B), the amino acid surface modification solution is an amino acid small molecule material dissolved in a solvent; the amino acid small molecule material is L-2,4-diaminobutyric acid (L-DABA), L-2,5-diaminopentanoic acid (D-Orn) or L-2,6-diaminohexanoic acid (Lys); the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, water, and ammonia water; the concentration of the amino acid surface modification solution is 0.1 to 10 mg / mL.

[0021] Preferably, the annealing temperature in step B) is 0-200° C. and the annealing time is 10-120 min.

[0022] The present invention provides a zinc oxide nanoparticle electron transport layer, which is prepared by the preparation method described in any one of the above technical solutions.

[0023] The present invention provides a flexible wearable electronic device, comprising the zinc oxide nanoparticle electron transport layer described in the above technical solution.

[0024] Compared with the prior art, the present invention provides a method for preparing a zinc oxide nanoparticle electron transport layer, comprising: A) coating a ZnO-NPs solution on a substrate to obtain a ZnO-NPs electron transport layer film; B) spin coating an amino acid surface modified solution on the ZnO-NPs electron transport layer film, and annealing. The amino acid surface modified ZnO-NPs of the present invention can reduce the surface defects of ZnO-NPs, effectively reduce charge recombination, improve the charge transfer and collection efficiency, reduce the leakage current of the device, and better suppress the recombination of carriers, thereby improving the energy conversion efficiency (PCE) of the organic solar cell device and improving the stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : Ultraviolet-visible spectra (UV-Vis) of ZnO-NPs and ZnO-NPs / lysine electron transport layer films in Example 1 and Comparative Example 1.

[0026] Figure 2 : Atomic force microscopy (AFM) images of ZnO-NPs and ZnO-NPs / lysine electron transport layer films in Example 1 and Comparative Example 1.

[0027] Figure 3 : X-ray photoelectron spectroscopy (XPS) of ZnO-NPs and ZnO-NPs / lysine electron transport layer films in Example 1 and Comparative Example 1.

[0028] Figure 4: Performance parameters of organic solar cells prepared with ZnO-NPs and ZnO-NPs / lysine electron transport layer films in Example 1 and Comparative Example 1 (a) IV curve; (b) EQE.

[0029] Figure 5 : Dark current curves of organic solar cells prepared with ZnO-NPs and ZnO-NPs / lysine electron transport layer films in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0030] The present invention provides a zinc oxide nanoparticle electron transport layer and a preparation method thereof and a flexible wearable electronic device. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be pointed out in particular that all similar replacements and modifications are obvious to those skilled in the art, and they all fall within the scope of protection of the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0031] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0032] In this application, "at least one" means one or more, "more than one" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items.

[0033] The present invention proposes an innovative amino acid surface modification technology and applies it to the surface of the electron transport layer film of zinc oxide nanoparticles (ZnO-NPs), aiming to achieve the comprehensive optimization of its low-temperature preparation, high light transmittance and excellent conductivity. The present invention adopts a chemical precipitation method to prepare the ZnO-NPs electron transport layer film, and then modifies its surface by lysine (Lys) molecules. The obtained ZnO-NPs / Lys composite electron transport layer not only retains the original photoelectric properties of zinc oxide nanoparticles, but also significantly reduces its surface defect density through amino acid modification, ensures high light transmittance in the visible spectrum, and optimizes the charge extraction capability, thereby meeting the growing demand of modern optoelectronic technology for high-performance electron transport layer materials.

[0034] The present invention provides a method for preparing a zinc oxide nanoparticle electron transport layer, comprising:

[0035] A) coating a ZnO-NPs solution onto a substrate to obtain a ZnO-NPs electron transport layer film;

[0036] B) Spin-coat the amino acid surface modification solution onto the ZnO-NPs electron transport layer film and anneal to obtain the result.

[0037] The present invention firstly prepares a ZnO-NPs solution.

[0038] The preparation method of the ZnO-NPs solution of the present invention comprises:

[0039] i) heating and mixing the zinc salt and the solvent to obtain a zinc salt solution;

[0040] ii) adding the precipitant solution dropwise to the zinc salt solution, heating and stirring, and cooling to obtain a precipitate;

[0041] iii) dispersing the precipitate into the dispersion liquid to obtain a ZnO-NPs solution.

[0042] The preparation method of the ZnO-NPs solution of the present invention first heats and mixes a zinc salt and a solvent to obtain a zinc salt solution. The zinc salt is one or more of zinc acetate, zinc nitrate, and zinc chloride; the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, and water. The heating temperature is 25 to 100°C; it can be 25°C, 30°C, 40°C, 50°C, 60°C, 65°C, 75°C, 85°C, 100°C; or a range between any two of the above.

[0043] Wherein, the mass ratio of zinc salt to solvent is 1:9;

[0044] The precipitant solution is added dropwise to the zinc salt solution, heated and stirred, and cooled to obtain a precipitate.

[0045] Dissolve the zinc salt in the solvent, heat and stir, and after the solute is completely dissolved, slowly add the precipitant solution to the dissolved zinc salt solution. 2+ After complete precipitation, keep heating and stirring, take out the bottom precipitate after natural cooling, wash 2 to 3 times, and finally disperse the precipitate into the dispersion liquid to prepare a ZnO-NPs solution of a certain concentration.

[0046] According to the present invention, the precipitant is one of potassium hydroxide, sodium hydroxide and sodium bicarbonate; the solvent of the precipitant solution is one or more of methanol, ethanol, isopropanol, dimethoxyethanol and water; the concentration of the precipitant solution is 0.1-100 mg / mL; preferably 3-100 mg / mL; specifically 3 mg / mL, 5 mg / mL, 10 mg / mL, 20 mg / mL, 50 mg / mL, 60 mg / mL, 70 mg / mL, 100 mg / mL, or a range between any two of the above.

[0047] The heating and stirring temperature was 25° C. and the time was 30 min; the dropping speed was 10 mL / min.

[0048] The precipitate is dispersed in a dispersion to obtain a ZnO-NPs solution. The dispersion is one or more of methanol, ethanol, isopropanol, water, chloroform, and chlorobenzene; the concentration of the ZnO-NPs solution is 0.1 to 100 mg / mL. Specifically, it can be 2 mg / mL, 3 mg / mL, 6 mg / mL, 30 mg / mL, 50 mg / mL, 60 mg / mL, 80 mg / mL, 100 mg / mL; or a range between any two of the above.

[0049] The ZnO-NPs solution was coated onto a substrate to obtain a ZnO-NPs electron transport layer film.

[0050] The substrate of the present invention is selected from ITO glass, crystalline silicon wafer, quartz wafer, PET, PEN or PI.

[0051] The present invention does not limit the specific operation of the coating, which is well known to those skilled in the art.

[0052] The amino acid surface modification solution is spin-coated on the ZnO-NPs electron transport layer film and annealed to obtain the film.

[0053] The amino acid surface modification solution of the present invention is amino acid small molecule materials dissolved in a solvent.

[0054] The amino acid small molecule material is L-2,4-diaminobutyric acid (L-DABA), L-2,5-diaminopentanoic acid (D-Orn) or L-2,6-diaminohexanoic acid (Lys); the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, water, and ammonia water;

[0055] The concentration of the amino acid surface modification solution is 0.1-10 mg / mL, and can be specifically 0.5 mg / mL, 0.8 mg / mL, 2 mg / mL, 3 mg / mL, 5 mg / mL, 6 mg / mL, 10 mg / mL, or a range between any two of the above.

[0056] The annealing temperature of the present invention is 0-200°C, specifically 0.5°C, 20°C, 25°C, 50°C, 60°C, 80°C, 100°C, 150°C, 200°C; or a range between any two of the above.

[0057] The annealing time of the present invention is 10 to 120 min, specifically 10 min, 30 min, 50 min, 70 min, 80 min, 100 min, 110 min, 120 min, or a range between any two of the above.

[0058] The present invention provides a zinc oxide nanoparticle electron transport layer, which is prepared by the preparation method described in any one of the above technical solutions.

[0059] The present invention provides a flexible wearable electronic device, comprising the zinc oxide nanoparticle electron transport layer described in the above technical solution.

[0060] Compared with the prior art, the present invention has the following beneficial effects:

[0061] 1) The present invention uses low-cost zinc salt and amino acid small molecules as raw materials and alcohol or water as solvent, which greatly reduces the cost of preparing a high-efficiency electron transport layer.

[0062] 2) The present invention adopts a chemical precipitation method to prepare a zinc oxide nanoparticle electron transport layer film, and uses amino acid small molecule materials for surface modification, does not require complex equipment, has a simple process, and can achieve large-scale industrial production.

[0063] 3) The surface of the ZnO-NPs / Lys composite electron transport layer film in the present invention is uniform, the annealing temperature requirement is low, the annealing time is short, and the operation is simple. Only simple operations are required to obtain an electron transport layer film with excellent optical and electrical properties.

[0064] 4) The present invention uses the prepared ZnO-NPs / Lys composite electron transport layer film in organic solar cells to increase the short-circuit current, inhibit leakage current, and ultimately achieve improved energy conversion efficiency and stability of thin-film solar cells; when it is applied to flexible devices, the mechanical properties of the flexible devices are significantly improved.

[0065] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0066] The numerical ranges and parameters involved in the present invention have presented the relevant numerical values ​​in the specific embodiments as accurately as possible. However, any numerical value essentially inevitably contains standard deviations due to individual testing methods. Therefore, unless otherwise explicitly stated, it should be understood that all numerical ranges or specific data used in this disclosure may have certain reasonable deviations within a certain range, for example: within 1% or 0.5%.

[0067] Some cases are recorded in the embodiments and comparative examples of the present invention, wherein the embodiments show certain implementation modes of the present invention. However, this does not mean that the effects of the present invention can only be achieved in these cases.

[0068] In order to further illustrate the present invention, a zinc oxide nanoparticle electron transport layer, a preparation method thereof, and a flexible wearable electronic device provided by the present invention are described in detail below in combination with embodiments.

[0069] Example 1

[0070] Dissolve hydrated zinc acetate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 22.8 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0071] The L-2,6 diaminohexanoic acid (Lys) small molecule was dissolved in a solvent of methanol: water at a ratio of 1:9, and stirred until completely dissolved to prepare a surface modification solution with a concentration of 0.8 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 100°C for 10 minutes.

[0072] Example 2

[0073] Dissolve hydrated zinc nitrate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 50 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0074] The L-2,5-diaminopentanoic acid (D-Orn) small molecule was dissolved in a solvent of methanol: water at a ratio of 1:9, and stirred until completely dissolved to prepare a surface modification solution with a concentration of 3 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 100°C for 20 minutes.

[0075] Example 3

[0076] Dissolve hydrated zinc chloride in ethanol solvent and heat and stir at 75°C. After the solute is completely dissolved, slowly add 5 mg / mL sodium hydroxide ethanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with ethanol. Finally, disperse the precipitate into a dispersion liquid with a methanol: chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0077] The L-2,4-diaminobutyric acid (L-DABA) small molecule was dissolved in a solvent of methanol: water at a ratio of 1:9, and stirred until completely dissolved to prepare a surface modification solution with a concentration of 0.5 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 100°C for 30 minutes.

[0078] Example 4

[0079] Dissolve hydrated zinc acetate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 22.8 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol: chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 30 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0080] The L-2,4-diaminobutyric acid (L-DABA) small molecule was dissolved in a solvent of methanol: water at a ratio of 1:9, and stirred until completely dissolved to prepare a surface modification solution with a concentration of 0.8 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 100°C for 50 minutes.

[0081] Example 5

[0082] Dissolve hydrated zinc acetate and zinc nitrate in a certain proportion in isopropanol solvent, heat and stir at 75°C. After the solute is completely dissolved, slowly add 3 mg / mL sodium hydroxide isopropanol solution to the dissolved zinc solution. 2+After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with isopropanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 80 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0083] The L-2,5-diaminopentanoic acid (D-Orn) small molecule was dissolved in a solvent of formazan and stirred until completely dissolved to prepare a surface modification solution with a concentration of 10 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 200°C for 60 minutes.

[0084] Example 6

[0085] Dissolve hydrated zinc acetate and zinc chloride in methanol solvent, heat and stir at 65°C. After the solute is completely dissolved, slowly add 100 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a methanol dispersion to prepare a ZnO-NPs solution with a concentration of 2 mg / mL. The ZnO-NPs solution is coated on a PET substrate to obtain a ZnO-NPs electron transport layer film.

[0086] The L-2,5-diaminopentanoic acid (D-Orn) small molecule was dissolved in a water solvent and stirred until completely dissolved to prepare a surface modification solution with a concentration of 5 mg / mL. The surface modification solution was spin-coated on the ZnO-NPs electron transport layer film, and the annealing temperature was 25°C and the time was 120 min.

[0087] Comparative Example 1

[0088] Dissolve hydrated zinc acetate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 22.8 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0089] Comparative Example 2

[0090] Dissolve hydrated zinc nitrate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 50 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1, and prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0091] Comparative Example 3

[0092] Dissolve hydrated zinc chloride in ethanol solvent and heat and stir at 75°C. After the solute is completely dissolved, slowly add 5 mg / mL sodium hydroxide ethanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with ethanol. Finally, disperse the precipitate into a dispersion liquid with a methanol: chloroform ratio of 9:1 to prepare a ZnO-NPs solution with a concentration of 6 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0093] Comparative Example 4

[0094] Dissolve hydrated zinc acetate in methanol solvent and heat and stir at 65°C. After the solute is completely dissolved, slowly add 22.8 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1, and prepare a ZnO-NPs solution with a concentration of 30 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0095] Comparative Example 5

[0096] Dissolve hydrated zinc acetate and zinc nitrate in a certain proportion in isopropanol solvent, heat and stir at 20°C. After the solute is completely dissolved, slowly add 3 mg / mL sodium hydroxide isopropanol solution to the dissolved zinc solution. 2+After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with isopropanol. Finally, disperse the precipitate into a dispersion liquid with a methanol:chloroform ratio of 9:1 to prepare a ZnO-NPs solution with an indium concentration of 80 mg / mL. The ZnO-NPs solution is coated on an ITO glass substrate to obtain a ZnO-NPs electron transport layer film.

[0097] Comparative Example 6

[0098] Dissolve hydrated zinc acetate and zinc chloride in methanol solvent, heat and stir at 65°C. After the solute is completely dissolved, slowly add 100 mg / mL potassium hydroxide methanol solution to the dissolved zinc solution. 2+ After complete precipitation, keep heating and stirring for a period of time, take out the bottom precipitate after natural cooling, and wash it three times with methanol. Finally, disperse the precipitate into a methanol dispersion to prepare a ZnO-NPs solution with a concentration of 2 mg / mL. The ZnO-NPs solution is coated on a PET substrate to obtain a ZnO-NPs electron transport layer film.

[0099] The films prepared in Example 1 and Comparative Example 1 were subjected to UV-Vis testing, AFM testing, and XPS testing, respectively. The ZnO-NPs / Lys film prepared in Example 1 and the ZnO-NPs film prepared in Comparative Example 1 were applied to organic solar cells, and their device performance was tested, including IV curve, EQE, dark current and other performance tests. The results are shown in the accompanying drawings.

[0100] By attaching Figure 1 From the UV-Vis test results, it can be found that the average transmittance of the ZnO-NPs electron transport layer film modified with Lys in Example 1 and the untreated ZnO-NPs film in Comparative Example 1 in visible light is basically the same.

[0101] By attaching Figure 2 It can be found from the AFM spectrum that the Lys-modified ZnO-NPs electron transport layer film in Example 1 has a lower surface roughness than that in Comparative Example 1, so that the film in Example 1 has a lower leakage current and a higher device efficiency when used in a device.

[0102] By attaching Figure 3 From the XPS spectrum, it can be found that the Lys-modified ZnO-NPs electron transport layer film in Example 1 has a higher lattice oxygen content and a lower defect oxygen content than that in Comparative Example 1. Therefore, Lys modification can effectively passivate surface defects and reduce carrier recombination during charge extraction.

[0103] By attaching Figure 4The device performance test shows that the organic solar cell prepared by the Lys-modified ZnO-NPs electron transport layer film in Example 1 has a higher conversion efficiency (PCE) and a better external quantum efficiency (EQE) than that in Comparative Example 1.

[0104] By attaching Figure 5 The device performance test shows that the organic solar cell prepared by the Lys-modified ZnO-NPs electron transport layer film in Example 1 has a lower dark current density.

[0105] The following conclusions can be drawn from the above data and attached figures:

[0106] The organic solar cell prepared in Example 1 provided by the present invention is more excellent than that in Comparative Example 1. The thin-film solar cell prepared by using Lys-modified ZnO-NPs as an electron transport layer has higher energy conversion efficiency and lower dark current.

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a zinc oxide nanoparticle electron transport layer, characterized in that: include: A) coating a ZnO-NPs solution onto a substrate to obtain a ZnO-NPs electron transport layer film; B) Spin-coat the amino acid surface modification solution onto the ZnO-NPs electron transport layer film and anneal to obtain the result.

2. The preparation method according to claim 1, characterized in that: The preparation method of the ZnO-NPs solution comprises: i) heating and mixing the zinc salt and the solvent to obtain a zinc salt solution; ii) adding the precipitant solution dropwise to the zinc salt solution, heating and stirring, and cooling to obtain a precipitate; iii) dispersing the precipitate into the dispersion liquid to obtain a ZnO-NPs solution.

3. The preparation method according to claim 1, characterized in that: In step i), the zinc salt is one or more of zinc acetate, zinc nitrate and zinc chloride; the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol and water; and the heating temperature is 25-100°C.

4. The preparation method according to claim 1, characterized in that: Step ii) the precipitant is one of potassium hydroxide, sodium hydroxide and sodium bicarbonate; the solvent of the precipitant solution is one or more of methanol, ethanol, isopropanol, dimethoxyethanol and water; the concentration of the precipitant solution is 0.1-100 mg / mL; the temperature of the heating and stirring is 25°C and the time is 30 min; the dropping speed is 10 mL / min.

5. The preparation method according to claim 1, characterized in that: Step iii) the dispersion liquid is one or more of methanol, ethanol, isopropanol, water, chloroform, and chlorobenzene; The concentration of the ZnO-NPs solution is 0.1-100 mg / mL.

6. The preparation method according to claim 1, characterized in that: In step A), the substrate is selected from ITO glass, crystalline silicon wafer, quartz wafer, PET, PEN or PI.

7. The preparation method according to claim 1, characterized in that: Step B) The amino acid surface modification solution is an amino acid small molecule material dissolved in a solvent; the amino acid small molecule material is L-2,4-diaminobutyric acid (L-DABA), L-2,5-diaminopentanoic acid (D-Orn) or L-2,6-diaminohexanoic acid (Lys); the solvent is one or more of methanol, ethanol, isopropanol, dimethoxyethanol, water, and ammonia water; the concentration of the amino acid surface modification solution is 0.1 to 10 mg / mL.

8. The preparation method according to claim 1, characterized in that: Step B) the annealing temperature is 0-200° C. and the time is 10-120 min.

9. A zinc oxide nanoparticle electron transport layer, characterized in that: The preparation method is as described in any one of claims 1 to 8.

10. A flexible wearable electronic device, characterized in that: The invention comprises the zinc oxide nanoparticle electron transport layer as claimed in claim 9.