Butt-joint laser beam welding method
Through laser cutting processing, the cutting surface of the steel plate with high precision inclination angle is formed, and the welding is carried out with a spiral laser beam, which solves the problems of welding fracture and burn-through of thin steel plates, achieving high-quality welding and productivity improvement.
Patent Information
- Application Number
- CN202380035507.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-26
- Filing Date
- 2023-01-06
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to achieve high-quality butt welding in the continuous processing production line of thin steel plates, especially in thin steel plates with a plate thickness of less than 1.0 mm, and welding fracture and burn-through are prone to occur.
The high-precision inclination angle of the steel plate cut-off surface is formed by laser cutting processing, and welding is carried out with a spiral laser beam to ensure the melt width and heat input of the welded part, and prevent burn-through and melting residues from occurring.
High-quality butt welding of thin steel plates is achieved, reducing the re-welding time, preventing welding fractures, and improving productivity.
Smart Images

Figure CN119013120A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a butt laser beam welding method for butting two thin steel plates together at their cut surfaces and irradiating the butted portions with a laser beam to perform welding. Background Art
[0002] In recent years, in the production lines of steel products, especially pickling lines, cold rolling lines, annealing lines, finishing lines, surface treatment lines, etc., steel sheets that are wound into coils are continuously processed while being unwound and passed through the production line from the viewpoint of improving quality and productivity. In such a continuous processing line, it is necessary to join the tail end of the preceding steel sheet with the front end of the succeeding steel sheet by some method at the entry side.
[0003] As the above-mentioned joining method, flash butt welding, lap welding, etc. have been widely used, but laser beam welding is mainly used for steel plates with poor brittleness containing a large amount of alloy components. In this laser beam welding, the tail end of the preceding thin steel plate and the front end of the succeeding thin steel plate are cut by a shearing machine provided in the welding device to adjust the accuracy of the end surface of the welded portion, and then the end surfaces are butted and then welded.
[0004] However, in the case of cutting by mechanical means such as shearing, it is difficult to make the cut surface completely straight. In addition, since the end surface after cutting generates a collapsed edge and a flash, no matter how the cutting accuracy is improved, the gap width (gap) between the butted steel plates cannot be made 0 (zero). To address this problem, a filler material (filler) is supplied to the gap between the steel plates to perform welding (for example, refer to Patent Documents 1 and 2).
[0005] However, the laser used for laser beam welding of steel plates generally has an output of less than 10 kW and a beam diameter of about 0.4 to 0.6 mm, so it is not easy to irradiate the weld with a laser beam with high accuracy. Therefore, the laser beam irradiated to the weld is swung (weaving) in a manner that crosses the butt joint of the steel plates (for example, refer to Patent Documents 3 to 5).
[0006] However, the techniques disclosed in the above-mentioned Patent Documents 3 and 4 do not supply fillers to the welded portion and cannot be applied to the case where fillers are supplied. In addition, the technique disclosed in the above-mentioned Patent Document 5 has the following problem: when the gap width between the butted steel plates is large or changes in the plate width direction, a welded joint with excellent mechanical strength cannot be stably obtained.
[0007] In order to solve the above problem, Patent Document 6 discloses a technique of turning one of the butted steel plates over to minimize the gap between the butted steel plates. In addition, Patent Document 7 discloses a method in which the opposite end faces (cut faces) of two plate-shaped raw materials to be butt-welded are formed into inclined faces inclined in the same direction relative to the vertical plane of the raw material surface, and after the opposite end faces are butted, a laser beam is irradiated on the butted portion from substantially vertically above to perform welding.
[0008] Prior art literature Patent Literature Patent Document 1: Japanese Patent Application Laid-Open No. 03-133587 Patent Document 2: Japanese Patent Application Laid-Open No. 08-290281 Patent Document 3: Japanese Patent Application Publication No. 2014-205166 Patent Document 4: International Publication No. 2020 / 179029 Patent Document 5: Japanese Patent Application Publication No. 2003-170284 Patent Document 6: Japanese Patent Application Publication No. 2001-205432 Patent Document 7: Japanese Patent Application Publication No. 2012-135796 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, even if the welding methods disclosed in the above-mentioned patent documents 6 and 7 are applied to the joining of thin steel plates with a thin plate thickness and a large width, it is difficult to obtain a sound joint over the entire plate width of the thin steel plate. In particular, in thin steel plates with a plate thickness of less than 1.0 mm, it is difficult to prevent weld fractures in a continuous processing production line.
[0011] The present invention has been made in view of the above problems existing in the prior art, and an object of the present invention is to provide a butt laser beam welding method capable of obtaining a high-quality butt weld joint even in a thin steel plate having a small plate thickness and a large width.
[0012] Technical solutions to solve problems
[0013] In order to solve the above-mentioned problems, the inventors have repeatedly conducted in-depth research, especially focusing on the technology of the above-mentioned Patent Document 7. As a result, the main reason why a sound weld cannot be formed by the above-mentioned prior art is that, since the above-mentioned technology is a technology for tailor-welded plates as described above, the cut surface of the plate-shaped raw material to be butt-welded is not formed with high precision. In addition, it was found that since the inclination angle of the above-mentioned relative end faces relative to the vertical plane is inappropriate, burn-through is likely to occur in a thin steel plate with a plate thickness of less than 1.0 mm. In addition, in order to solve the above-mentioned problems existing in the prior art, it was found that it is effective to use laser cutting processing to form the cut surface of the steel plate to be butted with high precision, and it is necessary to set the inclination angle of the cut surface of the steel plate to be butted to an appropriate range, thereby developing the present invention.
[0014] The present invention based on the above findings provides a butt laser beam welding method, which, after butting the cut surfaces of two steel plates with a plate thickness t of 0.1 to 3.0 mm against each other, feeds a filler to the butt joint, and irradiates the butt joint with a laser beam to melt the filler and the steel plates, thereby welding the two steel plates. The method is characterized in that the cut surfaces of the two steel plates are formed by laser cutting to have the same direction and an inclination angle θ greater than 20° and less than 60° relative to the vertical plane of the steel plate surface, and the width a of the cut surfaces in the length direction of the steel plates is less than 3.0 mm. Thereafter, the cut surfaces of the two steel plates are butt-joined in a beveled state for welding.
[0015] The butt laser beam welding method of the present invention is characterized in that a minimum molten width w of a weld formed by the laser beam irradiation is set to be at least 0.7 times the width a of the cut surface in the longitudinal direction of the steel plate.
[0016] The butt laser beam welding method of the present invention is characterized in that the laser beam is irradiated while being swung with respect to the butted portion of the butted steel plates so that the irradiation trajectory becomes a spiral shape.
[0017] Furthermore, the butt laser beam welding method of the present invention is characterized in that the swing width b of the laser beam is set to 2.5 mm or less.
[0018] The butt laser beam welding method of the present invention is characterized in that the heat input per unit plate thickness and per unit welding length of the laser beam is set to 10000 kJ / m 2 above.
[0019] Effects of the Invention
[0020] According to the present invention, since the cut surfaces of two steel plates are formed to have an appropriate inclination angle in the same direction relative to the vertical surface of the steel plate surface, and the cut surfaces are butted in an overlapping manner in a bevel joint shape, and then welded, it is possible to absorb the variation of the butt gap in the plate width direction of the thin steel plate and the adverse effects of the poor shape of the thin steel plate on welding, and a sound weld can be formed. In particular, the welding method of the present invention has the effect of preventing burn-through during welding, so even in a steel plate thinner than 1.0 mm in thickness, which is difficult to weld in the prior art, a high-quality butt laser welded joint can be obtained. Therefore, according to the present invention, not only can the time for re-welding caused by poor welding of thin steel plates be reduced, but also welding fractures in a continuous processing line can be prevented, which can greatly contribute to the improvement of productivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a diagram showing an example of a laser cutting processing device used in the butt laser welding method of the present invention. Figure 2 It is a diagram for explaining the butted portion in butt laser welding of the present invention. Figure 3 This is a diagram showing an example of a laser beam welding device used in the butt laser welding method of the present invention. Figure 4 It is a diagram for explaining the oscillation of the laser beam in the butt laser welding of the present invention. Figure 5 This is a diagram for explaining an example of a method of oscillating a laser beam. Figure 6 1 and 1 are views schematically illustrating a cross section of a laser beam welded portion. (a) is an example in which the minimum molten width w is larger than the width a of the butted portion, and (b) is an example in which the minimum molten width w is smaller than the width a of the butted portion. Figure 7 This is a diagram for explaining a welding method when there is a difference in plate thickness between steel plates to be welded. Figure 8 This is a diagram for explaining the thickness h of the welded portion when two steel plates to be welded have different plate thicknesses. DETAILED DESCRIPTION
[0022] First, the basic technical concept of the present invention will be described.
[0023] In the thin steel plate with a thin plate thickness and a large width, which is the object of the present invention, the formation of the opposite end faces (cut surfaces) to be butt-welded is performed by mechanical methods such as shearing. Therefore, for example, when the steel plate has an edge corrugation, an intermediate corrugation, a warp, or other shape defects, it is difficult to cut the thin steel plate straightly in the plate width direction, resulting in a dimensional error in the plate width direction. In addition, since the cut end face has collapsed edges, flash, etc., it has unevenness. Therefore, even if the cut surfaces are butted, a gap will be generated between the steel plates, and there will be a problem of large deviation in the plate width direction.
[0024] The above-mentioned unevenness and deviation of the gap width in the plate width direction of the butted portion of the steel plates can be solved to a certain extent by forming the cut surfaces of the butted steel plates to have an inclination angle in the same direction relative to the vertical surface of the steel plate surface, as disclosed in Patent Document 7. However, the prior art of Patent Document 7 is developed as a welding method suitable for forming a raw material for automobile body parts such as longitudinal beams and pillars (so-called tailored blank construction method). Therefore, no research has been conducted on the method for forming the cut surface to be butted. As a result, since the cut surfaces of the butted steel plates are not formed with high precision, there is a problem that it is difficult to obtain a high-quality butt welded joint.
[0025] Therefore, in order to solve the above-mentioned problem, the present invention uses a non-contact laser cutting process to form the cut surface of the steel plates to be butted with high precision. As a result, the cut surface can be formed straight and with high precision in the plate width direction regardless of the shape of the thin steel plate. In addition, in the laser cutting process, it becomes extremely easy to form the cut surface with an inclination angle relative to the vertical surface of the steel plate surface.
[0026] In addition, as another problem in the case of applying the technology of the above-mentioned patent document 7 to thin steel plates, it is known that there is the following problem: in steel plates with relatively thin plate thickness, especially thin steel plates with a plate thickness of less than 1.0 mm, when welding is performed by irradiating a laser beam to the butt joint, insufficient filling occurs in the weld due to burn-through, and the mechanical strength of the weld is deteriorated.
[0027] To address this problem, the inventors have re-examined the inclination angle disclosed in the above-mentioned Patent Document 7. As a result, it was found that in order to prevent burn-through in thin steel plates with a thickness of 3.0 mm or less, especially thin steel plates with a thickness of 1.0 mm that are prone to burn-through, the inclination angle θ of the cut surface to be butted against the vertical surface of the steel plate surface needs to be appropriately adjusted, specifically, it needs to be greater than 20°.
[0028] However, when the inclination angle θ is increased as described above, if the plate thickness increases and the width a of the cut surface in the longitudinal direction of the steel plate (equivalent to the width of the butt joint when the cut surfaces are overlapped in a bevel joint) increases, another problem occurs that a melt residue is generated at the butt joint of the cut surface (for “melt residue”, refer to the following). Figure 6 (b)). Therefore, in order to completely prevent the above-mentioned molten residue, it is preferred that the minimum molten width w of the weld formed by laser beam welding is set to be at least 0.7 times the width a of the butted portion in the longitudinal direction of the steel plates, that is, the width of the cut surface of the butted steel plates in the longitudinal direction of the steel plates.
[0029] However, even if the inclination angle θ of the cut surface is the same, the thicker the plate thickness, the larger the width a of the cut surface to be butted in the longitudinal direction of the steel plate. Therefore, when the laser beam is irradiated only linearly, the minimum melting width w of the weld cannot be increased, and melting residues will be generated. In addition, if the laser output is increased to expand the melting width in order to prevent melting residues, sputtering will occur and welding defects will be easily generated.
[0030] Therefore, in the butt welding of the present invention, it is preferred to irradiate the butt joint to be welded while oscillating the laser beam in a spiral manner, thereby expanding the melting width. The oscillation of the laser beam makes the heat energy input to the welded portion uniform, thereby suppressing the occurrence of burn-through and sputtering.
[0031] The present invention is developed based on the above technical ideas.
[0032] Next, the butt laser beam welding method of the present invention will be specifically described with reference to the drawings.
[0033] First, in the welding method of the present invention, as described above, the butt end faces (cut faces) of two steel plates to be butt-welded need to be formed by laser cutting to have the same inclination angle θ with respect to the vertical plane of the steel plate surface.
[0034] Figure 1 Schematic diagrams showing an example of a laser cutting apparatus used for forming the above-mentioned cut surface, (a) is a perspective view showing the entire apparatus, and (b) is a side view seen from the cutting direction side.
[0035] like Figure 1As shown, the laser cutting processing device comprises: two laser oscillators 1a and 1b for oscillating laser beams; transmission systems 2a and 2b for transmitting the laser beams oscillated from the two oscillators; and processing heads 3a and 3b connected to the two transmission systems and irradiating the steel plates with laser beams for cutting processing. In addition, the two butted steel plates Sa and Sb are irradiated with laser beams 4a and 4b at an angle θ relative to the surface perpendicular to the steel plate surface from the processing heads 3a and 3b, respectively, to form cut surfaces 5a and 5b.
[0036] In addition, Figure 1 In the figure, the two processing heads 3a and 3b move in the directions da and db shown in the figure to cut the steel plate. The inclination angles θa and θb of the cut surfaces of the two steel plates need to be in the same direction and at the same angle in order to butt them together in a bevel joint. In addition, during the cutting process, it is preferred to spray auxiliary gases 6a and 6b from the processing heads 3a and 3b to prevent oxidation of the cut surfaces.
[0037] In addition, Figure 1 In the figure, a device for cutting two steel plates at a time using two laser beam cutting machines is shown. However, in order to reduce the equipment cost, the device can be simplified by setting a laser beam oscillator as one and using a beam splitting mirror, a semi-transparent filter, etc. to branch the laser beam into two (simultaneous two branches), or irradiating the laser beam from two processing heads at different times (temporal branching), thereby cutting two steel plates at a time. In addition, two steel plates can also be cut by using one laser beam cutting machine to perform two cuts.
[0038] In addition, in the welding method of the present invention, the cut surfaces of the two steel plates are formed by having the inclination angles θa and θb (it should be noted that the above θa and θb are also referred to as “θ”) relative to the plane perpendicular to the surface of the steel plates as described above. Figure 2 As shown, the cut surfaces are overlapped so as to be in a bevel-joined state to form a butt joint 10, and then a filler is supplied to the butt joint and a laser beam is irradiated to perform welding.
[0039] Figure 3 Schematic diagrams showing an example of a laser beam welding device used for the above welding, (a) is a perspective view showing the whole device, and (b) is a side view seen from the welding progress direction side.
[0040] Figure 3The laser beam welding device comprises: a laser oscillator 1w for oscillating a laser beam; a transmission system 2w for transmitting the laser beam; and a processing head 3w for using the laser beam 1w to weld the two butted steel plates Sa and Sb, and a filler wire 9 is fed from a filler wire feeding device 7 disposed behind the processing head 3w to the butt joint of the two steel plates Sa and Sb via a feeding path 8, and a laser beam 4w is irradiated from the processing head 3w disposed above the butt joint, so that the butt joint and the filler wire are melted, thereby forming a weld 11. In addition, in Figure 3 In (b), for convenience of explanation, the filler wire 9 is shown to be fed from obliquely above. However, in the present invention, the feeding angle is not particularly limited as long as the filler wire can be effectively supplied to the butting portion.
[0041] At this time, the laser beam irradiated for the above welding is irradiated with the center of the butt joint portion of the cut surface of the butt joint steel sheet Sa and the butt joint steel sheet Sb as the target, but if Figure 3 As shown in (b), since the butted cut surfaces are formed obliquely relative to the vertical plane of the steel plate surface, the butted portion has a width a in the longitudinal direction of the steel plate, and the melting width required for welding becomes larger. Therefore, if the width a of the butted portion in the longitudinal direction of the steel plate becomes too large, the butted portion cannot be completely melted simply by irradiating the laser beam in a manner that moves the laser beam linearly in the welding direction.
[0042] Therefore, in the present invention, if Figure 4 As shown, it is preferred that the laser beam is rotated with the butting portion as the center, and the laser beam is irradiated to the butting portion while being swung so that the irradiation trajectory of the laser beam becomes a spiral shape.
[0043] In addition, there are various methods for swinging the laser beam, for example, Figure 5 As shown, a plurality of reflecting mirrors Ma and Mb may be built inside the machining head 3w, and the reflecting mirrors may be operated in conjunction with the movement of the machining head 3w in the welding direction dw to cause the laser beam 4w to oscillate.
[0044] In addition, the above Figure 3 The laser beam oscillator 1w of the laser beam welding device shown may be different from the oscillators 1a and 1b of the laser beam cutting device, but in order to simplify the device and reduce the equipment cost, it can also be shared with the oscillator of the laser beam cutting device.
[0045] Next, use the above Figure 1 The laser cutting processing device shown and Figure 3 The welding method of the present invention in which butt welding is performed using the laser beam welding device shown will be described.
[0046] Steel plate thickness t: 0.1~3.0mm
[0047] First, the plate thickness t of the thin steel plate to which the butt welding of the present invention is applied is set to be in the range of 0.1 to 3.0 mm. When it is less than 0.1 mm, even if the irradiation conditions of the laser beam are adjusted, it is difficult to prevent burn-through at the butt joint during welding. It is preferably 0.4 mm or more. On the other hand, when the plate thickness t exceeds 3.0 mm, since the cut surface to be butted is formed obliquely, the melting width required for welding becomes larger, and a high-output laser beam welding device is required. In addition, when the plate thickness t exceeds 3.0 mm, it is difficult to cause burn-through during welding, so there is no need to apply the present invention.
[0048] Furthermore, since the welding method of the present invention is excellent in preventing burn-through during welding, it is preferably applied to a steel plate of 1.0 mm or less in which burn-through is likely to occur in order to further obtain the above-mentioned effect.
[0049] In addition, the thickness of the two steel plates to be butt-welded is preferably the same, but as long as it is within the above thickness range, the difference in thickness between the two steel plates is within 1 / 3 of the thickness of the thicker steel plate. Figure 7 As shown, welding in this case is preferably performed with the center of the target position for laser beam irradiation and filler wire feeding being the center of the width of the cut surface of the steel plate on the thicker side.
[0050] Inclination angle θ of cut surface: more than 20° and less than 60°
[0051] In the butt welding method of the present invention, the angle θ of the cut surface of the steel plate to be butted relative to the vertical surface of the steel plate surface needs to be in the range of more than 20° and less than 60°. When the above-mentioned inclination angle θ is less than 20°, in steel plates with a plate thickness of less than 3.0 mm, especially steel plates with a thickness of less than 1.0 mm, since the overlapping width of the two steel plates at the butt joint is small, even if the cut surfaces are butted, it is easy to generate a gap between the steel plates and burn-through. On the other hand, when the inclination angle θ of the above-mentioned cut surface exceeds 60°, on the contrary, the width a of the butt joint formed by the overlap of the two steel plates becomes too large, and the melting width required for welding also becomes larger. Therefore, even if a high-output laser is used or the laser beam is oscillated, molten residues will remain in the butt joint after welding, resulting in a decrease in the soundness and mechanical strength of the weld. In addition, the preferred inclination angle θ is in the range of 25 to 45°.
[0052] In addition, the inclination angle θ of the two steel plates to be butted is preferably the same, but the difference between the two angles is allowed as long as it is within 10°. However, even in this case, the inclination angle θ of the two steel plates needs to be within the range of more than 20° and less than 60° of the present invention.
[0053] Width of butt joint: 3.0 mm or less
[0054] Even if the inclination angle θ of the cut surface of the steel plate to be butted is within the range of more than 20° and less than 60°, the thicker the steel plate is, the larger the width a of the butt joint of the cut surface in the length direction of the steel plate is. However, when the width a exceeds the irradiation width of the laser beam, even if the laser beam is swung to expand the irradiation range, molten residues will remain in the butt joint after welding. In addition, when the swing width of the laser beam is increased to increase the melting width, burn-through is more likely to occur. Not only that, a high-output laser is also required. Therefore, the width a of the butt joint in the length direction of the steel plate is less than 3.0 mm. Preferably less than 2.0 mm. In addition, from the viewpoint of preventing burn-through of the butt joint, the lower limit of the width a of the butt joint is preferably about 0.4 mm.
[0055] Laser beam swing width: less than 2.5 mm
[0056] Figure 6 Schematically shows a cross section of a welded portion formed by the laser beam welding method of the present invention. As described above, in the welding method of the present invention, Figure 6 As shown in (a), it is preferred that the minimum melting width w of the weld is set to be at least 0.7 times the width a of the butt joint. This is because when the minimum melting width w of the weld is less than 0.7 times the width a of the butt joint, as shown in Figure 6 As shown in (b), molten residue D is generated on both sides of the butt joint. In order to prevent this molten residue, the laser beam irradiated to the weld is made as follows: Figure 4 Swinging as shown is effective. However, when the swing width Lw is made too large, the input heat energy per unit area is reduced, resulting in a decrease in the welding speed. Therefore, when using a laser with a maximum output of about 10kW or less, the swing width Lw of the laser beam is preferably less than 2.5mm. Preferably, it is less than 1.0mm. In addition, the above-mentioned Lw refers to the center-to-center distance at the maximum amplitude of the laser beam. Therefore, for example, when the beam diameter of the laser is 0.5mm and the swing width Lw of the laser beam is 2.5mm, the irradiation width of the laser beam is 3.0mm. By the way, the melting width of the weld is related to the irradiation width of the above-mentioned laser beam, but it also depends on the output of the laser beam, the welding speed, and the thickness of the steel plate, so it may not be the same as the irradiation width.
[0057] In order to ensure a good penetration shape and prevent the generation of molten residue, it is preferred that the heat input per unit plate thickness and per unit welding length of the laser beam be set to 10000 kJ / m 2 above.
[0058] In addition, in the present invention, the cut surfaces of the two steel plates to be butted are in contact with each other, and the gap between the steel plates is basically 0 (zero). However, since there are concave and convex surfaces on the cut surface, it is impossible to be completely 0, but as long as the gap in the horizontal direction is less than 0.8 mm, it is allowed.
[0059] In addition, regarding the filler wire, in order to avoid the weld metal solidification and fracture in the subsequent plate passing process, it is preferred to use a filler wire with a low carbon content of 0.15 mass% or less and a tensile strength of 700 MPa or less. In addition, in order to prevent the thickness of the weld from becoming too thick, it is preferred to adjust the wire diameter and supply speed according to the plate thickness of the steel plate.
[0060] Example
[0061] Laser beam welding tests were conducted using thin steel plates having the composition shown in Table 1, with the balance being Fe and inevitable impurities, with a plate thickness of 0.20 mm, 0.60 mm, 1.20 mm, 1.60 mm, and 2.30 mm, and a plate width of 1000 mm. Specifically, Figure 1 The fiber laser cutting processing device with a maximum output of 10 kW is used to change the inclination angle θ relative to the vertical plane of the steel plate surface to 5°, 25°, 40°, 60° and 70°, and the longitudinal ends of two steel plates having the above-mentioned various components and plate thicknesses are cut to form a cut surface, and then the cut surfaces of the two steel plates are butted in an oblique joint shape to form a butt joint, and a Figure 3 The laser beam welding device shown in Table 2 supplies a filler wire to the butt joint and irradiates the laser beam to weld the two steel plates over the entire width. In addition, the laser used in the above welding uses a fiber laser with a maximum output of 10 kW and a beam diameter of 0.5 mm. The output and welding speed are varied as shown in Table 2 according to the plate thickness. In addition, in welding steel plates with a plate thickness of 1.20 mm or more, the irradiation trajectory is as follows: Figure 4 The laser beam was oscillated in a spiral manner as shown in Table 2, and the oscillation width was changed as shown in Table 2. In addition, for the filler wire, in order to prevent the weld metal from solidifying and causing breakage in the subsequent plate passing process, it is preferable to use a low-carbon wire. In this embodiment, a wire equivalent to YGW11 specified in JIS Z 3312: 2009 was used. In addition, as a reference example, the feed of the filler wire was not performed in a part of the welding.
[0062] [Table 1]
[0063] [Table 2]
[0064] Next, the welded portion of the two steel plates welded as described above was subjected to the following evaluation test.
[0065] [Appearance evaluation of welded parts]
[0066] The entire length of the weld was visually observed to check whether burn-through occurred or insufficient filling occurred.
[0067] [Evaluation of weld section]
[0068] Test pieces were collected from the weld start, center, and end of the weld, and the cross-sectional macroscopic structure photographs were taken using an optical microscope to measure the Figure 6 The minimum fusion width w of the weld section in the plate thickness direction and the thickness h of the weld center are shown, and the Figure 6 (b) Check whether there is any molten residue D remaining in the weld section. Figure 8 As shown, the thickness h at the center of the weld portion is the thickness of the weld metal at the center of the width of the minimum molten width w of the weld portion.
[0069] [Evaluation of strength characteristics of welded parts]
[0070] <Erickson test>
[0071] The 90 mm diameter sample was collected from the three locations of the weld start, center, and end of the weld so that the weld was included in the center. The Erichsen test (cup bulge test (opening test)) was carried out according to JIS Z 2247:2006. The case where no weld metal fracture occurred along the welding direction at any position was evaluated as acceptable (○), and the case where weld metal fracture occurred at least at one position was evaluated as unacceptable (×).
[0072] <Tensile test>
[0073] A No. 5 tensile test piece specified in JIS Z 2241:2011 was collected from three locations of the weld start, center, and end of the weld so that the weld was included in the center of the longitudinal direction of the parallel portion, and a tensile test was performed. The case where all the base materials were broken was evaluated as acceptable (○), and the case where at least one location was broken in a portion other than the base material was evaluated as unacceptable (×).
[0074] The results of the above evaluation tests are shown in Table 3. The followings were found from the results.
[0075] The welded portion welded under the conditions of the present invention does not generate burn-through, insufficient filling, or molten residue, and has excellent mechanical strength.
[0076] On the other hand, the welds No. 1, 6, 11, 16 and 21, whose inclination angle θ of the cut surface was smaller than the range of the present invention, had burn-through at the butt joint, resulting in insufficient filling and deterioration of mechanical strength.
[0077] On the contrary, the welds No. 5 and No. 10, whose inclination angle θ of the cut surface is larger than the range of the present invention, are thinner than 1.0 mm in thickness, so they still suffer from insufficient filling due to the occurrence of burn-through, and the mechanical strength is deteriorated. Similarly, the welds No. 15, 20, and 25, whose inclination angle θ is smaller than the range of the present invention, are thicker than 1.0 mm in thickness, so burn-through does not occur, but due to the large butt width, melt residues are generated in the welds, and the mechanical strength is deteriorated.
[0078] In addition, although the inclination angle θ of No. 24 is also within the range of the present invention, since the width of the butted portion exceeds 3.0 mm, melt residue is generated in the butted portion.
[0079] In addition, although melt residues were partially produced in No. 14 and No. 19, the extent was extremely slight and therefore had no effect on the results of the Erichsen test and the tensile test.
[0080] [Table 3]
[0081] Industrial Applicability
[0082] In the above description, laser beam welding of the tail end of a preceding coil and the front end of a succeeding coil at the entry side of a continuous processing line is taken as an example, but the technology of the present invention is not limited to the above welding, and for example, can also be appropriately used in the manufacture of tailor-welded plates.
[0083] Description of symbols 1a, 1b, 1w: Laser oscillator 2a, 2b, 2w: Transmission system 3a, 3b: Cutting head 3w: welding processing head 4a, 4b: Cutting laser beam 4w: Laser beam for welding 5a, 5b: Cutting groove (cutting part) 6a, 6b: Auxiliary gas 7: Filler wire supply device 8: Filler wire feeding section 9: Filler wire 10: Docking 11: Welding Department Sa, Sb: Steel plate θa, θb, θ: tilt angle da, db: Cutting direction dw: welding direction Ma, Mb: reflector t: Plate thickness a: Butt width h: Thickness at the center of the weld w: minimum melting width Lw: Laser beam swing width D: Melted residue.
Claims
1. A butt laser beam welding method, wherein after the cut surfaces of two steel plates having a thickness t of 0.1 to 3.0 mm are butted against each other, a filler is fed to the butt joint, and a laser beam is irradiated to the butt joint to melt the filler and the steel plates, thereby welding the two steel plates, wherein the butt laser beam welding method is characterized in that: The cut surfaces of the two steel plates are formed by laser cutting so as to have the same direction and an inclination angle θ of more than 20° and less than 60° relative to the vertical plane of the steel plate surface, and the width a of the cut surface in the longitudinal direction of the steel plate is less than 3.0 mm, and then, The cut surfaces of the two steel plates are butted and welded in a bevel-joined state.
2. The butt laser beam welding method according to claim 1, characterized in that: The minimum molten width w of the weld formed by the laser beam irradiation is set to be 0.7 times or more the width a of the cut surface in the longitudinal direction of the steel plate.
3. The butt laser beam welding method according to claim 1 or 2, characterized in that: The laser beam is irradiated with respect to the butted portion of the butted steel plates so that the irradiation trajectory becomes a spiral shape.
4. The butt laser beam welding method according to claim 3, characterized in that: The swing width b of the laser beam is set to 2.5 mm or less.
5. The butt laser welding method according to claim 4, characterized in that: The heat input per unit plate thickness and per unit welding length of the laser beam was set to 10000 kJ / m 2 above.
Citation Information
Patent Citations
Laser beam welding method for metallic strip
JP1991133587A
Laser welding machine
JP1996290281A
Method for manufacturing tailored blank material
JP2001205432A