Demolding film
By combining with a mold release film composed of an acrylic resin and a crosslinking agent without silicone, combined with a polyester resin base, the problems of increasing peeling force after heating and deformation of the resin sheet in the prior art are solved, and light peeling properties and High-speed peeling effect.
Patent Information
- Application Number
- CN202380032213.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-15
- Publication Date
- 2024-11-22
AI Technical Summary
The peeling force of the existing release film increases after heating, making it difficult to peel off at high speed, and may lead to deformation or damage of the resin sheet, and the performance of the long-chain alkyl-based release agent is not fully exerted.
A release film without silicone is used, which consists of acrylic resin, a crosslinking agent and a release agent. The ratio of acrylic resin to a crosslinking agent is 0.1≤a/b≤8.0, and the release agent and a crosslinking agent are The ratio is 0.1≤c/b≤12.0, the mass of the A-1 component of the acrylic resin exceeds 50%, and a laminated structure is formed on the substrate film, which consists of polyester resin and contains naphthalene dicarboxylic acid.
It has achieved light peeling properties before and after heating, and can maintain light release properties during high-speed peeling, suppress deformation and wrinkles of the mold release film, and ensure the uniform thickness and stable peeling force of the resin sheet.
Smart Images

Figure BDA0005068877800000041 
Figure BDA0005068877800000042 
Figure BDA0005068877800000061
Abstract
Description
Technical Field
[0001] The invention relates to a release film. Background Art
[0002] Release films formed by laminating a release layer on a substrate such as a polyethylene film are used for various purposes, such as structural components for batteries, protection of adhesive layers (protection for OCA (Optical Clear Adhesive) and protection for adhesive tapes), percutaneous absorption-type drug diaphragms in the medical field, process papers used in the manufacturing process of electronic components such as ceramic capacitors, and protection of components for image displays. To give a specific example, an adhesive sheet is composed of a substrate and an adhesive layer, and is used as a film for the manufacturing process of electronic components, etc. Before being used as a process film, the adhesive sheet is attached to the release film. In order to improve the demolding property, a release agent layer is provided on the surface of the release film (the contact surface with the adhesive layer). As constituent materials of the release agent layer, silicone-based release agents, fluorine-based release agents, and long-chain alkyl-based release agents can be listed.
[0003] Silicone-based mold release agents have excellent mold release properties. However, silicone components are easily transferred to the molded object, and silicone contamination causes malfunctions of electronic equipment, making them difficult to use in electronic components. Fluorine-based mold release agents have excellent mold release properties and heat resistance. However, they are expensive and have poor wettability. Long-chain alkyl-based mold release agents have better wettability than silicone-based and fluorine-based mold release agents. However, they may not have sufficient mold release properties.
[0004] Patent Document 1 (Japanese Patent Publication No. 2010-144046) discloses a release agent that can prevent the repulsion of an adhesive resin when it is applied to the release agent and thereby maintain good peeling performance from an adhesive resin film. The release agent comprises a poly(meth)acrylate as a main agent, wherein the poly(meth)acrylate comprises (A) a mono- or poly-alkylene glycol (meth)acrylate unit having an alkyl or aryl group as a terminal and (B) an alkyl (meth)acrylate unit having an alkyl group with 1 to 30 carbon atoms.
[0005] Patent Document 2 (Japanese Patent Application Laid-Open No. 2007-002092) discloses a release agent having a lighter release property than a silicone resin release agent and having no migration property, and comprises an active ingredient obtained by cross-linking a prepolymer obtained by copolymerizing at least an alkyl (meth)acrylate and a hydroxyalkyl (meth)acrylate with an isocyanate group-containing compound.
[0006] In Patent Document 3 (Japanese Patent Publication No. 2014-151481), a laminated polyester film is disclosed as a release polyester film with less degradation of release properties due to heat during processing, characterized in that at least one surface of the polyester film has a coating layer formed by a coating liquid containing a release agent and an active methylene-blocked isocyanate compound.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2010-144046
[0010] Patent Document 2: Japanese Patent Application Publication No. 2007002092
[0011] Patent Document 3: Japanese Patent Application Publication No. 2014-151481 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] However, the technique of Patent Document 1 has a large release force, and a release agent having a lighter release force is desired.
[0014] In addition, the technique of Patent Document 2 has a problem that the wettability of the release agent is insufficient. In the technique of Patent Document 3, the peeling force after heating is high and the increase in the peeling force due to heating cannot be sufficiently suppressed.
[0015] In the manufacturing process of electronic components, heat and pressure are sometimes applied to the release film. In this case, the long-chain alkyl release agent tends to increase its peeling force after heating. Furthermore, in the manufacturing process of the desired product, in order to further improve productivity, it is required to peel at a high speed. However, when peeling at a high speed, especially when peeling at a high speed after heating, the peeling force tends to increase. Moreover, even if peeling is possible, cohesive failure may occur in the release layer, and the components of the release layer may be transferred to the demolding object.
[0016] As described above, long-chain alkyl-based release agents have a problem in that they cannot fully exhibit their performance as release agents, and improvement of this problem has been demanded.
[0017] As another problem, when heat and pressure are applied to the release film, the release film itself may be deformed and wrinkled, etc. In this case, for example, when a resin sheet is formed on the release film, a resin sheet of uniform thickness is not formed, and therefore, the peeling force when the resin sheet is peeled off from the release film is not constant, and the resin sheet may be deformed or damaged.
[0018] As described above, conventional release films have a problem in that they cannot fully exhibit their performance, and improvement of this problem has been desired.
[0019] The present invention solves the above-mentioned technical problems and provides, for example, a release film having a light release force before and after heating and even when peeled at a high speed, having a high glass transition temperature, and containing substantially no silicone.
[0020] Solutions for solving problems
[0021] The present inventors have conducted intensive studies to solve the above-mentioned technical problems and have found that the above-mentioned object can be achieved by a release film having the following structure, thereby completing the present invention.
[0022] That is, the present invention includes the following configurations:
[0023] [1] A release film comprising a base film and a release layer,
[0024] The release layer comprises an acrylic resin (A), a crosslinking agent (B) and a release agent (C),
[0025] The acrylic resin (A) comprises a component A-1 represented by the following formula (1) and a component A-2 represented by the following formula (2),
[0026] The release layer does not substantially contain an organic silicon component, and the release layer is laminated on the substrate film.
[0027] The ratio a / b of the mass (a) of the acrylic resin (A) to the mass (b) of the crosslinking agent (B) contained in the release layer satisfies the formula (I),
[0028] The glass transition temperature of the resin constituting the substrate film is 100° C. or higher.
[0029] (I)0.1≤a / b≤8.0.
[0030]
[0031] In the formula (1), R1 represents (CnH2n+1) (n=an integer of 8 to 20), R4 represents H or CH3,
[0032]
[0033] In the formula (2), R2 represents (CmH2mOH) (m=an integer of 1 to 10) or H, and R4 represents H or CH3.
[0034] [2] In one embodiment, a release film is provided, wherein a ratio c / b of a mass (b) of a crosslinking agent (B) to a mass (c) of a release agent contained in a release layer satisfies the formula (II),
[0035] (II)0.1≤c / b≤12.0.
[0036] [3] In one embodiment, a release film is provided, wherein the mass of A-1 exceeds 50 parts by mass when the total mass of the components A-1 and A-2 of the acrylic resin (A) in the release layer is 100 parts by mass.
[0037] [4] In one embodiment, a release film is provided, wherein the release agent (C) contains a non-silicone-containing long-chain alkyl group and a reactive functional group and does not contain an acrylic group.
[0038] [5] In one embodiment, a release film is provided, wherein a normal peel force (PF1) at a peeling speed of 0.3 m / min. is 500 mN / 50 mm or less.
[0039] [6] In one embodiment, a release film is provided, wherein the release force (PF2) after heating (70°C, 20 hours) at a peeling speed of 0.3 m / min. is less than or equal to twice the normal release force (PF1).
[0040] [7] In one embodiment, a release film is provided, wherein the release force (PF3) after heating (70°C, 20 hours) at a peeling speed of 30 m / min. is 30 times or less of the normal peel force (PF1).
[0041] [8] In one embodiment, a release film is provided, wherein the base film is a film obtained by curing a composition containing a polyester resin, wherein the polyester resin contains naphthalene dicarboxylic acid as a dicarboxylic acid component.
[0042] [9] In one embodiment, a laminated film is provided, wherein an adhesive layer is laminated on at least one surface of the release film.
[0043] Effects of the Invention
[0044] According to the present invention, it is possible to provide a release layer film which has light release properties before and after heating and which maintains light release properties even when peeled at a high speed.
[0045] In addition, when heat and pressure are applied to the release film, the release film of the present invention can suppress deformation, wrinkles, etc. Moreover, for example, the peeling force when peeling the resin sheet from the release film can be kept constant, and the deformation and damage of the resin sheet can be prevented. Therefore, the resin sheet produced by the release film of the present invention can also be applied to electronic components, etc. DETAILED DESCRIPTION
[0046] The inventors have conducted intensive research and, as a result, the present invention relates to a release film comprising a substrate film and a release layer.
[0047] The release layer comprises an acrylic resin (A), a crosslinking agent (B) and a release agent (C),
[0048] The acrylic resin (A) comprises a component A-1 represented by the following formula (1) and a component A-2 represented by the following formula (2),
[0049] The release layer does not substantially contain an organic silicon component, and the release layer is laminated on the substrate film.
[0050] The ratio a / b of the mass (a) of the acrylic resin (A) to the mass (b) of the crosslinking agent (B) contained in the release layer satisfies the formula (I),
[0051] The substrate film is a film containing naphthalene dicarboxylic acid,
[0052] (I)0.1≤a / b≤8.0.
[0053]
[0054] In the formula (1), R1 represents (CnH2n+1) (n=an integer of 8 to 20), and R4 represents H or CH3.
[0055]
[0056] In the formula (2), R2 represents (CmH2mOH) (m=an integer of 1 to 10) or H, and R4 represents H or CH3.
[0057] (Base film)
[0058] The release film of the present invention comprises a substrate film and a release layer disposed on the surface of the substrate. When a release body is disposed on the release layer of the release film, the release body can be formed into the same shape as the substrate. In addition, the release layer and the release body are easily peeled off, so the shape of the release body can also be deformed into a desired shape and maintained. The release layer can be disposed on one surface of the surface of the substrate, or on both surfaces.
[0059] As the substrate film, a known substrate can be used. For example, as the substrate, a resin film formed of polyester such as polyethylene terephthalate and polyethylene naphthalate, polyolefin such as polypropylene, polyimide, etc. can be used. In particular, from the perspective of cost and productivity, a polyester film is preferred, and a polyethylene terephthalate and polyethylene naphthalate film is more preferred.
[0060] In one embodiment, the substrate film is a film cured from a composition containing a polyester resin, and the polyester resin contains naphthalene dicarboxylic acid as a dicarboxylic acid component. Although it should not be limited to a specific theory, by making the substrate film a film containing naphthalene dicarboxylic acid as a dicarboxylic acid component, even after heating at 70°C for 20 hours, it can show excellent dimensional stability, especially high surface smoothness, and the release layer of the present invention can also maintain surface smoothness. Since it is a release layer with high surface smoothness after heating, when peeling off a resin sheet from the release layer after heating at 70°C for 20 hours, for example, the resin sheet can be peeled off with a light peeling force. Furthermore, stable peeling properties can be exhibited at a wide range of peeling speeds from 0.3m / min. to 30m / min. of peeling speed. As such, since the substrate film after heating can maintain high surface smoothness, the peeling speed can be appropriately selected according to the manufactured resin sheet, and it can also contribute to the high-speed operation process of the resin sheet.
[0061] In one embodiment, in the polyester resin-containing composition, the polyester resin contains naphthalene dicarboxylic acid as a dicarboxylic acid component as a main component.
[0062] The thickness of the substrate is preferably 10 μm or more and 188 μm or less, and more preferably 25 μm or more and 100 μm or less. By making the thickness of the substrate 10 μm or more, it is possible to suppress deformation caused by heat during substrate production, processing, and molding. On the other hand, when the thickness of the substrate is 188 μm or less, the amount of the substrate discarded after use can be suppressed while satisfying the physical properties required by the substrate, and the burden on the environment can be reduced.
[0063] An easy-adhesion coating layer for improving adhesion may be disposed between the substrate and the release layer. In addition, a coating layer for imparting lubricity, heat resistance, antistatic properties, etc. may be disposed on the opposite side of the substrate to the side on which the release layer is disposed.
[0064] The average surface roughness (Sa) of the surface of the laminated release layer of the substrate film used in the present invention is preferably in the range of 1 to 50 nm, more preferably 2 to 30 nm. The maximum protrusion height (P) of the surface of the laminated release layer of the substrate film used in the present invention is preferably 2 μm or less, more preferably 1.5 μm or less. If Sa is 50 nm or less and P is 2 μm or less, the uneven thickness of the release layer can be suppressed and the smoothness of the surface of the release layer can be kept constant, thereby reducing the uneven thickness of the release body, and suppressing the possibility of the release body being broken starting from the thin part when it is peeled from the release film.
[0065] The average surface roughness (Sa) of the substrate film used in the present invention in the area opposite to the surface of the laminated release layer is preferably in the range of 10 to 100 nm, more preferably 2 to 30 nm. The maximum protrusion height (P) of the substrate film used in the present invention opposite to the surface of the laminated release layer is preferably 2 μm or less, more preferably 1.5 μm or less. If Sa is above 10 nm, the sliding property of the release surface and the reverse release surface is improved, and the winding property is excellent. In addition, if P is below 2 μm, the surface of the release layer will not be damaged during winding, and the possibility of a portion of the release layer being peeled off is reduced. Furthermore, the possibility of rupture starting from the portion where the release layer is peeled off when the release body is peeled off from the release film can be suppressed.
[0066] The haze of the substrate film used in the present invention is preferably 10% or less, more preferably 5% or less, and even more preferably 3% or less. If the haze is 10% or less, it is easy to perform appearance inspection when processing the release film, the adhesive layer on the release film, etc.
[0067] The substrate film in the present invention can use polyester film scraps and recycled materials from plastic bottles. In the present invention, since such film scraps and recycled materials from plastic bottles can be used, the environmental load can be greatly reduced. Moreover, in the form of including film scraps and recycled materials from plastic bottles, the improvement of the sliding property of the film and the easy discharge of air can also be maintained. The release layer of the present invention can appropriately recycle, process, and reuse polyester films used in various applications.
[0068] When such recycled raw materials (materials) are included, the particles may include particles of a size that causes the average surface roughness (Sa) of the area on the surface of the laminated release layer of the substrate film to be within the range of 1 to 50 nm. In addition, the particles may include particles of a size that causes the maximum protrusion height (P) on the surface of the laminated release layer of the substrate film to be less than 2 μm.
[0069] For example, the size of the particles of the substrate of the present invention may be within the range of (0.001 μm or more and 10 μm or less). If the particles have such a size range, the average surface roughness (Sa) and the maximum protrusion height (P) of the surface of the laminated release layer of the substrate film can be satisfied.
[0070] In one embodiment, the substrate has a surface layer substantially free of inorganic particles, and a release layer may be laminated on the surface layer.
[0071] The glass transition temperature of the resin constituting the substrate film used in the present invention is preferably 100°C or more, more preferably 110°C or more, and most preferably 115°C or more. When the temperature is above 100°C, when a resin sheet is formed on a release film, the release film itself will not deform even when heat or pressure is applied, and can maintain flatness, so a resin sheet with uniform thickness can be formed, which is preferred. When the temperature is above 115°C, a resin sheet with more uniform thickness can be formed without damaging the flatness of the film, which is particularly preferred. The glass transition temperature is, for example, below 150°C, below 140°C, or below 130°C. In one embodiment, the glass transition temperature of the resin constituting the substrate film is above 110°C and below 150°C, for example, above 115°C and below 140°C, or above 115°C and below 135°C.
[0072] (Release layer)
[0073] The release layer of the present invention is a release layer that contains an acrylic resin (A), a crosslinking agent (B) and a release agent (C) and does not substantially contain a silicone component. For example, the release layer can be formed by curing a release layer-forming composition containing an acrylic resin (A), a crosslinking agent (B) and a release agent (C).
[0074] (Acrylic resin)
[0075] The release layer of the present invention contains an acrylic resin (A).
[0076] In addition, the acrylic resin (A) contained in the release layer of the present invention preferably has a long-chain alkyl group. Although it has not yet been analyzed theoretically, it can be considered through repeated experiments that by making the acrylic resin (A) have a long-chain alkyl group, the release agent described later can be efficiently oriented on the surface of the release layer. In particular, the acrylic resin (A) involved in the present invention can, for example, show good wettability to the adhesive composition that forms the adhesive. Furthermore, for the release body such as the adhesive formed on the release layer, the acrylic resin (A) of the present invention can provide a release layer film that has light peeling properties before and after heating and maintains light release properties even when peeled at high speed.
[0077] In this way, the acrylic resin (A) can contribute to mold releasability in addition to functioning as a binder in the mold release layer. For example, the molecular weight of the acrylic resin (A) is preferably more than 500.
[0078] The acrylic resin of the present invention may further include a methacrylic resin, for example, a polymer of methyl methacrylate (MMA) or a copolymer thereof with acrylate.
[0079] It should be noted that, in the present invention, before heating refers to the conditions of temperature 22° C. and humidity 60%, and after heating refers to the state after heating for 20 hours at a temperature of 70° C. In addition, in the present invention, after heating may refer not only to the state immediately after heating, but also to the state after cooling to below the ambient temperature (e.g., below 40° C.).
[0080] In addition, the release layer of the present invention contains an acrylic resin (A) and does not substantially contain an organosilicon component. Therefore, it is possible to suppress the transfer of the organosilicon component to the demolding body, thereby, for example, preventing the demolding body from being contaminated by organosilicon, for example, avoiding malfunctions of electronic equipment caused by the demolding body. In this specification, "substantially containing no organosilicon component" means that an organosilicon component is not intentionally added to the components forming the release layer. For example, in the manufacturing process of the release layer, there is a possibility of containing a very small amount of organosilicon composition that may be accidentally present, etc. In view of such actual conditions, the amount of the organosilicon component contained in the release layer is preferably less than 0.1 parts by mass relative to 100 parts by mass of the release layer.
[0081] The acrylic resin (A) may be, for example, an acrylic polymer obtained by copolymerizing a long-chain alkyl acrylate, a graft polymer to which a long-chain alkyl group is grafted, or a block polymer to which a long-chain alkyl group is added at the terminal.
[0082] The acrylic resin (A) includes a component A-1 represented by the following formula (1) and a component A-2 represented by the following formula (2). In one embodiment, the acrylic resin (A) may be a cross-linked polymer containing the components A-1 and A-2.
[0083]
[0084] In the formula (1), R1 represents (CnH2n+1) (n=an integer of 8 to 20), and R4 represents H or CH3.
[0085]
[0086] In the formula (2), R2 represents (CmH2mOH) (m=an integer of 1 to 10) or H, and R4 represents H or CH3.
[0087] When the total mass of the components A-1 and A-2 of the acrylic resin (A) in the release layer is 100 parts by mass, the mass of A-1 is preferably more than 50 parts by mass. When the mass of A-1 exceeds 50 parts by mass, the release property of the release layer tends to be reduced, so it is preferred. The mass of A-1 is preferably more than 70 parts by mass, more preferably more than 80 parts by mass, and most preferably more than 90 parts by mass.
[0088] For example, the mass of A-1 may be 99 parts by mass or less, 96 parts by mass or less, or 92 parts by mass or less. In one embodiment, the mass of A-1 may be 85 parts by mass or less.
[0089] When the amount of the component A-1 is within the above range, the physical properties of the release layer can be maintained even before and after heating.
[0090] Therefore, the effects of the release layer of the present invention, such as the characteristics of having easy release properties both before and after heating and being able to maintain easy release properties even when peeled at high speed, can be more effectively exerted.
[0091] In the present invention, by setting the amount of the component A-1 within the above range, even when the release film of the present invention is stored for, for example, several days to several months after heating, the release film can be stored without significantly deteriorating the physical properties of the acrylic resin (A) before heating.
[0092] In the formula (1) representing the A-1 component, R1 is an alkyl group having a carbon number n of 8 or more and 20 or less. By making the carbon number n be 8 or more, the A-1 component can exhibit good demoulding properties, and can suppress the adhesiveness of the demoulding layer that may be caused by the alkyl group with a small number of carbon atoms. On the other hand, when the carbon number n is 20 or less, the softness of the A-1 component can be maintained, and the wettability of the coating surface of the demoulding layer can be fully ensured. The carbon number n is preferably 10 or more and 18 or less, and more preferably 10 or more and 16 or less. In one embodiment, in the formula (1), the carbon number n in R1 can be 10 or more and 15 or less.
[0093] In addition, R1 may be either linear or branched. When R1 is linear, the release property of the release layer tends to be reduced, which is preferred.
[0094] In the formula (1) representing the component A-1, R4 is H or CH3, either of which is suitable. As a raw material of the component A-1, a monomer represented by the following formula (7) can be used.
[0095]
[0096] In the formula (7), R1 represents (CnH2n+1) (n=an integer of 8 to 20), and R4 represents H or CH3.
[0097] Specific examples of the raw material for the component A-1 include lauryl (meth)acrylate and stearyl (meth)acrylate.
[0098] In R2 of formula (2) representing the A-2 component, the number of carbon atoms m is 1 to 10. When the number of carbon atoms m is 10 or less, the crosslinking density of the release layer of the present invention can be prevented from becoming sparse, the cohesive force of the release layer itself can be suppressed from becoming weak, and the peeling force can be suppressed from becoming heavy. The number of carbon atoms m is preferably 2 to 8, and more preferably 2 to 4.
[0099] In the formula (2) representing the component A-2, R4 is H or CH3, either of which is suitable. As a raw material of the component A-2, a monomer represented by the following formula (8) can be used.
[0100]
[0101] In the formula (8), R2 is (CmH2mOH) (m=an integer of 1 to 10) or H, and R4 represents H or CH3.
[0102] Specific examples of the raw material for the component A-2 include hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate.
[0103] (Crosslinking agent)
[0104] As the crosslinking agent (B) used in the formation of the release layer of the present invention, polyisocyanate, melamine, epoxy, aluminum chelate, titanium chelate, ultraviolet curable resin, or a mixture of two or more thereof can be used. Among them, by using melamine, the cured film is rigid and has excellent chemical resistance and weather resistance, so it is preferred. For crosslinking using aluminum chelate and titanium chelate, it is sometimes undesirable to contain metal components depending on the application.
[0105] In the present invention, the ratio a / b of the mass (a) of the acrylic resin to the mass (b) of the crosslinking agent contained in the release layer satisfies the formula (I):
[0106] (I)0.1≤a / b≤8.0
[0107] In one embodiment, the ratio a / b of the mass (a) of the acrylic resin to the mass (b) of the crosslinking agent is greater than or equal to 0.2 and less than or equal to 5.0, for example, greater than or equal to 0.2 and less than or equal to 4.0, may be greater than or equal to 0.2 and less than or equal to 3.0, or may be greater than or equal to 0.2 and less than or equal to 2.5. By making the ratio a / b of the mass (a) of the acrylic resin to the mass (b) of the crosslinking agent within the above range, the acrylic resin (A) and the acrylic resin (A) further added as needed are crosslinked by the crosslinking agent, and the elastic modulus of the release layer is improved, so that the peeling force can be further reduced. In addition, since the release component of the acrylic resin (A) oriented on the surface of the release layer is also fixed by the crosslinking agent after heating, the increase in the peeling force after heating is suppressed. If the ratio a / b of the mass (a) of the acrylic resin to the mass (b) of the crosslinking agent is less than or equal to 0.1, the release component of the acrylic resin (A) present on the surface of the release layer becomes less, so, for example, in the method of using the adhesive for the demolded body, the peeling force may become heavier.
[0108] In addition, when the ratio a / b of the mass of the acrylic resin (a) to the mass of the crosslinking agent (b) is 8.0 or more, the amount of the crosslinking agent decreases, so the acrylic resin (A) is not sufficiently crosslinked, and there is a concern that the release layer strength is insufficient, and the peeling force may increase. In addition, this problem tends to become more significant when peeling at a high speed.
[0109] As the melamine compound used in the release layer of the present invention, conventional compounds can be used without particular limitation. It is preferably obtained by condensing melamine and formaldehyde and having one or more triazine rings and methylol and / or alkoxymethyl groups in one molecule. Specifically, it is preferably a compound obtained by dehydration condensation reaction and etherification of a methylol melamine derivative obtained by condensing melamine and formaldehyde with methanol, ethanol, isopropanol, butanol, etc. as a lower alcohol. As methylolated melamine derivatives, for example, monomethylol melamine, dimethylol melamine, trimethylol melamine, tetramethylol melamine, pentamethylol melamine, hexamethylol melamine can be listed. One kind can be used, or two or more kinds can be used.
[0110] The melamine used in the present invention may be a commercial product. For example, CYMEL300, CYMEL301, CYMEL303LF, CYMEL350, CYMEL370N, CYMEL771, CYMEL325, CYMEL327, CYMEL703, CYMEL712, CYMEL701, CYMEL266, CYMEL267, CYMEL285, CYMEL232, CYMEL235, CYMEL236, CYMEL238, CYMEL272, CYMEL212, CYMEL253, CYMEL254, CYMEL202, CYMEL207 (Allnex) Japan Co., Ltd.), NIKALACMW-30M, NIKALACMW-30, NIKALACMW-30HM, NIKALACMW-390, NIKALACMW-100LM, NIKAL ACMA-1-750LM, NIKALACMW-22, NIKALACMS-21, NIKALACMS-11, NIKALACMW-24A-1, NIKALACMS-001, NIKALA CMA-1-002, NIKALACMA-1-730, NIKALACMA-1-750, NIKALACMA-1-708, NIKALACMA-1-706, NIKALACMA-1-042, NIKALACMA-1-035, NIKALAC, MA-1-45, NIKALACMA-1-43, NIKALACMA-1-417, NIKALACMA-1-410 (Nippon Carbide Co., Ltd.), etc. Among them, from the perspective of curability at low temperature / short time and adhesion to polyester film, fully ether-type methylated melamine resins are preferred. As commercially available products, CYMEL303LF, NIKALACMW-30, etc. can be listed.
[0111] In order to promote the crosslinking reaction of the melamine compound, an acid catalyst is preferably added to the release layer of the present invention, and an acid catalyst is preferably added to the release layer forming composition and applied to cure it. The acid catalyst used is not particularly limited, and an existing acid catalyst can be used, preferably a sulfonic acid catalyst.
[0112] As the sulfonic acid catalyst, for example, p-toluenesulfonic acid, xylenesulfonic acid, cumenesulfonic acid, dodecylbenzenesulfonic acid, dinonylnaphthalenesulfonic acid, trifluoromethanesulfonic acid and the like can be preferably used. In view of reactivity, p-toluenesulfonic acid can be particularly preferably used.
[0113] Sulfonic acid catalysts have higher acidity and better reactivity than other acid catalysts such as carboxylic acid catalysts, so the release layer can be processed at a lower temperature. Therefore, it is preferred because it can suppress the decrease in film planarity and deterioration in winding appearance caused by heat during processing.
[0114] The sulfonic acid catalyst used in the present invention may also be a commercial product. Examples of commercial products include DRYER (registered trademark) 900 (p-toluenesulfonic acid, manufactured by Hitachi Chemical Co., Ltd.), NACURE (registered trademark) DNNDSA series (dinonylnaphthalene disulfonic acid, manufactured by Kusumoto Chemicals Co., Ltd.), DNNSA series (dinonylnaphthalene (mono)sulfonic acid, manufactured by Kusumoto Chemicals Co., Ltd.), DDBSA series (dodecylbenzenesulfonic acid, manufactured by Kusumoto Chemicals Co., Ltd.), and p-TSA series (p-toluenesulfonic acid, manufactured by Kusumoto Chemicals Co., Ltd.).
[0115] (Release Agent)
[0116] In one embodiment, the release layer further comprises a release agent (C). The release agent (C) preferably contains a reactive functional group. Although it has not yet been analyzed theoretically, after repeated experiments, it is believed that the added release agent (C) is cross-linked with the acrylic resin (A) present near the surface of the release layer, and compared with the case of only the acrylic resin (A), the long-chain alkyl component is densely present near the surface of the release layer, thereby reducing the peeling force. In addition, the release agent (C) is also cross-linked after heating, so that it can be left on the surface of the release layer, so it can be considered that the rise of the peeling force can also be suppressed after heating.
[0117] In one embodiment, the release agent (C) contains a long-chain alkyl group and a reactive functional group that does not contain silicone, and further does not contain an acrylic group. In this way, by not containing silicone components and not containing acrylic groups, the long-chain alkyl group can be efficiently arranged on the surface of the release layer. In addition, it is speculated that if the substrate film is a film containing naphthalene dicarboxylic acid, the adhesion with the release layer becomes better, the adhesion between the substrate and the release layer can be improved, and further, stable peeling properties are exhibited at a wide range of peeling speeds from 0.3 m / min. to 30 m / min.
[0118] The release agent used in the present invention is preferably a compound that does not contain an acrylic group and further contains a long-chain alkyl group that does not contain silicone and a reactive functional group, preferably a low molecular weight polyolefin wax, a long-chain alkyl additive, a higher alcohol, etc. These structures may be linear or branched. Among these, two or more materials may be mixed and used.
[0119] The release agent used in the present invention is preferably a low molecular weight, preferably a molecular weight of 100 or more and 500 or less. By setting the molecular weight of the release agent within the above range, it can be easily oriented on the surface of the release layer, and the peeling force can be reduced. On the other hand, when the molecular weight is 100 or more, the release property of the release agent can be exerted, and the possibility of showing adhesion can be suppressed. In addition, when the molecular weight is 500 or less, the solubility of the release agent can be suppressed from decreasing, the flatness of the surface of the release film can be suppressed from decreasing, and the possibility of damage to the appearance of the obtained release body can be reduced.
[0120] (Low molecular weight polyolefin wax)
[0121] As the low molecular weight polyolefin wax, for example, low molecular weight wax such as polyethylene wax and polypropylene wax can be used.
[0122] (Long-chain alkyl additives)
[0123] As long-chain alkyl additives, additives other than acrylic resin (A) may be added. For example, low molecular weight additives having an alkyl chain such as Peeloyl 1010 and Peeloyl 1010S (both manufactured by Ipponda Oil & Fats Industry Co., Ltd.) may be used as appropriate. The above-mentioned demoulding additives are added in an amount that can exhibit the specified demoulding properties.
[0124] (Higher alcohol)
[0125] Examples of the higher alcohol include octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, hexadecanol, heptadecanol, stearyl alcohol, eicosanol, and behenyl alcohol as linear higher alcohols.
[0126] The number of carbon atoms of the higher alcohol is preferably 8 or more and 24 or less. When the number of carbon atoms is 8 or more, the release layer exhibits good release properties. When the number of carbon atoms is 24 or less, the solubility in the solvent is good, so the possibility of damaging the appearance of the coating film is reduced, which is preferred.
[0127] In one embodiment, the ratio c / b of the mass (b) of the cross-linking agent contained in the release layer to the mass (c) of the release agent satisfies the formula (II).
[0128] (II) 0.1 ≤ c / b ≤ 12.0
[0129] For example, as the addition amount of the release agent in the present invention, the ratio c / b of the mass (b) of the crosslinking agent to the mass (c) of the release agent may be 10.0 or less, preferably 7.0 or less, for example 5.0 or less, or 4.0 or less. In addition, the ratio c / b may be 0.15 or more, or 0.2 or more. In one embodiment, it may be 0.1≤c / b≤7.0, or 0.1≤c / b≤5.0.
[0130] By adjusting the ratio of release agent / crosslinking agent (c / b) within this range, the release agent components can be segregated to the surface of the release layer, thereby reducing the normal peeling force. Furthermore, since the release agent components oriented on the surface of the release layer are also fixed by the crosslinking agent after heating, the increase of the peeling force after heating and the high-speed peeling force after heating is suppressed.
[0131] On the other hand, when the ratio of release agent / crosslinking agent is 12.0 or more, the crosslinking agent is small, so the release component may not be retained on the surface of the release layer during heating, and the release force after heating may increase.
[0132] Although not limited to a specific theory, the release agent (C) can be used in combination with the acrylic resin (A) according to the present invention to prevent the release agent (C) from peeling off from the surface of the release layer and to provide sufficient film strength and releasability.
[0133] In one embodiment, the ratio a / c of the mass (a) of the acrylic resin contained in the release layer to the mass (c) of the release agent satisfies the formula (III).
[0134] (III) 0.1≤a / c≤7.0
[0135] For example, as the amount of the release agent added in the present invention, the ratio a / c of the mass (a) of the acrylic resin to the mass (c) of the release agent is preferably 5.0 or less, more preferably 3.0 or less, and most preferably 2.0 or less. In addition, the ratio a / c is preferably 0.3 or more, more preferably 0.5 or more, and most preferably 0.7 or more.
[0136] By adjusting the acrylic resin / release agent (a / c) within this range, the release agent component can be segregated to the surface of the release layer to reduce the normal peeling force. In addition, since the release agent component oriented on the surface of the release layer is fixed by the cross-linking agent even after heating, the increase of the peeling force after heating and the high-speed peeling force after heating is suppressed.
[0137] When the ratio of acrylic resin / releasing agent (a / c) is 0.1 or less, the amount of the releasing agent is too large, so the releasing agent is excessively segregated on the surface of the releasing layer, and a film having sufficient hardness cannot be obtained, which is not preferable.
[0138] Although not limited to a specific theory, the release agent (C) can be used in combination with the acrylic resin (A) of the present invention to prevent the release agent (C) from peeling off from the surface of the release layer and to provide sufficient film strength and releasability.
[0139] The release layer of the present invention may contain additives such as adhesion improvers and antistatic agents within a range that does not hinder the effects of the present invention. In addition, in order to improve adhesion to the substrate, it is also preferred to pre-treat the polyester film surface by anchor coating, corona treatment, plasma treatment, atmospheric pressure plasma treatment, etc. before providing the release coating.
[0140] The thickness of the release layer is preferably 0.01 μm to 10 μm, and more preferably 0.05 μm to 1 μm. When the thickness of the release layer is less than 0.01 μm, it is difficult to uniformly mold the release layer, and the peeling force may become unstable. On the other hand, when the thickness of the release layer exceeds 10 μm, the use ratio of recycled raw materials decreases, which is uneconomical and therefore not preferred.
[0141] The average surface roughness (Sa) of the release layer is preferably in the range of 1 to 50 nm, more preferably 2 to 30 nm. The maximum protrusion height (P) of the surface of the laminated release layer of the substrate film used in the present invention is preferably 2 μm or less, more preferably 1.5 μm or less. If Sa is 50 nm or less and P is 2 μm or less, the uneven thickness of the release layer can be suppressed, and the smoothness of the surface of the release layer can be kept constant, and the possibility of the release body being broken from the thin part when being peeled from the release film can be suppressed.
[0142] In addition, the rate of change of the average surface roughness (Sa) and the maximum protrusion height (P) of the region before and after heating is preferably within 20%, more preferably within 10%, and further preferably within 5%. If the rate of change of the average surface roughness (Sa) and the maximum protrusion height (P) of the region before and after heating is within 20%, the bonding area between the release layer and the molded object increases after heating, and the possibility of re-peeling due to the anchoring effect when the molded object is peeled from the release layer is low, so it is preferred.
[0143] In the present invention, the method for forming the release coating is not particularly limited, and the following method can be used: a coating liquid in which a release resin is dissolved or dispersed is spread on one surface of a polyester film of a substrate by coating, etc., and after removing the solvent by drying, etc., heating and drying, heat curing or ultraviolet curing is performed. At this time, the drying temperature during solvent drying and heat curing is preferably below 180°C, more preferably below 160°C, and most preferably below 140°C. The heating time is preferably below 30 seconds, more preferably below 20 seconds, and further preferably below 10 seconds. When it is below 180°C, the planarity of the film can be maintained, and the possibility of causing uneven thickness of the release layer is small, so it is preferred. When it is below 140°C, it can be processed without damaging the planarity of the film, and the possibility of causing uneven thickness of the release layer is further reduced, so it is particularly preferred.
[0144] In the present invention, the coating liquid for applying the release coating is not particularly limited, but preferably a solvent having a boiling point of 70°C or higher is added. By adding a solvent having a boiling point of 70°C or higher, bumping during drying can be prevented, the coating film can be leveled, and the planarity of the coating film surface after drying can be improved. As for the amount of addition, it is preferably added in an amount of about 50 to 99% by mass relative to the entire coating liquid.
[0145] As a coating method for the above-mentioned coating liquid, any known coating method can be applied, for example, a conventionally known method such as a roll coating method such as a gravure coating method, a reverse coating method, a rod coating method such as a wire bar method, a die coating method, a spray coating method, an air knife coating method, etc. can be used.
[0146] The normal peeling force, the peeling force after heating, and the peeling force at high-speed peeling after heating of the release film obtained in the present invention are preferably within the ranges shown below.
[0147] The release film obtained in the present invention may have a normal peel force (PF1) of 1000 mN / 50 mm or less, for example, 600 mN / 50 mm or less, or 500 mN / 50 mm or less at a peeling speed of 0.3 m / min. Although the explanation should not be limited to a specific theory, in the present invention, in addition to the feature that the release layer does not substantially contain an organosilicon component, the light peelability is derived by making the mass of A-1 exceed 50 parts by mass when the total mass of the A-1 component and the A-2 component of the acrylic resin (A) in the release layer is 100 parts by mass.
[0148] In one embodiment, the release film obtained in the present invention has a normal peel force (PF1) of 50 mN / 50 mm or more, for example, 80 mN / 50 mm or more at a peeling speed of 0.3 m / min.
[0149] If it is within the above range, the normal peeling force is light, so it is preferred. In particular, when the normal peeling force is 50 mN / 50 mm or more and 1000 mN / 50 mm or less, the possibility of the mold release body being peeled off during the conveying process is low, so it is preferred. When the peeling force before heating is 1000 mN / 50 mm or less, especially 500 mN / 50 mm or less, the possibility of the mold release body being deformed when peeling the mold release body is low, so it is preferred.
[0150] Normal peel force refers to normal peel force at a peeling speed of 0.3 m / min., and can be used to evaluate the peel force when peeling off a molded object, such as an adhesive (as an example, an acrylic adhesive tape (manufactured by Nitto Denko Corporation, No. 31B), etc.) disposed on the release layer of the present invention. In addition, the normal peel force can be measured at room temperature (25°C). The same peel force can also be applied to the molded object after heating.
[0151] In one embodiment, the peeling force (PF2) after heating (70°C, 20h) at a peeling speed of 0.3m / min. is less than 2 times the normal peeling force (PF1). If the peeling force (PF2) after heating is less than 2 times the normal peeling force, the peeling force after heating is low, so it is preferred. The peeling force (PF2) after heating is further preferably less than 1.9 times the normal peeling force (PF1), and most preferably less than 1.8 times. When the peeling force after heating is less than 2 times the normal peeling force, the molded body will not deform when the molded body is peeled after heating, so it is preferred.
[0152] Although the explanation should not be limited to a specific theory, in the present invention, in addition to the feature that the release layer does not substantially contain a silicone component, in particular, the mass of A-1 when the total mass of the A-1 component and the A-2 component of the acrylic resin (A) in the release layer is set to 100 parts by mass is greater than 50 parts by mass, thereby being able to maintain light peelability before and after heating.
[0153] In one embodiment, the peeling force (PF3) after heating (70°C, 20h) at a peeling speed of 30m / min. is 30 times or less of the normal peeling force (PF1). By having such a relationship, the high-speed peeling force after heating is low, so it is preferred. The peeling force (PF3) is further preferably 25 times or less of the normal peeling force (PF1), and most preferably 20 times or less. When the peeling force (PF3) is 30 times or less of the normal peeling force (PF1), the possibility of deformation of the demolding body when the demolding body is peeled at a high speed after heating is low, so it is preferred.
[0154] In the present invention, a laminated film can be obtained by providing an adhesive layer on at least one surface of a release film. The laminated film can be obtained, for example, by applying an adhesive composition to the surface of at least one side of the release film of the present invention, drying it as needed, and forming an adhesive layer on at least one side of the substrate. For example, the release layer may have an adhesive layer on the surface opposite to the substrate.
[0155] The present invention is applicable not only to adhesive sheets, but also to other uses such as structural members for batteries, adhesive layer protection (OCA (Optical Clear Adhesive) protection, adhesive tape protection, etc.), percutaneous absorption type drug diaphragms in the medical field, process papers used in the manufacturing process of electronic parts such as ceramic capacitors, and protection of image display members. It is expected that the same effect can be achieved.
[0156] Example
[0157] Hereinafter, the present invention will be described in more detail using examples, but the present invention is not limited to these examples. The characteristic values used in the present invention were evaluated by the following methods.
[0158] <Evaluation>
[0159] (Normal peel force (PF1))
[0160] An adhesive tape ("31B" manufactured by Nitto Denko Corporation) was pasted on the surface of the release film, and after being crimped using a crimping roller with a linear pressure of 5 kgf / mm, it was placed under conditions of a temperature of 22°C and a humidity of 60% for 20 hours. The release film with the adhesive tape pasted thereon was cut into rectangular strips of 25 mm in width and 150 mm in length. One end of the adhesive tape was fixed, and one end of the release film was held, and the side of the release film was stretched at a speed of 300 mm / min. to measure the T-peel strength. A tensile testing machine ("AUTOGRAPHAG-A-1" manufactured by Shimadzu Corporation) was used in the measurement. The results are shown in Table 1.
[0161] (Peel force after heating (PF2))
[0162] An adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B") was pasted on the surface of the release film, and after being crimped using a crimping roller with a line pressure of 5kgf / mm, the release film pasted with the adhesive tape was cut into rectangular strips of 25mm wide and 150mm long, and heated in an oven at a temperature of 70°C for 20 hours. Then, one end of the adhesive tape was fixed, one end of the release film was held, and the release film side was stretched at a speed of 300mm / min. to peel it off, and the T-peel strength was measured. A tensile tester ("AUTOGRAPHAG-A-1" manufactured by Shimadzu Corporation) was used in the determination of the T-peel strength. The results are shown in Table 1.
[0163] (High-speed peel force after heating (PF3))
[0164] An adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B") was pasted on the surface of the release film, and after being crimped using a crimping roller with a line pressure of 5kgf / mm, the release film with the adhesive tape was cut into rectangular strips of 25mm wide and 150mm long, and heated in an oven at a temperature of 70°C for 20 hours. Then, the release film side was fixed on a metal plate with a double-sided tape, and one end of the adhesive tape was held, and the adhesive tape side was stretched at a speed of 30m / min. to peel off, and the 180° peel strength was measured. A tensile tester ("High-speed Peel Tester TE-701" of TESTER SANGYO Co., Ltd.) was used in the determination of the 180° peel strength. The results are shown in Table 1.
[0165] (Silicone Migration)
[0166] An adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B") was pasted on the surface of the release film, and after being crimped using a crimping roller with a linear pressure of 5kgf / mm, the release film with the adhesive tape was cut into rectangular strips with a width of 25mm and a length of 150mm, and heated in an oven at a temperature of 70°C for 20 hours. Then, one end of the adhesive tape was fixed, one end of the release film was held, and the release film side was stretched at a speed of 300mm / min. to peel off, and the Si strength (I1) of the adhesive tape after peeling was measured. In addition, the Si strength (I0) of the adhesive tape not pasted on the surface of the release film was measured as a blank, and I1-I0 was calculated. When I1-I0>0, it is considered that there is migration of silicone, and the mobility is recorded as ×. When I1-I0=0, it is considered that there is no migration of silicone, and the mobility is recorded as ○. The results are shown in Table 1.
[0167] (Thin film planarity)
[0168] A film sample of 1m wide x 10m long cut from the center of the width direction of the release film is placed under a three-wavelength fluorescent lamp in such a way that the width direction of the film sample is parallel to the axial direction of the elongated three-wavelength fluorescent lamp, and then the reflected glare of the three-wavelength fluorescent lamp on the film sample is visually inspected. If heat wrinkles appear after heating the film sample at 150°C for 30 minutes, the image of the three-wavelength fluorescent lamp reflected on the film sample becomes chaotic or intermittent. The case where the image of the three-wavelength fluorescent lamp is roughly a straight line is judged as ○. In addition, the case where the image is slightly chaotic and / or intermittent is judged as △.
[0169] (Glass transition temperature)
[0170] The glass transition temperature (extrapolated onset temperature) of the polymer was measured using DSC (EXSTAR6000 manufactured by Seiko Instruments Co., Ltd.) at a sample amount of 10 mg and a temperature increase rate of 20° C. / min.
[0171] (Example 1)
[0172] (Preparation of acrylic resin (A1) and release layer coating liquid)
[0173] Stearyl acrylate (CH2=C(H)COOC 15 H 25 ) and hydroxyethyl acrylate (CH2=C(H)COOC2H4OH) in a ratio of 99:1, toluene is added so that the solid content concentration becomes 40 mass %, and 0.5 mol % of azobisisobutyronitrile (AIBN) is added under a nitrogen flow for copolymerization to obtain an acrylic resin (A1).
[0174] An acrylic resin (A1), a melamine resin (NIKALAC MW-30, manufactured by Nippon Carbide Co., Ltd.) as a crosslinking agent (B), a higher alcohol (pentadecanol, manufactured by Tokyo Chemical Industry Co., Ltd.) as a release agent (C), and p-toluenesulfonic acid (dryer #900, manufactured by Hitachi Chemical Polymer Co., Ltd.) as a curing catalyst were added in the amounts shown in Table 1, and a solvent (toluene / MEK=50 / 50: mass ratio) was further added to adjust the solid content concentration to 6.0 mass % to obtain a release layer coating liquid.
[0175] (Formation of Release Layer)
[0176] The obtained release layer coating liquid was coated on a PEN film using a gravure coater, and then dried at 130°C for 30 seconds to form a release layer with a thickness of 0.2 μm. The obtained release film was evaluated for normal peeling force, peeling force after heating, high-speed peeling force after heating, silicone migration, glass transition temperature, and film flatness.
[0177] (Examples 2 to 5, Comparative Examples 1 to 3)
[0178] A release layer was formed in the same manner as in Example 1 except that the composition was changed to that shown in Table 1. The obtained release film was evaluated for normal peel strength, heated peel strength, heated high-speed peel strength, silicone migration, glass transition temperature, and film planarity.
[0179] (Comparative Example 4)
[0180] (Preparation of acrylic resin (A4) and release layer coating liquid)
[0181] Toluene was added to methyl acrylate (CH2=C(H)COOCH3) so as to give a solid content concentration of 40% by mass, and 0.5 mol% of azobisisobutyronitrile (AIBN) was added under a nitrogen stream for copolymerization to obtain an acrylic resin (A4).
[0182] A release layer was formed in the same manner as in Example 1 except that the acrylic resin was changed to A4. The obtained release film was evaluated for normal peel strength, heated peel strength, heated high-speed peel strength, silicone migration, glass transition temperature, and film flatness.
[0183] (Comparative Example 5)
[0184] A release layer was formed in the same procedure as in Example 3 except that a thermosetting silicone-based release agent was used as a release agent together with a platinum catalyst. The obtained release film was evaluated for normal peel strength, peel strength after heating, high-speed peel strength after heating, silicone migration, glass transition temperature, and film flatness.
[0185] (Reference Example 6)
[0186] A release layer was formed in the same manner as in Example 1 except that a polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., E5100, thickness: 38 μm, surface roughness (Sa): 0.0365 nm (corona treated surface), surface maximum cross-sectional height (St): 3.72, haze: 3.7%) was used as a substrate film and the release layer coating liquid was applied to the corona treated surface. The obtained release film was evaluated for normal peeling force, peeling force after heating, high-speed peeling force after heating, silicone migration, glass transition temperature, and film planarity.
[0187] [Table 1]
[0188]
[0189] [Table 2]
[0190]
[0191] <Evaluation Results>
[0192] According to the present invention, it is possible to provide a release layer film which has light release properties both before and after heating and which maintains light release properties even when peeled at a high speed.
[0193] On the other hand, in Comparative Example 1, when the sum of the mass of the A-1 component and the A-2 component of the acrylic resin (A) is set to 100 parts by mass, the mass of A-1 does not exceed 50 parts by mass, so PF1 increases significantly, and the peeling force of PF2 increases significantly, so the release layer cannot be peeled off from the adhesive tape. In Comparative Example 2, since the amount of the cross-linking agent is too small, sufficient film strength cannot be obtained, PF1 and PF2 increase significantly, and PF3 is too large to peel off the release layer from the adhesive tape. In Comparative Example 3, since no release agent is contained, PF2 increases significantly, and the release layer cannot be peeled off from the adhesive tape. In addition, since Comparative Example 4 is composed of an acrylic resin that does not contain A-1 components and A-2 components, the release layer cannot be peeled off from the adhesive tape even at room temperature. In Comparative Example 5, since a silicone-based release agent is used, the migration of silicone is confirmed.
[0194] In Reference Example 6, since PET containing no naphthalene dicarboxylic acid was used as the base film, it was confirmed that the planarity of the film was slightly impaired compared with the present invention.
[0195] The embodiments and examples disclosed herein are illustrative in all aspects and are not restrictive. The scope of the present invention is indicated by the claims rather than the above embodiments, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0196] Industrial Applicability
[0197] The release film of the present invention is preferably used in applications such as electronic component production processes where it is difficult to use silicone release films.
Claims
1. A release film comprising a substrate film and a release layer, The release layer comprises an acrylic resin (A), a crosslinking agent (B) and a release agent (C), The acrylic resin (A) comprises a component A-1 represented by the following formula (1) and a component A-2 represented by the following formula (2), The release layer does not substantially contain an organic silicon component, and the release layer is laminated on the substrate film. The ratio a / b of the mass (a) of the acrylic resin (A) to the mass (b) of the crosslinking agent (B) contained in the release layer satisfies the formula (I), The glass transition temperature of the resin constituting the substrate film is 100° C. or higher. (I) 0.1≤a / b≤8.0; In formula (1), R 1 represents (CnH2n+1) (n=an integer of 8 to 20), R 4 Indicates H or CH 3 , In formula (2), R 2 represents (CmH2mOH) (m=an integer of 1 to 10) or H, R 4 Indicates H or CH 3 .
2. The release film according to claim 1, in, The ratio c / b of the mass (b) of the crosslinking agent (B) contained in the release layer to the mass (c) of the release agent satisfies the formula (II), (II)0.1≤c / b≤12.
0.
3. The release film according to claim 1 or 2, It is characterized in that When the total mass of the components A-1 and A-2 of the acrylic resin (A) in the release layer is 100 parts by mass, the mass of A-1 exceeds 50 parts by mass.
4. The release film according to claim 1, in, The release agent (C) contains a non-silicone-containing long-chain alkyl group and a reactive functional group, and does not contain an acrylic group. 5 . The release film according to claim 1 , which has a normal peel force (PF1) of 500 mN / 50 mm or less at a peeling speed of 0.3 m / min. 6 . The release film according to claim 1 , wherein the release force (PF2) after heating (70° C., 20 h) at a peeling speed of 0.3 m / min. is less than or equal to twice the normal peel force (PF1).
7. The release film according to claim 1, wherein the release force (PF3) after heating (70°C, 20h) at a peeling speed of 30 m / min. is 30 times or less of the normal peel force (PF1).
8. The release film according to claim 1, in, The substrate film is a film formed by curing a composition containing a polyester resin, wherein the polyester resin contains naphthalene dicarboxylic acid as a dicarboxylic acid component. 9 . A laminated film comprising: a pressure-sensitive adhesive layer laminated on at least one surface of the release film according to claim 1 .
Citation Information
Patent Citations
Film having releasability and production of the same film
JP2000159910A
Thermal curing release coating agent, release film and manufacturing method therefor
JP2018115224A