Resin composition, prepreg, resin sheet, laminate, metal foil-clad laminate, and printed wiring board

By combining dielectric powder, aromatic phosphorus compounds, and thermosetting resins, the dielectric loss problem of high dielectric constant and low dielectric loss tangent insulating layers in high-frequency electrical signal transmission is solved, and the peel strength and moisture absorption and heat resistance of printed circuit boards are improved, thereby enhancing the reliability and thermal characteristics of the circuit boards.

CN119013353APending Publication Date: 2024-11-22MITSUBISHI GAS CHEM CO INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032348.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing technologies struggle to reduce dielectric loss tangent while maintaining a high relative permittivity. Furthermore, the use of fillers can easily lead to interlayer delamination during laminate manufacturing, and insufficient hygroscopicity and thermal stability affect the reliability of printed circuit boards.

Method used

An insulating layer with high dielectric constant and low dielectric loss tangent is formed by using a resin composition containing dielectric powder, aromatic phosphorus compound and thermosetting resin, and by optimizing the proportion and particle size of each component, thereby enhancing the peel strength and moisture absorption and heat resistance of metal foil.

Benefits of technology

This technology reduces dielectric loss in high-frequency electrical signal transmission while improving the metal foil peel strength and moisture absorption and heat resistance of printed circuit boards, thereby enhancing the reliability and thermal characteristics of the circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005069626670000031
    Figure BDA0005069626670000031
  • Figure BDA0005069626670000032
    Figure BDA0005069626670000032
  • Figure BDA0005069626670000041
    Figure BDA0005069626670000041
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method suitable for manufacturing a semiconductor device having a high dielectric constant and a low dielectric loss tangent, the present invention relates to a resin composition for an insulating layer of a printed wiring board, the resin composition having high metal foil peel strength, excellent moisture absorption and heat resistance, and excellent thermal characteristics; and a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed wiring board, each of which is obtained using the resin composition. This resin composition contains a dielectric powder (A), an aromatic phosphorus compound (B), and a thermosetting resin (C).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed circuit board. Background Art

[0002] In recent years, the signal band of information communication equipment such as PHS and mobile phones, and the CPU clock time of computers have reached the GHz band and are being high-frequencyized. The dielectric loss of the electric signal is proportional to the square root of the relative dielectric constant of the insulating layer forming the circuit, the dielectric loss tangent, and the product of the frequency of the electric signal. Therefore, the higher the frequency of the signal used, the greater the dielectric loss will become. Since the increase in dielectric loss will attenuate the electric signal and damage the reliability of the signal, in order to suppress this situation, the insulating layer needs to select a material with a small dielectric constant and dielectric loss tangent.

[0003] On the other hand, the insulating layer of the high-frequency circuit has requirements such as the formation of a delay circuit, impedance integration of the circuit board in the low-impedance circuit, densification of the wiring pattern, and composite circuitization with a built-in capacitor in the substrate itself, and sometimes there is a situation where the insulating layer is required to have a high dielectric constant. Therefore, some people have proposed electronic components using an insulating layer with a high dielectric constant and a low dielectric loss tangent (for example, patent document 1). The insulating layer with a high dielectric constant and a low dielectric loss tangent is formed by dispersing fillers such as ceramic powder and metal powder that has been subjected to insulation treatment in a resin.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2000-91717 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] Generally, in order to increase the relative dielectric constant of the insulating layer, it is required to mix a filler with a high relative dielectric constant, but at the same time, the dielectric loss tangent will also increase, so there is a problem that the transmission loss of the high-frequency signal will increase. Therefore, a material with a lower dielectric loss tangent while maintaining a high relative dielectric constant is required.

[0009] In addition, in the filler used to manufacture the insulating layer with high dielectric constant and low dielectric loss tangent, gaps may be generated depending on the filler mixed, and interlayer delamination may be caused during the manufacture of the laminated board. Therefore, there is also a problem of deterioration of thermal characteristics and dielectric characteristics (high dielectric constant and low dielectric loss tangent) in printed circuit boards, etc.

[0010] Furthermore, if the filler and resin are highly hygroscopic, the dielectric properties and manufacturability of the printed circuit board may deteriorate. If the insulating layer has low hygroscopic heat resistance, the moisture contained in the insulating layer will evaporate during reflow soldering, thereby generating gaps, which may cause interlayer delamination during the manufacture of the laminate. Therefore, in the field of electronic materials that require high reliability, an insulating layer with excellent hygroscopic heat resistance is required.

[0011] Furthermore, when the insulating layer is formed into a metal foil-clad laminate, sufficient metal foil peeling strength (for example, copper foil peeling strength) is required.

[0012] The present invention has been made to solve the above-mentioned problems, and its object is to provide a resin composition suitable for producing an insulating layer of a printed wiring board having a high dielectric constant and a low dielectric loss tangent, and having high metal foil peel strength, excellent moisture absorption heat resistance, and excellent thermal characteristics, and a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed wiring board obtained by using the resin composition.

[0013] Solutions for solving problems

[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems in the prior art and, as a result, have found that a specific resin composition can solve the above-mentioned problems, thereby completing the present invention.

[0015] That is, the present invention is as follows.

[0016] [1] A resin composition comprising a dielectric powder (A), an aromatic phosphorus compound (B), and a thermosetting resin (C).

[0017] [2] The resin composition according to [1], wherein the dielectric powder (A) contains one or more selected from the group consisting of titanium dioxide, barium titanate, calcium titanate, and strontium titanate.

[0018] [3] The resin composition according to [1] or [2], wherein the average particle size of the dielectric powder (A) is 0.1 to 5 μm.

[0019] [3] The resin composition according to any one of [1] to [3], wherein the content of the dielectric powder (A) is 50 to 500 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0020] [4] The resin composition according to any one of [1] to [4], wherein the aromatic phosphorus compound (B) comprises one or more selected from the group consisting of phosphaphenanthrene compounds, aromatic phosphorus compounds represented by the following formula (1), aromatic phosphorus compounds represented by the following formula (2), aromatic phosphorus compounds represented by the following formula (3), and aromatic phosphorus compounds represented by the following formula (4).

[0021]

[0022] (In formula (1), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, X represents a divalent organic group, m each independently represents 0 or 1, and n represents 0 to 5. In formula (1), at least one R is an aryl group having 6 to 30 carbon atoms.)

[0023]

[0024] (In formula (2), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, X represents a divalent organic group, m each independently represents 0 or 1, and n represents 0 to 5. In formula (2), at least one R is an aryl group having 6 to 30 carbon atoms.)

[0025]

[0026] (In formula (3), A each independently represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and n represents an integer of 3 to 15.)

[0027]

[0028] (In formula (4), A represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms.)

[0029] [6] The resin composition according to [5], wherein the aromatic phosphorus compound represented by the formula (1) comprises one or more selected from the group consisting of an aromatic phosphorus compound represented by the following formula (6) and an aromatic phosphorus compound represented by the following formula (8).

[0030]

[0031] (In formula (6), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms.)

[0032]

[0033] (In formula (8), R represents an alkyl group having 1 to 4 carbon atoms, l represents an integer of 3 to 11, m represents an integer of 0 to 22, and n represents an integer of 1 to 10.)

[0034] [7] The resin composition according to any one of [1] to [6], wherein the content of the aromatic phosphorus compound (B) is 1 to 40 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0035] [8] The resin composition according to any one of [1] to [7], wherein the thermosetting resin (C) comprises one or more selected from the group consisting of cyanate compounds, maleimide compounds, epoxy compounds, phenol compounds, modified polyphenylene ether compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.

[0036] [9] The resin composition according to [8], wherein the maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (11), a maleimide compound represented by the following formula (12), and a maleimide compound represented by the following formula (13).

[0037]

[0038] (In formula (11), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1 to 10.

[0039]

[0040] (In formula (12), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and represents 1<n2≤5. )

[0041]

[0042] (In formula (13), Ra each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group. q represents an integer of 0 to 4. When q is an integer of 2 to 4, Ra may be the same or different in the same ring. Rb each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. r represents an integer of 0 to 3. When r is 2 or 3, Rb may be the same or different in the same ring. n represents the average number of repeating units and represents a value of 0.95 to 10.0.)

[0043]

[10] The resin composition according to [8] or [9], wherein the content of the maleimide compound is 15 to 85 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0044]

[11] The resin composition according to any one of [1] to

[10] , further comprising a filler different from the dielectric powder (A).

[0045]

[12] The resin composition according to

[11] , wherein the filler comprises one or more selected from the group consisting of silica, alumina, talc, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder.

[0046]

[13] The resin composition according to

[11] or

[12] , wherein the content of the filler is 50 to 300 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0047]

[14] The resin composition according to any one of [1] to

[13] , which is used for a printed wiring board.

[0048]

[15] A prepreg comprising a substrate and the resin composition according to any one of [1] to

[14] impregnated or coated on the substrate.

[0049]

[16] A resin sheet comprising the resin composition according to any one of [1] to

[14] .

[0050]

[17] A laminate comprising at least one selected from the group consisting of the prepreg described in

[15] and the resin sheet described in

[16] .

[0051]

[18] A metal foil-clad laminate comprising the laminate according to

[17] and a metal foil disposed on one or both surfaces of the laminate.

[0052]

[19] A printed circuit board comprising an insulating layer and a conductor layer disposed on one or both sides of the insulating layer,

[0053] The insulating layer contains a cured product of the resin composition according to any one of [1] to

[14] .

[0054] Effects of the Invention

[0055] According to the resin composition of the present invention, there can be provided a resin composition suitable for use in manufacturing an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent, and having high metal foil peel strength, excellent moisture absorption heat resistance, and excellent thermal properties, and a prepreg, a resin sheet, a laminate, a metal foil-clad laminate, and a printed circuit board obtained using the resin composition. DETAILED DESCRIPTION

[0056] The following is a detailed description of a method for implementing the present invention (hereinafter referred to as "this embodiment"). The following this embodiment is an example for illustrating the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented by appropriately deforming within the scope of its purpose.

[0057] In the present embodiment, unless otherwise specified, "resin solid content" or "resin solid content in the resin composition" refers to the resin component after removing the dielectric powder (A), filler, additives (silane coupling agent, wetting dispersant, curing accelerator, and other components), and solvent (solvent) in the resin composition. "100 parts by mass of resin solid content" or "100 parts by mass of the total resin solid content in the resin composition" means that the total of the resin component after removing the dielectric powder (A), filler, additives (silane coupling agent, wetting dispersant, curing accelerator, and other components), and solvent (solvent) in the resin composition is 100 parts by mass.

[0058] [Resin composition]

[0059] The resin composition of the present embodiment contains dielectric powder (A), an aromatic phosphorus compound (B), and a thermosetting resin (C).

[0060] In this embodiment, if the resin composition contains dielectric powder (A), aromatic phosphorus compound (B), and thermosetting resin (C), a cured product suitable for an insulating layer of a printed circuit board having a high dielectric constant and a low dielectric loss tangent, high metal foil peel strength, excellent moisture absorption heat resistance, and excellent thermal properties can be obtained. The reason for this is not yet clear, but the present inventors infer as follows.

[0061] That is, the cured product of the resin composition containing dielectric powder usually has a tendency to be excellent in heat resistance and electrical properties. However, in order to obtain this effect, it is necessary to mix a large amount of dielectric powder in the resin composition, but if the filling amount of the dielectric powder increases, there is a tendency for the relative dielectric constant and the dielectric loss tangent to increase. Therefore, the cured product obtained by such a resin composition has a tendency that the transmission loss of high-frequency signals increases.

[0062] In this regard, by the resin composition of the present embodiment containing dielectric powder (A) and aromatic phosphorus compound (B), the low dielectric loss tangent of aromatic phosphorus compound (B) can suitably suppress the rise of dielectric loss tangent produced by the filling amount of dielectric powder (A) becoming more. Therefore, it is possible to obtain a cured product having low dielectric loss tangent while maintaining a high relative dielectric constant. On this basis, by containing a thermosetting resin (C) in a resin composition, it is therefore possible to suitably suppress the deterioration of the glass transition temperature, thermal expansion coefficient, and metal foil peel strength caused by containing an aromatic phosphorus compound (B), and it is possible to obtain a cured product with excellent mechanical properties and heat resistance. But the reason is not limited thereto.

[0063] Next, each component contained in the resin composition will be described in detail.

[0064] <Dielectric powder (A)>

[0065] The resin composition of the present embodiment contains dielectric powder (A). The dielectric powder (A) may be used alone or in combination of two or more.

[0066] The shape of the dielectric powder (A) is not particularly limited, and examples thereof include: flaky, spherical, plate-like, and irregular shapes, etc. The shape is preferably spherical, from the perspective of being better dispersed with the aromatic phosphorus compound (B) and the thermosetting resin (C) described later, obtaining a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties, and obtaining an insulating layer having better metal foil peel strength.

[0067] The relative dielectric constant of the dielectric powder (A) is preferably 20 or more, more preferably 25 or more. If the relative dielectric constant is 20 or more, there is a tendency to obtain an insulating layer with a high relative dielectric constant. It should be noted that the relative dielectric constant of the dielectric powder (A) in the present embodiment is a value measured at 10 GHz using a cavity resonator method. In the present embodiment, the relative dielectric constant of the dielectric powder (A) can be calculated using the Bruggeman formula (composite rule). The specific method for measuring the relative dielectric constant can refer to the embodiments.

[0068] The dielectric loss tangent of the dielectric powder (A) is preferably less than 0.015, more preferably less than 0.010, and further preferably less than 0.008. If the dielectric loss tangent is less than 0.015, there is a tendency to obtain an insulating layer with a low dielectric loss tangent. In addition, in the present embodiment, the dielectric loss tangent of the dielectric powder (A) is a value at 10 GHz measured using a cavity resonance method. In the present embodiment, the dielectric loss tangent of the dielectric powder (A) can be calculated using the Bruggeman formula (composite rule). The specific method for measuring the dielectric loss tangent can refer to the embodiment.

[0069] From the viewpoint of dispersibility, the average particle size (D50) of the dielectric powder (A) is preferably 0.1 to 5 μm, more preferably 0.15 to 3 μm. It should be noted that in the present embodiment, the average particle size (D50) refers to the value when the volume of a predetermined amount of powder put into a dispersion medium is accumulated from small particles and reaches 50% of the total volume by measuring the particle size distribution using a laser diffraction-scattering particle size distribution measuring device. The average particle size (D50) can be obtained by measuring the particle size distribution using a laser diffraction-scattering method and calculating it. The specific measurement method can be referred to in the examples.

[0070] Examples of the dielectric powder (A) include titanium monoxide (TiO), barium titanate (BaTiO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), titanium trioxide (Ti2O3), and titanium dioxide (TiO2). Among these, the dielectric powder (A) preferably contains one or more selected from the group consisting of titanium dioxide, barium titanate, calcium titanate, and strontium titanate, from the perspective of having a higher relative dielectric constant and a more suitable dielectric loss tangent, being more well dispersed in the aromatic phosphorus compound (B) and the thermosetting resin (C), having a lower catalytic activity for the thermosetting resin (C), and having a better moldability. It is more preferable to contain strontium titanate from the perspective of having a higher relative dielectric constant and a more suitable dielectric loss tangent, being more well dispersed in the aromatic phosphorus compound (B) and the thermosetting resin (C), having a lower catalytic activity for the thermosetting resin (C), and having a better moldability. In addition, titanium oxide, titanium trioxide, and titanium dioxide are preferred as the dielectric powder (A) because they have a high relative dielectric constant and a suitable dielectric loss tangent.

[0071] As strontium titanate, known strontium titanate can be used, for example, oxides having a perovskite structure mainly represented by ABO3 can be mentioned. Strontium titanate may also contain (SrO) XA compound having a structure represented by TiO2 (0.9≤x<1.0, 1.0<x≤1.1). In the compound, a part of Sr may be replaced by other metal elements, such as at least one of La (lanthanum), Ba (barium), and Ca (calcium). In addition, in the compound, a part of Ti may be replaced by other metal elements, such as Zr (zirconium).

[0072] Titanium dioxide preferably has a rutile-type or anatase-type crystal structure, and more preferably has a rutile-type crystal structure.

[0073] As the dielectric powder (A), commercial products can be used. Examples of commercial products include STT-30A and EC-300 manufactured by Titanium Industry Co., Ltd., AEROXIDE (registered trademark, hereinafter the same) TiO2T805 manufactured by NIPPON AEROSIL Co., Ltd., and AEROXIDE TiO2T806 manufactured by NIPPON AEROSIL Co., Ltd. NKT90 (the above are trade names), etc.; as barium titanate, 208108 manufactured by ALDRICH Co., Ltd. (the above are trade names); as calcium titanate, CT series manufactured by Fuji Titanium Industry Co., Ltd.; as strontium titanate, ST-2 manufactured by KCM Corporation, ST-03 manufactured by Sakai Chemical Industry Co., Ltd., 396141 manufactured by ALDRICH Co., Ltd., ST, HST-1, HPST-1, HPST-2 manufactured by Fuji Titanium Industry Co., Ltd., SW-100, SW-50C, SW-100C, SW-200C, SW-320C, SW-350 (the above are trade names), etc. manufactured by Titanium Industry Co., Ltd.; as titanium trioxide, STR-100A-LP manufactured by Sakai Chemical Industry Co., Ltd., and MT-N1 manufactured by TAYCA Corporation (the above are trade names).

[0074] The content of the dielectric powder (A) is preferably 50 to 500 parts by mass, more preferably 60 to 450 parts by mass, and further preferably 70 to 400 parts by mass relative to a total of 100 parts by mass of the resin solid components in the resin composition. When the content of the dielectric powder (A) is within the above range, there is a tendency to obtain a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent), better moisture absorption heat resistance, and better thermal properties, and to obtain an insulating layer having better metal foil peel strength, so that the dielectric powder (A) is better dispersed with the aromatic phosphorus compound (B) and the thermosetting resin (C).

[0075] <Aromatic phosphorus compound (B)>

[0076] The resin composition of the present embodiment contains an aromatic phosphorus compound (B).

[0077] In the present embodiment, the aromatic phosphorus compound (B) is not particularly limited as long as it contains a phosphorus atom in its molecule and exhibits aromaticity. The aromatic phosphorus compound (B) may be used alone or in combination of two or more.

[0078] As the aromatic phosphorus compound (B), it is preferred to include at least one selected from the group consisting of a phosphaphenanthrene compound, an aromatic phosphorus compound represented by the following formula (1), an aromatic phosphorus compound represented by the following formula (2), an aromatic phosphorus compound represented by the following formula (3), and an aromatic phosphorus compound represented by the following formula (4). These aromatic phosphorus compounds tend to disperse the dielectric powder (A) better, be more compatible with the thermosetting resin (C), and obtain a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties, and to obtain an insulating layer having better metal foil peel strength.

[0079] Examples of the phosphaphenanthrene compound include 9,10-dihydro-9-oxa-10-phosphaphenanthrene 10-oxide and 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene 10-oxide. In addition, commercially available products may be used as the phosphaphenanthrene compound, examples of which include HCA, HCA-HQ, M-Ester, M-Acid, and SANKO (registered trademark)-BCA (these are trade names, Sanko Co., Ltd.).

[0080]

[0081] In formula (1), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms. X represents a divalent organic group. m each independently represents 0 or 1. n represents 0 to 5. In formula (1), at least one R is an aryl group having 6 to 30 carbon atoms.

[0082] The alkyl group having 1 to 30 carbon atoms in R is preferably an alkyl group having 1 to 20 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. The alkyl group having 3 or more carbon atoms may be linear or branched. Examples of such alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, neopentyl, n-hexyl, 2,3-dimethylbutyl (thexyl), n-heptyl, n-octyl, n-ethylhexyl, n-nonyl, and n-decyl.

[0083] The alkyl group having 1 to 30 carbon atoms in R is preferably at least one selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, and an n-butyl group, from the viewpoint that the dielectric powder (A) can be better dispersed, the thermosetting resin (C) can be better compatible, a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties can be obtained, and an insulating layer having better metal foil peel strength can be obtained.

[0084] As the aryl group having 6 to 30 carbon atoms in R, an aryl group having 6 to 20 carbon atoms is preferred, and an aryl group having 6 to 12 carbon atoms is more preferred. The aryl group may have a substituent. Examples of the substituent include a hydroxyl group, a sulfonic acid group; an alkyl group such as a methyl group, an ethyl group, and a propyl group; an alkoxy group such as a methoxy group, an ethoxy group, and a propoxy group; a nitro group; and an acyl group. Examples of such an aryl group include a phenyl group, a methylphenyl group (tolyl group), a xylyl group, an isopropylphenyl group, a tert-butylphenyl group, a di(tert-butyl)-phenyl group, a p-cumylphenyl group, a dicyclohexylphenyl group, a phenol group, a cyanophenyl group, a nitrophenyl group, a naphthylene group (naphthyl group), a methylnaphthyl group, a biphenyl group, an anthracene group, a tetraphenyl group, an anthracyl group, a pyrenyl group, a perylenyl group, a pentacene group, a benzopyrenyl group, phenyl group, pyrene group, thienyl group, and triphenylene group.

[0085] From the perspective of better dispersion of the dielectric powder (A), better compatibility with the thermosetting resin (C), a tendency to obtain a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and thermal properties, and a tendency to obtain an insulating layer having better metal foil peel strength, the aromatic group having 1 to 30 carbon atoms in R is preferably at least one selected from the group consisting of phenyl, tolyl, xylyl, and isopropylphenyl.

[0086] In formula (1), at least one R is an aryl group having 6 to 30 carbon atoms, preferably at least two Rs are aryl groups having 6 to 30 carbon atoms, more preferably at least three Rs are aryl groups having 6 to 30 carbon atoms, and further preferably four Rs are aryl groups having 6 to 30 carbon atoms.

[0087] X as a divalent organic group may or may not have a substituent. Examples of the substituent include an alkyl group, an alkoxy group, an alkylthio group, an aryl group, an aryloxy group, an arylthio group, a halogen atom, and a halogenated aryl group. The substituent may be a group formed by combining these substituents, or a group formed by bonding these substituents to heteroatoms such as oxygen atoms, sulfur atoms, and nitrogen atoms.

[0088] X is preferably a group derived from a divalent arylene group. As such a group, a divalent group derived from benzene, a divalent group derived from naphthalene, a divalent group derived from anthracene, and a divalent arylene group represented by the following formula (5) can be cited. These divalent groups may also have substituents. The substituents may also refer to the above. From the perspective of the tendency to obtain an insulating layer with a better metal foil peel strength, X is preferably a divalent group derived from benzene, a divalent group derived from naphthalene, and a divalent arylene group represented by formula (5), and more preferably a divalent group derived from benzene.

[0089]

[0090] In formula (5), A represents a direct bond, an alkylene group, an alkylidene group, a cycloalkylene group, a cycloalkylidene group, an arylalkylene group, or an arylalkylidene group.

[0091] Examples of the alkylene group include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, and a hexamethylene group. Among these, an alkylene group having 1 to 5 carbon atoms is preferred.

[0092] Examples of the alkylidene group include an ethylidene group and an isopropylidene group.

[0093] Examples of the cycloalkylene group include cyclopentanediyl, cyclohexanediyl, and cyclooctanediyl. Among these, cycloalkylene groups having 5 to 10 carbon atoms are preferred.

[0094] Examples of the cycloalkylidene group include a cyclohexylidene group, a 3,5,5-trimethylcyclohexylidene group, and a 2-adamantylidene group. Among these, a cycloalkylidene group having 5 to 10 carbon atoms is preferred, and a cycloalkylidene group having 5 to 8 carbon atoms is more preferred.

[0095] Examples of the aryl moiety of the arylalkylene group include aryl groups having 6 to 14 carbon atoms, such as phenyl, naphthyl, biphenylyl, and anthracenyl. The alkylene moiety can also be referred to as described above.

[0096] Examples of the aryl moiety of the arylalkylidene group include aryl groups having 6 to 14 carbon atoms, such as phenyl, naphthyl, biphenylyl, and anthracenyl. The same may be said of the alkylene moiety.

[0097] The divalent arylene group represented by formula (5) is preferably a divalent group derived from a dihydroxy compound such as 2,2'-dihydroxybiphenyl, 2,4'-dihydroxybiphenyl, 3,3'-dihydroxybiphenyl, 3,4'-dihydroxybiphenyl, 4,4'-dihydroxybiphenyl; bisphenol A, bisphenol TMC, 1,2-dihydroxynaphthalene, 1,3-dihydroxynaphthalene, 1,4-dihydroxynaphthalene, 1,5-dihydroxynaphthalene, 1,6-dihydroxynaphthalene, 1,7-dihydroxynaphthalene, 1,8-dihydroxynaphthalene, 2,3-dihydroxynaphthalene, 2,6-dihydroxynaphthalene, and 2,7-dihydroxynaphthalene.

[0098] At least one of m is preferably 1, more preferably two of m are 1, further preferably three of m are 1, and further preferably four of m are 1.

[0099] n is preferably an integer of 1-3.

[0100] The aromatic phosphorus compound represented by formula (1) may be a mixture of compounds having different n. In the case of a mixture, n is an average value of the mixture and is in the range of 0.5 to 3.

[0101] The aromatic phosphorus compound represented by formula (1) preferably contains one or more selected from the group consisting of an aromatic phosphorus compound represented by formula (6), an aromatic phosphorus compound represented by formula (7), such as resorcinol bis(diphenyl) phosphate, resorcinol bis(di(xylyl)) phosphate, bisphenol A bis(diphenyl) phosphate (BDP), biphenyl bis(diphenyl) phosphate, and an aromatic phosphorus compound represented by formula (8), and more preferably contains one or more selected from the group consisting of an aromatic phosphorus compound represented by formula (6) and an aromatic phosphorus compound represented by formula (8).

[0102]

[0103] In formula (6), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms.

[0104] The same may be said for the alkyl group having 1 to 30 carbon atoms and the aryl group having 6 to 30 carbon atoms. The alkyl group having 1 to 30 carbon atoms is preferably a methyl group, an ethyl group, an n-propyl group, and an n-butyl group. The aryl group having 6 to 30 carbon atoms is preferably a phenyl group, a tolyl group, a xylyl group, and an isopropylphenyl group.

[0105] The aromatic phosphorus compound represented by formula (6) is preferably an aromatic phosphorus compound represented by formula (7) from the perspectives that the dielectric powder (A) can be further dispersed, the compatibility with the thermosetting resin (C) can be further improved, a cured product having further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and further excellent moisture absorption heat resistance and further excellent thermal properties can be obtained, and an insulating layer having further excellent metal foil peel strength can be obtained.

[0106]

[0107] As the aromatic phosphorus compound represented by the formula (7), a commercially available product can be used, and examples thereof include PX-200 (trade name, Daihachi Chemical Industry Co., Ltd.).

[0108]

[0109] In formula (8), R represents an alkyl group having 1 to 4 carbon atoms. l represents an integer of 3 to 11. m represents an integer of 0 to 22. n represents an integer of 1 to 10.

[0110] The same may be said about the alkyl group having 1 to 4 carbon atoms. The alkyl group having 1 to 4 carbon atoms is preferably a methyl group, an ethyl group, an n-propyl group, or an n-butyl group.

[0111] l is an integer of 3 to 11, and forms a cyclic alkyl group. Examples of the cyclic alkyl group include cyclohexane, cyclooctane, cyclodecane, and cyclododecane.

[0112] m is preferably an integer of 0 to 10, more preferably an integer of 0 to 3, and even more preferably 0, 2, or 3.

[0113] n is preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and even more preferably 1 or 2.

[0114] The aromatic phosphorus compound represented by formula (8) is preferably an aromatic phosphorus compound represented by formula (9) from the perspectives that the dielectric powder (A) can be further dispersed, the compatibility with the thermosetting resin (C) can be further improved, a cured product having further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and further excellent moisture absorption heat resistance and further excellent thermal properties can be obtained, and an insulating layer having further excellent metal foil peel strength can be obtained.

[0115]

[0116] In formula (9), n represents an integer of 1 to 10. Preferably, n is an integer of 1 to 3.

[0117] As the aromatic phosphorus compound represented by the formula (9), a commercially available product can be used, and examples thereof include SR-3000 (trade name, Daihachi Chemical Industry Co., Ltd.).

[0118] As the aromatic phosphorus compound (B), it is preferred to include one or more selected from the group consisting of an aromatic phosphorus compound represented by formula (6) and an aromatic phosphorus compound represented by formula (8). In this case, the aromatic phosphorus compound represented by formula (6) and the aromatic phosphorus compound represented by formula (8) preferably contain 5% by mass or more in total, more preferably 10% by mass or more in total, further preferably 20% by mass or more in total, and further preferably 30% by mass or more in total in 100% by mass of the aromatic phosphorus compound (B). The upper limit is not particularly limited, and the total amount is 100% by mass or less, and the total amount may also be 90% by mass or less.

[0119]

[0120] In formula (2), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms. X represents a divalent organic group. m each independently represents 0 or 1. n represents 0 to 5. In formula (2), at least one R is an aryl group having 6 to 30 carbon atoms.

[0121] R, X, m, and n in the formula (2), including preferred embodiments, may refer to R, X, m, and n in the aromatic phosphorus compound represented by the formula (1), respectively.

[0122]

[0123] In formula (3), A each independently represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms. R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and n represents an integer of 3 to 15.

[0124] The same may be said about the alkyl group having 1 to 30 carbon atoms and the aryl group having 6 to 30 carbon atoms.

[0125] The alkyl group having 1 to 30 carbon atoms in A is preferably at least one selected from the group consisting of methyl, ethyl, n-propyl, and n-butyl. The aryl group having 6 to 30 carbon atoms in A is preferably at least one selected from the group consisting of phenyl, tolyl, xylyl, and isopropylphenyl.

[0126] The alkyl group having 1 to 30 carbon atoms in R is preferably at least one selected from the group consisting of methyl, ethyl, n-propyl, and n-butyl. The aryl group having 6 to 30 carbon atoms in R is preferably at least one selected from the group consisting of phenyl, tolyl, xylyl, and isopropylphenyl.

[0127] As the alkenyl group having 2 to 30 carbon atoms in A, an alkenyl group having 2 to 20 carbon atoms is preferred, and an alkenyl group having 2 to 10 carbon atoms is more preferred. The alkenyl group having 2 to 30 carbon atoms may be linear or branched. Examples of such alkenyl groups include vinyl, allyl, 4-pentenyl, isopropenyl, isopentenyl, 2-heptenyl, 2-octenyl, and 2-nonenyl. The alkenyl group having 2 to 30 carbon atoms in A is preferably one or more selected from the group consisting of vinyl, allyl, and isopropenyl. In addition, the alkenyl group having 2 to 30 carbon atoms in R is preferably one or more selected from the group consisting of vinyl, allyl, and isopropenyl.

[0128] Examples of the aromatic phosphorus compound represented by formula (2) include hexaphenoxycyclotriphosphazene and pentafluoro(phenoxy)cyclotriphosphazene.

[0129]

[0130] In formula (4), A represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms. Each R independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms.

[0131] The same may be said about the alkyl group having 1 to 30 carbon atoms, the alkenyl group having 2 to 30 carbon atoms, and the aryl group having 6 to 30 carbon atoms.

[0132] The alkyl group having 1 to 30 carbon atoms in A is preferably at least one selected from the group consisting of a methyl group, an ethyl group, an n-propyl group, and an n-butyl group. The alkenyl group having 2 to 30 carbon atoms in A is preferably at least one selected from the group consisting of a vinyl group, an allyl group, and an isopropenyl group. The aryl group having 6 to 30 carbon atoms in A is preferably at least one selected from the group consisting of a phenyl group, a tolyl group, a xylyl group, and an isopropylphenyl group.

[0133] The alkyl group having 1 to 30 carbon atoms in R is preferably at least one selected from the group consisting of methyl, ethyl, n-propyl, and n-butyl. The aryl group having 6 to 30 carbon atoms in R is preferably at least one selected from the group consisting of phenyl, tolyl, xylyl, and isopropylphenyl.

[0134] The content of the aromatic phosphorus compound (B) is preferably 1 to 40 parts by mass, more preferably 2 to 35 parts by mass, further preferably 5 to 32 parts by mass, further preferably 8 to 30 parts by mass, and further preferably 10 to 28 parts by mass relative to a total of 100 parts by mass of the resin solid components in the resin composition. When the content of the aromatic phosphorus compound (B) is within the above range, there is a tendency to further disperse the dielectric powder (A), further compatibility with the thermosetting resin (C), obtain a cured product having further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and further excellent moisture absorption heat resistance, and further excellent thermal properties, and obtain an insulating layer having further excellent metal foil peel strength.

[0135] The content of the aromatic phosphorus compound (B) in the resin composition is preferably 1 to 40 parts by mass, more preferably 2 to 37 parts by mass, further preferably 5 to 36 parts by mass, further preferably 10 to 35 parts by mass, further preferably 15 to 30 parts by mass, and may be 15 to 25 parts by mass, relative to 100 parts by mass of the total of the aromatic phosphorus compound (B) and the thermosetting resin (C), from the viewpoint of good compatibility with the aromatic phosphorus compound (B) and the thermosetting resin (C), a cured product having more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and more excellent moisture absorption heat resistance and thermal properties can be obtained, and an insulating layer having more excellent metal foil peel strength can be obtained.

[0136] <Thermosetting resin (C)>

[0137] The resin composition of the present embodiment contains a thermosetting resin (C).

[0138] The thermosetting resin (C) is not particularly limited as long as it is a thermosetting resin or compound. The thermosetting resin (C) may be used alone or in combination of two or more.

[0139] The thermosetting resin (C) preferably contains one or more selected from the group consisting of cyanate compounds, maleimide compounds, epoxy compounds, phenol compounds, modified polyphenylene ether compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group, more preferably contains one or more selected from the group consisting of maleimide compounds, cyanate compounds, phenol compounds, and epoxy compounds, and further preferably contains one or more selected from the group consisting of maleimide compounds, cyanate compounds, phenol compounds, and epoxy compounds, from the viewpoint that there is a tendency that the dielectric powder (A) is better dispersed, the aromatic phosphorus compound (B) is better compatible, a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties can be obtained, and an insulating layer having better metal foil peel strength can be obtained.

[0140] The content of the thermosetting resin (C) is preferably 1 to 98.5 parts by mass, more preferably 2 to 97 parts by mass, further preferably 3 to 93.5 parts by mass, further preferably 4 to 90 parts by mass, and further preferably 5 to 87 parts by mass relative to a total of 100 parts by mass of the resin solid components in the resin composition. When the content of the thermosetting resin (C) is within the above range, there is a tendency that the dielectric powder (A) is further well dispersed, the aromatic phosphorus compound (B) is further well compatible, a cured product having further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and further excellent moisture absorption heat resistance, and further excellent thermal properties can be obtained, and an insulating layer having further excellent metal foil peel strength can be obtained.

[0141] In the resin composition, the content of the thermosetting resin (C) is preferably 60 to 99 parts by mass, more preferably 63 to 98 parts by mass, further preferably 64 to 95 parts by mass, further preferably 65 to 90 parts by mass, and further preferably 70 to 85 parts by mass, based on 100 parts by mass of the total of the aromatic phosphorus compound (B) and the thermosetting resin (C), from the viewpoint of good compatibility with the aromatic phosphorus compound (B) and the thermosetting resin (C), a cured product having more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and more excellent moisture absorption heat resistance and thermal properties can be obtained, and an insulating layer having more excellent metal foil peel strength can be obtained.

[0142] (Cyanate ester compound)

[0143] The resin composition of the present embodiment may contain a cyanate compound.

[0144] As the cyanate compound, any known compound can be used as long as it has two or more cyanato groups (hereinafter also referred to as "cyanate ester group" or "cyanate group") directly bonded to an aromatic ring in one molecule. The cyanate compound can be used alone or in combination of two or more.

[0145] Examples of such cyanate compounds include phenol novolac type cyanate compounds, cresol novolac type cyanate compounds, naphthalene ring-containing novolac type cyanate compounds, allyl group-containing novolac type cyanate compounds, naphthol aralkyl type cyanate compounds, naphthylene ether type cyanate compounds, xylene resin type cyanate compounds, bisphenol M type cyanate compounds, bisphenol A type cyanate compounds, diallyl bisphenol A type cyanate compounds, bisphenol E type cyanate compounds, bisphenol F type cyanate compounds, biphenyl aralkyl type cyanate compounds, Cyanate compounds, bis(3,3-dimethyl-4-cyanatophenyl)methane, 1,3-dicyanatobenzene, 1,4-dicyanatobenzene, 1,3,5-tricyanatobenzene, 1,3-dicyanatonaphthalene, 1,4-dicyanatonaphthalene, 1,6-dicyanatonaphthalene, 1,8-dicyanatonaphthalene, 2,6-dicyanatonaphthalene, 2,7-dicyanatonaphthalene, 1,3,6-tricyanatonaphthalene, 4,4'-dicyanatobiphenyl, bis(4-cyanatophenyl)ether, bis(4-cyanatophenyl)sulfide and bis(4-cyanatophenyl)sulfone. In addition, these cyanate compounds may be prepolymers or polymers of cyanate compounds.

[0146] From the viewpoint that there is a tendency that the dielectric powder (A) can be dispersed more well, that the dielectric powder (A) is more compatible with the aromatic phosphorus compound (B), that a cured product having more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and having more excellent moisture absorption heat resistance and more excellent thermal properties can be obtained, and that an insulating layer having more excellent metal foil peel strength can be obtained, the cyanate ester compound preferably contains one or more selected from the group consisting of phenol novolac type cyanate ester compounds, naphthol aralkyl type cyanate ester compounds, naphthylene ether type cyanate ester compounds, xylene resin type cyanate ester compounds, bisphenol M type cyanate ester compounds, bisphenol A type cyanate ester compounds, diallyl bisphenol A type cyanate ester compounds, bisphenol E type cyanate ester compounds, bisphenol F type cyanate ester compounds, and biphenyl aralkyl type cyanate ester compounds, and prepolymers or polymers of these cyanate ester compounds, and more preferably contains one or more selected from the group consisting of naphthol aralkyl type cyanate ester compounds and bisphenol A type cyanate ester compounds.

[0147] Such a naphthol aralkyl type cyanate ester compound is more preferably a compound represented by formula (10).

[0148]

[0149] In formula (10), R 3 Each independently represents a hydrogen atom or a methyl group, preferably a hydrogen atom. In formula (1), n3 is an integer greater than 1, preferably an integer from 1 to 20, and more preferably an integer from 1 to 10.

[0150] As the bisphenol A type cyanate ester compound, one or more selected from the group consisting of 2,2-bis(4-cyanatophenyl)propane and a prepolymer of 2,2-bis(4-cyanatophenyl)propane may be used.

[0151] As such bisphenol A type cyanate compounds, commercially available products can be used, for example, Primaset (registered trademark) BADCy (trade name, Lonza Corporation, 2,2-bis(4-cyanatophenyl)propane, cyanate group equivalent: 139 g / eq.) and CA210 (trade name, Mitsubishi Gas Chemical Co., Ltd., a prepolymer of 2,2-bis(4-cyanatophenyl)propane, cyanate group equivalent: 139 g / eq.).

[0152] These cyanate compounds can also be produced according to known methods. As a specific production method, for example, the method described in Japanese Patent Application Laid-Open No. 2017-195334 (particularly paragraphs 0052 to 0057) can be cited.

[0153] The content of the cyanate compound is preferably 1 to 65 parts by mass, more preferably 2 to 60 parts by mass, further preferably 3 to 55 parts by mass, further preferably 4 to 50 parts by mass, further preferably 5 to 45 parts by mass, and particularly preferably 6 to 40 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. When the content of the cyanate compound is within the above range, there is a tendency that the dispersibility of the dielectric powder (A) and the compatibility with the aromatic phosphorus compound (B) are better, a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties can be obtained, and an insulating layer having better metal foil peel strength can be obtained.

[0154] (Maleimide compound)

[0155] The resin composition of the present embodiment may contain a maleimide compound.

[0156] As long as the maleimide compound has one or more maleimide groups in one molecule, known maleimide compounds can be used appropriately, and their types are not particularly limited. The number of maleimide groups in one molecule of the maleimide compound is more than 1, preferably more than 2. The maleimide compound can be used alone or in combination of two or more.

[0157] Examples of the maleimide compound include N-phenylmaleimide, N-hydroxyphenylmaleimide, bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, bis(3,5-dimethyl-4-maleimidephenyl)methane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, bis(3,5-diethyl-4-maleimidephenyl)methane, a maleimide compound represented by formula (11), a maleimide compound represented by formula (12), a maleimide compound represented by formula (13), prepolymers of these maleimide compounds, and prepolymers of the above maleimide compounds and amine compounds.

[0158] The maleimide compound is preferably a maleimide compound having an aromatic skeleton, and more preferably a maleimide compound selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-)-phenylene)imide, and bis(4-(4-)-phenylene)imide. The invention further comprises one or more of the group consisting of bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, maleimide compounds represented by formula (11), maleimide compounds represented by formula (12), and maleimide compounds represented by formula (13), and further preferably comprises one or more of the group consisting of bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, maleimide compounds represented by formula (12), and maleimide compounds represented by formula (13). From the perspective of obtaining a resin composition with a lower dielectric loss tangent, it is further preferred to include a maleimide compound represented by formula (13). In addition, from the perspective of obtaining a cured product with further excellent dielectric properties, hygroscopic heat resistance, and thermal properties, and obtaining an insulating layer with further excellent metal foil peel strength, it is preferred to include a maleimide compound represented by formula (12).

[0159] In the present embodiment, if the resin combination contains a maleimide compound with an aromatic skeleton, there is a tendency to obtain a more excellent dielectric property (high dielectric constant and low dielectric loss tangent) and a cured product with more excellent hygroscopic heat resistance and more excellent thermal properties, and to obtain an insulating layer with more excellent metal foil peel strength. The reason is not yet clear, but the present inventors speculate as follows. That is, it is speculated that if the resin combination contains a maleimide compound with an aromatic skeleton, it is more compatible with an aromatic phosphorus compound (B) and can be more well dispersed dielectric powder (A), so that the above effect can be obtained. However, the reason is not limited to this.

[0160]

[0161] In formula (11), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer of 1-10.

[0162]

[0163] In formula (12), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and 1 <n2≤5。

[0164] Examples of the alkyl group having 1 to 5 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, butyl, and pentyl; and branched alkyl groups such as isopropyl, isobutyl, sec-butyl, and tert-butyl.

[0165]

[0166] In formula (13), Ra each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group. q represents an integer of 0 to 4. When q is an integer of 2 to 4, Ra may be the same or different in the same ring. Rb each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. r represents an integer of 0 to 3. When r is 2 or 3, Rb may be the same or different in the same ring. n is the average number of repeating units, and represents a value of 0.95 to 10.0.

[0167] Examples of the alkyl group having 1 to 10 carbon atoms include, in addition to the alkyl group having 1 to 5 carbon atoms exemplified above, n-pentyl, isopentyl, neopentyl, n-hexyl, isohexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, isononyl, and n-decyl.

[0168] Examples of the alkoxy group having 1 to 10 carbon atoms include a methoxy group, an ethoxy group, an n-propoxy group, an n-butoxy group, an n-pentyloxy group, and an n-hexyloxy group.

[0169] Examples of the alkylthio group having 1 to 10 carbon atoms include a methylthio group and an ethylthio group.

[0170] Examples of the aryl group having 6 to 10 carbon atoms include phenyl, cyclohexylphenyl, phenol, cyanophenyl, nitrophenyl, naphthyl, biphenyl, anthracene, naphthacene, anthracyl, pyrenyl, peryl, pentacene, benzopyrene, phenyl group, pyrene group, and triphenylene group.

[0171] Examples of the aryloxy group having 6 to 10 carbon atoms include a phenoxy group and a p-tolyloxy group.

[0172] Examples of the arylthio group having 6 to 10 carbon atoms include a phenylthio group and a p-tolylthio group.

[0173] Examples of the cycloalkyl group having 3 to 10 carbon atoms include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, and a cycloheptyl group.

[0174] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0175] In the formula (13), Ra is preferably each independently an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms.

[0176] In formula (13), q is preferably 2 or 3, more preferably 2. It should be noted that the groups other than Ra directly bonded to the benzene ring are hydrogen atoms. That is, for example, when q is 0, all Ra represent hydrogen atoms.

[0177] In formula (13), preferably all Rb are hydrogen atoms. In addition, it is also preferred that: r is an integer of 1 to 3, and Rb is independently an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms. In addition, the group other than Rb directly bonded to the benzene ring is a hydrogen atom. That is, for example, when r is 0, all Rb represent hydrogen atoms.

[0178] The maleimide compound represented by formula (13) can be produced by a known method. As a specific production method, for example, the method described in WO2020 / 217679 can be mentioned.

[0179] The maleimide compound may be a commercial product or a product obtained by a known method. Examples of commercial products of the maleimide compound include BMI-70 (bis(3-ethyl-5-methyl-4-maleimidephenyl)methane), BMI-80 (2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane), and BMI-1000P (the above are trade names, K.I. Chemical Industry Co., Ltd.); BMI-3000, BMI-4000, BMI-5100, BMI-6000, BMI-7000, BMI-8000, BMI-9000, BMI-10000, BMI-10000, BMI-10001, BMI-10002, BMI-10003, BMI-10004, BMI-10005, BMI-10006, BMI-10007, BMI-10008, BMI-10009, BMI-1000A, BMI-1000A, BMI-1000A, BMI-1000A -7000, and BMI-2300 (the maleimide compound represented by the above formula (11)) (the above are trade names, Yamato Chemical Industry Co., Ltd.); MIR-3000-70MT (trade name, the maleimide compound represented by the above formula (12), Nippon Kayaku Co., Ltd.); NE-X-9470S (trade name, the maleimide compound represented by the above formula (13), DIC Corporation), etc.

[0180] The content of the maleimide compound is preferably 15 to 85 parts by mass, more preferably 20 to 80 parts by mass, and further preferably 25 to 75 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. By making the content of the maleimide compound within the above range, there is a tendency that the dispersibility of the dielectric powder (A) and the compatibility with the aromatic phosphorus compound (B) are better, a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties can be obtained, and an insulating layer having better metal foil peel strength can be obtained.

[0181] (Epoxides)

[0182] The resin composition of the present embodiment may contain an epoxy compound.

[0183] As long as the epoxy compound has one or more epoxy groups in one molecule, known epoxy compounds can be used appropriately, and the type thereof is not particularly limited. The number of epoxy groups in one molecule of the epoxy compound is 1 or more, preferably 2 or more. One epoxy compound may be used alone, or two or more epoxy compounds may be used in combination.

[0184] As the epoxy compound, conventionally known epoxy compounds and epoxy resins can be used. For example, biphenyl aralkyl epoxy resins, naphthalene epoxy resins, binaphthalene epoxy resins, multifunctional phenol epoxy resins, naphthylene ether epoxy resins, phenol aralkyl epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, xylene novolac epoxy resins, naphthalene skeleton modified novolac epoxy resins, dicyclopentadiene novolac epoxy resins, biphenyl novolac epoxy resins, phenol aralkyl novolac epoxy resins, naphthol aralkyl novolac epoxy resins, aralkyl novolac epoxy resins, aromatic hydrocarbon formaldehyde epoxy compounds, anthraquinone epoxy compounds, anthracene epoxy resins, naphthol aralkyl novolac epoxy resins, Oxygen compounds, dicyclopentadiene type epoxy resins, Xylok type epoxy compounds, bisphenol A type epoxy resins, bisphenol E type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol A novolac type epoxy resins, phenol type epoxy compounds, biphenyl type epoxy resins, aralkyl novolac type epoxy resins, triazine skeleton epoxy compounds, triglycidyl isocyanurate, alicyclic epoxy resins, polyol type epoxy resins, glycidyl amine, glycidyl ester resins, compounds obtained by epoxidizing double bonds of compounds containing double bonds such as butadiene, and compounds obtained by reacting hydroxyl-containing silicone resins with epichlorohydrin, etc.

[0185] From the perspectives of better dispersion of the dielectric powder (A), better compatibility with the aromatic phosphorus compound (B), a tendency to obtain a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties, and a tendency to obtain an insulating layer having better metal foil peel strength, the epoxy compound preferably includes one or more selected from the group consisting of biphenyl aralkyl type epoxy resins, naphthalene type epoxy resins, naphthylene ether type epoxy resins, and butadiene skeleton-containing epoxy resins, and more preferably includes one or more selected from the group consisting of naphthalene type epoxy resins and biphenyl aralkyl type epoxy resins.

[0186] The biphenyl aralkyl type epoxy resin is preferably a compound represented by the following formula (14).

[0187]

[0188] In the formula (14), ka represents an integer of 1 or more, preferably an integer of 1-20, and more preferably an integer of 1-10.

[0189] As the biphenyl aralkyl type epoxy resin, commercial products can be used, and products produced by a known method can also be used. Examples of commercial products include: NC-3000, NC-3000L, NC-3000H, and NC-3000FH (compounds represented by the above formula (14), wherein ka is an integer of 1 to 10) (the above are trade names, Nippon Kayaku Co., Ltd.) and the like.

[0190] As the naphthalene type epoxy resin, a compound represented by the following formula (15) is preferred.

[0191]

[0192] In formula (15), R 3b Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms (e.g., methyl or ethyl), an aralkyl group, a benzyl group, a naphthyl group, a naphthyl group containing at least one glycidyloxy group, or a naphthylmethyl group containing at least one glycidyloxy group, and n represents an integer greater than 0 (e.g., 0 to 2).

[0193] Examples of commercially available products of the compound represented by the above formula (15) include EPICLON (registered trademark) EXA-4032-70M (where n=0 in the above formula (15), and R 3b are all hydrogen atoms), EPICLON (registered trademark) HP-4710 (in the above formula (15), n=0, and R 3b is a naphthylmethyl group containing at least one glycidyloxy group) (the above are trade names, DIC Corporation).

[0194] The naphthylene ether type epoxy resin is preferably a bifunctional epoxy compound represented by the following formula (16) or a polyfunctional epoxy compound represented by the following formula (17), or a mixture thereof.

[0195]

[0196] In formula (16), R 13 Each independently represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms (for example, a methyl group or an ethyl group), or an alkenyl group having 2 to 3 carbon atoms (for example, a vinyl group, an allyl group, or a propenyl group).

[0197]

[0198] In formula (17), R 14 Each independently represents a hydrogen atom, an alkyl group having 1 to 3 carbon atoms (for example, a methyl group or an ethyl group), or an alkenyl group having 2 to 3 carbon atoms (for example, a vinyl group, an allyl group, or a propenyl group).

[0199] The naphthylene ether type epoxy resin may be a commercial product or a product produced by a known method. Examples of commercial products include HP-6000, EXA-7300, EXA-7310, EXA-7311, EXA-7311L, EXA7311-G3, EXA7311-G4, EXA-7311G4S, and EXA-7311G5 (the above are trade names, DIC Corporation). Among these, HP-6000 (trade name) is preferred.

[0200] The butadiene skeleton-containing epoxy resin may be any epoxy resin having a butadiene skeleton and an epoxy group in the molecule. Examples of such a resin include butadiene skeleton-containing epoxy resins represented by the following formulae (18) to (20).

[0201]

[0202] In formula (18), X represents an integer of 1 to 100, and Y represents an integer of 0 to 100.

[0203]

[0204] In formula (19), R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, a and b each independently represent an integer of 1 to 100, and c and d each independently represent an integer of 0 to 100. Examples of the alkyl group include methyl, ethyl, propyl, and butyl.

[0205]

[0206] In formula (20), e represents an integer of 24 to 35, and f represents an integer of 8 to 11.

[0207] The epoxy resin containing a butadiene skeleton may be a commercial product or a product produced by a known method. Examples of commercial products include: R-15EPT and R-45EPT (compounds in the above formula (18) where X=50 and Y=0) (these are trade names, Nagase ChemteX Co., Ltd.); Epolead (registered trademark) PB3600 and PB4700 (these are trade names, DAICEL Co., Ltd.); and Nippon Polybutadiene E-1000-3.5 (trade name, Shin Nippon Petrochemical Co., Ltd.).

[0208] The content of the epoxy compound is preferably 1 to 50 parts by mass, more preferably 10 to 45 parts by mass, and further preferably 20 to 40 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. When the content of the epoxy compound is within the above range, there is a tendency that the dispersibility of the dielectric powder (A) and the compatibility with the aromatic phosphorus compound (B) are better, a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better moisture absorption heat resistance and better thermal properties can be obtained, and an insulating layer having better metal foil peel strength can be obtained.

[0209] (Phenol compounds)

[0210] The resin composition of the present embodiment may contain a phenol compound.

[0211] As the phenol compound, any known phenol compound can be appropriately used as long as it has two or more phenolic hydroxyl groups in one molecule, and the type thereof is not particularly limited. The phenol compound can be used alone or in combination of two or more.

[0212] Examples of the phenolic compound include cresol novolac type phenolic resins, biphenyl aralkyl type phenolic resins represented by formula (21), naphthol aralkyl type phenolic resins represented by formula (22), aminotriazine novolac type phenolic resins, naphthalene type phenolic resins, phenol novolac resins, alkylphenol novolac resins, bisphenol A type novolac resins, dicyclopentadiene type phenolic resins, Xylok type phenolic resins, terpene-modified phenolic resins, and polyvinylphenols.

[0213] Among these, from the viewpoint of obtaining excellent moldability and surface hardness, preferably, at least one selected from the group consisting of cresol novolac type phenolic resin, biphenyl aralkyl type phenolic resin represented by formula (21), naphthol aralkyl type phenolic resin represented by formula (22), aminotriazine novolac type phenolic resin, and naphthalene type phenolic resin is preferred, and more preferably, at least one selected from the group consisting of biphenyl aralkyl type phenolic resin represented by formula (21) and naphthol aralkyl type phenolic resin represented by formula (22).

[0214]

[0215] In formula (21), R 4 Each independently represents a hydrogen atom or a methyl group, and n4 is an integer of 1-10.

[0216]

[0217] In formula (22), R 5 Each independently represents a hydrogen atom or a methyl group, and n5 is an integer of 1-10.

[0218] The content of the phenolic compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the phenolic compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0219] (Modified polyphenylene ether compound)

[0220] The resin composition of the present embodiment may contain a modified polyphenylene ether compound.

[0221] As long as part or all of the ends of the modified polyphenylene ether compound are modified, known modified polyphenylene ether compounds can be appropriately used without particular limitation. In addition, in this specification, the "modification" of the modified polyphenylene ether compound means that part or all of the ends of the polyphenylene ether compound are substituted with reactive functional groups such as carbon-carbon unsaturated double bonds. The modified polyphenylene ether compound can be used alone or in combination of two or more.

[0222] Examples of the polyphenylene ether compound involved in the modified polyphenylene ether compound include polymers containing at least one structural unit selected from the group consisting of the structural unit represented by formula (23), the structural unit represented by formula (24), and the structural unit represented by formula (25).

[0223]

[0224] In formula (23), R8, R9, R 10 and R 11 Each independently represents an alkyl group having 6 or less carbon atoms, an aryl group, a halogen atom or a hydrogen atom.

[0225]

[0226] In formula (24), R 12 , R 13 , R 14 , R 18 , R 19 Each independently represents an alkyl group having 6 or less carbon atoms or a phenyl group. 15 , R 16 , R 17 Each independently represents a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.

[0227]

[0228] In formula (25), R 20 , R 21 , R 22 , R 23 , R 24 , R25 , R 26 , R 27 Each independently represents a hydrogen atom, an alkyl group having no greater than 6 carbon atoms, or a phenyl group. -A- represents a linear, branched, or cyclic divalent hydrocarbon group having no greater than 20 carbon atoms.

[0229] Examples of -A- in formula (25) include divalent organic groups such as methylene, ethylidene, 1-methylethylidene, 1,1-propylidene, 1,4-phenylenebis(1-methylethylidene), 1,3-phenylenebis(1-methylethylidene), cyclohexylidene, phenylmethylene, naphthylmethylene, and 1-phenylethylidene, but are not limited to these.

[0230] Preferred modified polyphenylene ether compounds include, for example, polyphenylene ether compounds in which a part or all of the terminals are modified with functional groups such as vinylbenzyl groups or other ethylenically unsaturated groups, epoxy groups, amino groups, hydroxyl groups, mercapto groups, carboxyl groups, methacryl groups, and silyl groups.

[0231] As a modified polyphenylene ether compound having a hydroxyl group at the end, SA90 (trade name, SABIC INNOVATIVE PLASTICS CO., LTD.) etc. are mentioned, for example.

[0232] As a modified polyphenylene ether compound having a methacryloyl group at the end, SA9000 (trade name, SABIC INNOVATIVE PLASTICS CO., LTD.) etc. are mentioned, for example.

[0233] The method for producing the modified polyphenylene ether compound is not particularly limited as long as the effects of the present invention can be obtained. For example, the modified polyphenylene ether compound can be produced by the method described in Japanese Patent No. 4591665.

[0234] The modified polyphenylene ether compound more preferably includes a modified polyphenylene ether compound having an ethylenically unsaturated group at the terminal. Examples of the ethylenically unsaturated group include alkenyl groups such as vinyl, allyl, acryloyl, methacryloyl, propenyl, butenyl, hexenyl, and octenyl; cycloalkenyl groups such as cyclopentenyl and cyclohexenyl; and alkenylaryl groups such as vinylbenzyl and vinylnaphthyl. Among them, vinylbenzyl is preferred.

[0235] The terminal ethylenically unsaturated group may be one or more and may be the same functional group or different functional groups.

[0236] The modified polyphenylene ether compound having an ethylenically unsaturated group at the end is preferably a compound represented by formula (26) from the perspective of being able to better disperse the dielectric powder (A), being better compatible with the aromatic phosphorus compound (B), being able to obtain a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and having better moisture absorption and heat resistance, and having better thermal properties, and being able to obtain an insulating layer having better metal foil peel strength.

[0237]

[0238] In formula (26), X represents an aromatic group, -(YO) m - represents a polyphenylene ether moiety. R1, R2, and R3 each independently represent a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, m represents an integer of 1 to 100, n represents an integer of 1 to 6, and q represents an integer of 1 to 4. m is preferably an integer of 1 to 50, and more preferably an integer of 1 to 30. In addition, n is preferably an integer of 1 to 4, and more preferably 1 or 2, and ideally 1. In addition, q is preferably an integer of 1 to 3, and more preferably 1 or 2, and ideally 2.

[0239] Examples of the aromatic group represented by X in formula (26) include a group obtained by removing q hydrogen atoms from one ring structure selected from a benzene ring structure, a biphenyl ring structure, an indene ring structure, and a naphthalene ring structure (e.g., a phenylene group, a biphenylene group, an indenylene group, and a naphthylene group). Among them, a biphenylene group is preferred.

[0240] Here, the aromatic group represented by X may include a diphenyl ether group in which an aryl group is bonded via an oxygen atom, a benzophenone group in which an aryl group is bonded via a carbonyl group, a 2,2-diphenylpropane group in which an aryl group is bonded via an alkylene group, and the like.

[0241] In addition, the aromatic group may be substituted with a common substituent such as an alkyl group (preferably an alkyl group having 1 to 6 carbon atoms, particularly a methyl group), an alkenyl group, an alkynyl group, a halogen atom, etc. However, since the aromatic group is substituted on the polyphenylene ether portion via an oxygen atom, the limit of the number of common substituents depends on the number of polyphenylene ether portions.

[0242] As the polyphenylene ether portion in formula (26), the structural unit represented by formula (23), the structural unit represented by formula (24), and the structural unit represented by formula (25) can be used. Among them, it is more preferable to contain the structural unit represented by formula (23).

[0243] In addition, as the modified polyphenylene ether compound represented by formula (26), the number average molecular weight is preferably 500 to 7000. In addition, a modified polyphenylene ether compound having a minimum melt viscosity of 50000 Pa·s or less in formula (26) can be used. From the perspective of better dispersion of the dielectric powder (A), better compatibility with the aromatic phosphorus compound (B), a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better hygroscopic heat resistance, and better thermal properties, and a tendency to obtain an insulating layer having better metal foil peel strength, a modified polyphenylene ether compound having a number average molecular weight of 1000 to 7000 and a minimum melt viscosity of 50000 Pa·s or less in formula (26) is more preferred.

[0244] The number average molecular weight is measured using a gel permeation chromatograph according to a predetermined method. The number average molecular weight is more preferably 1,000 to 3,000.

[0245] The minimum melt viscosity is measured using a dynamic viscoelasticity measuring device according to a predetermined method. The minimum melt viscosity is more preferably 500 to 50,000 Pa·s.

[0246] As the modified polyphenylene ether compound, in formula (26), a compound represented by the following formula (27) is preferred:

[0247]

[0248] In formula (27), X is an aromatic group, -(YO) m -and-(OY) m - each represents a polyphenylene ether moiety, and m represents an integer of 1 to 100. m is preferably an integer of 1 to 50, more preferably an integer of 1 to 30.

[0249] X, -(YO) in formula (27) m -, and m have the same meanings as in formula (26). -(OY) in formula (27) m - and -(YO) in formula (26) m - have the same meaning.

[0250] Preferably, X in formula (26) and formula (27) is formula (28), formula (29), or formula (30), and -(YO) in formula (26) and formula (27) m -and-(OY) m - is a structure in which the formula (31) or the formula (32) is arranged, or is a structure in which the formula (31) and the formula (32) are arranged in blocks or randomly.

[0251]

[0252]

[0253] In formula (29), R 28 , R 29 , R 30 and R 31 Each independently represents a hydrogen atom or a methyl group. -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0254] As specific examples of -B-, the same specific examples as those of -A- in formula (25) can be given.

[0255]

[0256] In formula (30), -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0257] As specific examples of -B-, the same specific examples as those of -A- in formula (25) can be given.

[0258]

[0259] The method for producing the modified polyphenylene ether compound having a structure represented by formula (27) is not particularly limited, and it can be produced, for example, by vinylbenzyl etherifying the terminal phenolic hydroxyl group of a bifunctional phenylene ether oligomer obtained by oxidative coupling of a bifunctional phenol compound and a monofunctional phenol compound.

[0260] As such a modified polyphenylene ether compound, a commercially available product can be used, and for example, OPE-2St1200 and OPE-2st2200 (these are trade names, Mitsubishi Gas Chemical Co., Ltd.) can be preferably used.

[0261] The content of the modified polyphenylene ether compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. By making the content of the modified polyphenylene ether compound within the above range, there is a tendency for the low dielectric loss tangent and reactivity to be further improved.

[0262] (Alkenyl-substituted nadic acid imide compound)

[0263] The resin composition of the present embodiment may contain an alkenyl-substituted nadic imide compound.

[0264] The alkenyl-substituted nadic acid imide compound is not particularly limited as long as it is a compound having one or more alkenyl-substituted nadic acid imide groups in one molecule. The alkenyl-substituted nadic acid imide compound may be used alone or in combination of two or more.

[0265] Examples of the alkenyl-substituted nadic acid imide compound include compounds represented by the following formula (33).

[0266]

[0267] In formula (33), R1 independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms (e.g., methyl or ethyl), and R2 represents an alkylene group having 1 to 6 carbon atoms, a phenylene group, a biphenylene group, a naphthylene group, or a group represented by formula (34) or (35).

[0268]

[0269] In formula (34), R3 represents methylene, isopropylidene, CO, O, S or SO2.

[0270]

[0271] In formula (35), R4 each independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.

[0272] The alkenyl-substituted nadic acid imide compound represented by formula (33) may be a commercially available product or a product produced by a known method. Examples of commercially available products include BANI-M and BANI-X (these are trade names, Maruzen Petrochemical Co., Ltd.).

[0273] The content of the alkenyl-substituted nadic acid imide compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the alkenyl-substituted nadic acid imide compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0274] (Oxetane resin)

[0275] The resin composition of the present embodiment may contain an oxetane resin.

[0276] The oxetane resin is not particularly limited, and a generally known oxetane resin can be used. The oxetane resin may be used alone or in combination of two or more.

[0277] Examples of the oxetane resin include oxetane, 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, alkyloxetanes such as 3,3-dimethyloxetane, 3-methyl-3-methoxymethyloxetane, 3,3-bis(trifluoromethyl)perfluorooxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (trade name, Toagosei Co., Ltd.), and OXT-121 (trade name, Toagosei Co., Ltd.).

[0278] The content of the oxetane resin is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and still more preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. When the content of the oxetane resin is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0279] (Benzoxazine compounds)

[0280] The resin composition of the present embodiment may contain a benzoxazine compound.

[0281] The benzoxazine compound is not particularly limited as long as it has two or more dihydrobenzoxazine rings in one molecule, and a generally known benzoxazine compound can be used. The benzoxazine compound can be used alone or in combination of two or more.

[0282] Examples of the benzoxazine compound include bisphenol A-type benzoxazine BA-BXZ, bisphenol F-type benzoxazine BF-BXZ, and bisphenol S-type benzoxazine BS-BXZ (these are trade names, Konishi Chemical Industries, Ltd.).

[0283] The content of the benzoxazine compound is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and even more preferably 10 to 30 parts by mass relative to 100 parts by mass of the total resin solid content in the resin composition. When the content of the benzoxazine compound is within the above range, there is a tendency for the adhesiveness, flexibility, etc. to be more excellent.

[0284] (Compound having a polymerizable unsaturated group)

[0285] The resin composition of the present embodiment may contain a compound having a polymerizable unsaturated group.

[0286] The compound having a polymerizable unsaturated group is not particularly limited, and generally known compounds can be used. The compound having a polymerizable unsaturated group can be used alone or in combination of two or more.

[0287] Examples of the compound having a polymerizable unsaturated group include vinyl compounds such as ethylene, propylene, styrene, divinylbenzene, and divinylbiphenyl; (meth)acrylates of monohydric or polyhydric alcohols such as methyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, polypropylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; epoxy (meth)acrylates such as bisphenol A epoxy (meth)acrylate and bisphenol F epoxy (meth)acrylate; and benzocyclobutene resins.

[0288] The content of the compound having a polymerizable unsaturated group is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, and further preferably 10 to 30 parts by mass relative to a total of 100 parts by mass of the resin solid content in the resin composition. By making the content of the compound having a polymerizable unsaturated group within the above range, there is a tendency for better adhesion, flexibility, etc.

[0289] <Thermoplastic elastomer>

[0290] The resin composition of the present embodiment may contain a thermoplastic elastomer.

[0291] The thermoplastic elastomer is not particularly limited as long as it is a thermoplastic elastomer. The thermoplastic elastomer may be used alone or in combination of two or more.

[0292] As a thermoplastic elastomer, a styrene-based elastomer and other thermoplastic elastomers other than a styrene-based elastomer are mentioned, for example.

[0293] Examples of the styrene-based elastomer include styrene-butadiene random copolymers, styrene-butadiene-styrene block copolymers, styrene-isoprene-styrene block copolymers, styrene-hydrogenated butadiene-styrene block copolymers, styrene-hydrogenated isoprene-styrene block copolymers, styrene-butadiene block copolymers, styrene-isoprene block copolymers, styrene-hydrogenated butadiene block copolymers, styrene-hydrogenated isoprene block copolymers, and styrene-hydrogenated (isoprene / butadiene) block copolymers.

[0294] As styrene (styrene unit) in the polystyrene block structure, styrene having a substituent may be used, and examples of such styrene include α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene.

[0295] In 100% by mass of the styrene elastomer, the styrene content in the styrene elastomer is preferably 10% by mass or more, more preferably 20% by mass or more. The upper limit of the styrene content is, for example, less than 100% by mass, preferably less than 99% by mass, and more preferably 70% by mass or less. In this specification, the styrene content refers to a value represented by (a) / (b)×100 (unit: mass %) when the mass of the styrene unit contained in the styrene elastomer is (a) g and the mass of the entire styrene elastomer is (b) g.

[0296] As the styrene-based elastomer, commercially available products may also be used. Examples of commercially available products include: TR2630 and TR2003 (the above are trade names, JSR Corporation) as styrene-butadiene-styrene block copolymers; SIS5250 (trade name, JSR Corporation) as a styrene-isoprene-styrene block copolymer; SEPTON (registered trademark) 2104 (KURARAY Co., Ltd.) as a styrene-hydrogenated isoprene-styrene block copolymer; and H-1043 (trade name, Asahi Kasei Corporation) as a styrene-hydrogenated butadiene-styrene block copolymer.

[0297] Examples of thermoplastic elastomers other than the styrene-based elastomer include polyisoprene, polybutadiene, butyl rubber, ethylene-propylene rubber, fluororubber, silicone rubber, hydrogenated compounds thereof, and alkyl compounds thereof.

[0298] The content of the thermoplastic elastomer is preferably 0.5 to 30 parts by mass, more preferably 1 to 25 parts by mass, further preferably 1.5 to 20 parts by mass, further preferably 2 to 15 parts by mass, and further preferably 3 to 10 parts by mass relative to a total of 100 parts by mass of the resin solid component in the resin composition. When the content of the thermoplastic elastomer is within the above range, there is a tendency to further disperse the dielectric powder (A), further compatibility with the aromatic phosphorus compound (B) and the thermoplastic resin (C), obtain a cured product having further excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and further excellent moisture absorption heat resistance, and further excellent thermal properties, and obtain an insulating layer having further excellent metal foil peel strength.

[0299] <Packing>

[0300] From the perspective of the tendency of dispersing the dielectric powder (A) better, obtaining a cured product having better dielectric properties (high dielectric constant and low dielectric loss tangent) and better hygroscopic heat resistance, and better thermal properties, and obtaining an insulating layer having better metal foil peel strength, the resin composition of the present embodiment preferably further comprises a filler different from the dielectric powder (A). The filler is not particularly limited as long as it is different from the dielectric powder (A). One filler may be used alone, or two or more fillers may be used in combination.

[0301] The relative dielectric constant of the filler is preferably less than 20, and more preferably not more than 15. In this embodiment, the relative dielectric constant of the filler can be measured and calculated by the same method as that of the dielectric powder (A).

[0302] The average particle size (D50) of the filler is preferably 0.10 to 10.0 μm, more preferably 0.30 to 5.0 μm. The average particle size (D50) of the filler can be calculated in the same manner as the average particle size (D50) of the dielectric powder (A).

[0303] Examples of fillers include silicon dioxide, silicon compounds (e.g., white carbon), metal oxides (e.g., aluminum oxide, molybdenum compounds (e.g., molybdic acid, zinc molybdates such as ZnMoO4 and Zn3Mo2O9, ammonium molybdate, sodium molybdate, potassium molybdate, calcium molybdate, molybdenum disulfide, molybdenum trioxide, molybdic acid hydrates, zinc ammonium molybdate hydrates such as (NH4)Zn2Mo2O9·(H3O)), zinc oxide, magnesium oxide, and zirconium oxide), metal nitrides (e.g., boron nitride, silicon nitride, and aluminum nitride), metal sulfates (e.g., barium sulfate), metal hydroxides (e.g., aluminum hydroxide, aluminum hydroxide heat-treated products (e.g., aluminum hydroxide is heated to reduce a portion of crystal water), boehmite, and magnesium hydroxide), and zinc compounds (e.g., zinc borate and zinc stannate). , clay, kaolin, talc, calcined clay, calcined kaolin, mica, E-glass, A-glass, NE-glass, C-glass, L-glass, D-glass, S-glass, M-glass G20, glass staple (including glass fine powders such as E glass, T glass, D glass, S glass, and Q glass), hollow glass, spherical glass, and inorganic fillers such as metal particles that have been insulatingly treated for metals such as gold, silver, palladium, copper, nickel, iron, cobalt, zinc, Mn-Mg-Zn series, Ni-Zn series, Mn-Zn series, carbonyl iron, Fe-Si series, Fe-Al-Si series, and Fe-Ni series; rubber powders such as styrene type, butadiene type, and acrylic type; core-shell type rubber powder; silicone resin powder; silicone rubber powder; organic fillers such as silicone composite powder.

[0304] Among these, the filler preferably contains one or more selected from the group consisting of silica, alumina, talc, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder, and more preferably contains one or more selected from the group consisting of silica, talc, and zinc molybdate.

[0305] The filler may also be a surface-treated filler having an inorganic oxide formed on at least a portion of the surface of the filler core particle. Examples of such fillers include surface-treated molybdenum compound particles (supported type) having an inorganic oxide formed on at least a portion of the surface of a core particle composed of a molybdenum compound.

[0306] Inorganic oxide is as long as it is given to at least a portion of the surface of the filler core particles. Inorganic oxide can be locally given to the surface of the filler core particles, or it can be given in a manner that covers the entire surface of the filler core particles. From the perspective of being able to obtain a cured product with more excellent dielectric properties (high dielectric constant and low dielectric loss tangent) and having more excellent hygroscopic heat resistance and more excellent thermal properties, being able to obtain an insulating layer with more excellent metal foil peel strength, inorganic oxide is preferably uniformly given in a manner that covers the entire surface of the filler core particles, i.e., uniformly forming a film of inorganic oxide on the surface of the filler core particles.

[0307] Examples of the surface-treated molybdenum compound particles (supported type) include particles obtained by surface-treating molybdenum compound particles using a silane coupling agent, or particles obtained by surface-treating the particles with an inorganic oxide by a sol-gel method or a liquid phase deposition method.

[0308] As inorganic oxide, preferably the one with excellent heat resistance, its kind is not particularly limited, more preferably metal oxide.Metal oxide can be listed, for example: SiO2, Al2O3, TiO2, ZnO, In2O3, SnO2, NiO, CoO, V2O5, CuO, MgO, and ZrO2, etc.These can be used alone or in combination of two or more.Among these, from the viewpoints of heat resistance, insulating properties, and cost, it is preferably selected from one or more of the group consisting of silicon dioxide (SiO2), titanium dioxide (TiO2), aluminum oxide (Al2O3), and zirconium dioxide (ZrO2).

[0309] As the surface-treated molybdenum compound particles, it is preferred that the inorganic oxide is imparted to at least a portion of the surface or the entire surface of the core particle composed of the molybdenum compound, that is, it is imparted to at least a portion of the periphery or the entire periphery of the core particle. In such surface-treated molybdenum compound particles, it is more preferred that silicon dioxide is imparted as an inorganic oxide to at least a portion of the surface or the entire surface of the core particle composed of the molybdenum compound, that is, it is imparted to at least a portion of the periphery or the entire periphery of the core particle. As the core particle composed of the molybdenum compound, it is more preferred to be one or more selected from the group consisting of molybdic acid, zinc molybdate, and zinc ammonium molybdate hydrate.

[0310] The thickness of the inorganic oxide on the surface can be appropriately set according to the desired performance, and there is no particular restriction. From the perspective of being able to form a uniform inorganic oxide coating, having better adhesion to the filler core particles, being able to obtain a cured product with better thermal properties, high glass transition temperature, low thermal expansion coefficient, low water absorption, and better dielectric properties (high dielectric constant and low dielectric loss tangent), being able to obtain an insulating layer with further excellent metal foil peel strength and further suitable surface hardness, its thickness is preferably 3 to 500 nm.

[0311] The average particle size (D50) of the surface-treated molybdenum compound particles is preferably 0.1 to 10 μm from the viewpoint of dispersibility in the resin composition. The average particle size (D50) of the surface-treated molybdenum compound particles can be calculated in the same manner as the average particle size (D50) of the dielectric powder (A).

[0312] The core particles composed of a molybdenum compound can be produced by various known methods such as a pulverization method and a granulation method, and the production method is not particularly limited. In addition, commercially available products can also be used.

[0313] The method for producing the surface-treated molybdenum compound particles is not particularly limited, and the surface-treated molybdenum compound particles are obtained by appropriately using various known methods such as sol-gel method, liquid phase deposition method, dip coating method, spray coating method, printing method, chemical plating method, sputtering method, evaporation method, ion plating method, and CVD method. The inorganic oxide or its precursor is imparted to the surface of the core particle composed of the molybdenum compound, thereby obtaining the surface-treated molybdenum compound particles. The method for imparting the inorganic oxide or its precursor to the surface of the core particle composed of the molybdenum compound can be any of a wet method and a dry method.

[0314] As a preferred method for producing surface-treated molybdenum compound particles, for example, the following method can be cited: a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides (alkoxysilanes) and aluminum alkoxides are dissolved, and a mixed solution of water, alcohol and a catalyst is added dropwise while stirring to hydrolyze the alkoxide, thereby forming a film of silicon oxide or aluminum oxide on the surface of the compound as a low-refractive index film, and then the obtained powder is separated from the solid and liquid, and heat-treated after vacuum drying. As other preferred production methods, for example, the following method can be cited: a molybdenum compound (core particle) is dispersed in an alcohol solution in which metal alkoxides such as silicon alkoxides and aluminum alkoxides are dissolved, and a mixing treatment is performed at high temperature and low pressure to form a film of silicon oxide or aluminum oxide on the surface of the compound, and then the obtained powder is vacuum dried and pulverized. By these methods, surface-treated molybdenum compound particles having a film of metal oxides such as silicon dioxide and aluminum oxide on the surface of the molybdenum compound can be obtained.

[0315] The content of the filler is preferably 50 to 300 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition. When two or more fillers are contained, the total amount may be within the above range.

[0316] <Silane coupling agent>

[0317] The resin composition of the present embodiment may contain a silane coupling agent. By containing a silane coupling agent, the resin composition has a tendency to further improve the dispersibility of the dielectric powder (A) in the resin composition and the filler compounded as needed, and to further improve the bonding strength between each component contained in the resin composition and the substrate described later. The silane coupling agent can be used alone or in combination of two or more.

[0318] The silane coupling agent is not particularly limited, and the silane coupling agent commonly used for the surface treatment of inorganic substances can be used. For example, aminosilane compounds (for example, 3-aminopropyl triethoxysilane, N-β-(aminoethyl)-γ-aminopropyl trimethoxysilane, etc.), epoxy silane compounds (for example, 3-glycidoxypropyl trimethoxysilane, etc.), acrylic silane compounds (for example, γ-acryloxypropyl trimethoxysilane, etc.), cationic silane compounds (for example, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyl trimethoxysilane hydrochloride, etc.), styryl silane compounds, phenyl silane compounds, etc. The silane coupling agent can be used alone or in combination of two or more. Among these, the silane coupling agent is preferably selected from one or more of the group consisting of epoxy silane compounds and styryl silane compounds. Examples of epoxysilane compounds include KBM-403 (trade name), KBM-303 (trade name), KBM-402 (trade name), and KBE-403 (trade name) of Shin-Etsu Chemical Co., Ltd. Examples of styrylsilane compounds include KBM-1403 (trade name), etc.

[0319] The content of the silane coupling agent is not particularly limited, and may be 0.1 to 5.0 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

[0320] <Wetting and dispersing agent>

[0321] The resin composition of the present embodiment may contain a wetting dispersant. The resin composition containing a wetting dispersant tends to further improve the dispersibility of the filler. The wetting dispersant may be used alone or in combination of two or more.

[0322] The wetting dispersant may be a known dispersant (dispersion stabilizer) for dispersing fillers, and examples thereof include DISPER BYK (registered trademark)-110, 111, 118, 140, 180, 161, 2009, 2055, 2152, 2155, W969, W996, W9010, and W903 (these are trade names) manufactured by BYK-Chemie Japan Co., Ltd.

[0323] The content of the wetting and dispersing agent is not particularly limited, but is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the total resin solid content in the resin composition.

[0324] <Curing accelerator>

[0325] The resin composition of the present embodiment may further contain a curing accelerator. The curing accelerator may be used alone or in combination of two or more.

[0326] Examples of curing accelerators include imidazoles such as triphenylimidazole (e.g., 2,4,5-triphenylimidazole); organic peroxides such as benzoyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, and di-tert-butyl peroxyphthalate; azo compounds such as azobisnitrile; N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2-N-ethylphenylaminoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethyl Tertiary amines such as butanediamine and N-methylpiperidine; phenols such as phenol, xylenol, cresol, resorcinol, and catechol; organic metal salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octoate, manganese octoate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, and iron acetylacetonate; substances obtained by dissolving these organic metal salts in hydroxyl-containing compounds such as phenol and bisphenol; inorganic metal salts such as tin chloride, zinc chloride, and aluminum chloride; organic tin compounds such as dioctyltin oxide, other alkyl tins, and alkyl tin oxides, etc. Among these, triphenylimidazoles such as 2,4,5-triphenylimidazole and manganese octoate tend to promote the curing reaction and increase the glass transition temperature, and are therefore preferred.

[0327] The content of the curing accelerator is not particularly limited, but may be 0.001 to 2.0 parts by mass, or 0.01 to 1.0 parts by mass, based on 100 parts by mass of the total resin solid content in the resin composition.

[0328] <Solvent>

[0329] The resin composition of the present embodiment may further contain a solvent. By containing a solvent, the resin composition has a tendency to further improve the viscosity decrease, the handling property (operability) and the impregnation property of the substrate during the preparation of the resin composition. One solvent may be used alone or in combination of two or more.

[0330] The solvent is not particularly limited as long as it can dissolve part or all of the components in the resin composition, and examples thereof include ketones (acetone, methyl ethyl ketone, etc.), aromatic hydrocarbons (e.g., toluene, xylene, etc.), amides (e.g., dimethylformamide, etc.), propylene glycol monomethyl ether and its acetate, etc.

[0331] <Other ingredients>

[0332] The resin composition of the present embodiment may contain components other than the above within the range that does not impair the desired properties. For example, flame retardant compounds include bromine compounds such as 4,4'-dibromobiphenyl, nitrogen-containing compounds such as melamine and benzoguanamine, and silicon compounds. In addition, various additives include ultraviolet absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, lubricants, defoamers, dispersants, leveling agents (surface adjusters), gloss agents, inhibitors, etc.

[0333] The content of other components is not particularly limited, but is usually 0.01 parts by mass or more and 10 parts by mass or less, respectively, relative to 100 parts by mass of the total resin solid content in the resin composition.

[0334] [Method for producing resin composition]

[0335] The manufacturing method of the resin composition of the present embodiment can be listed as follows: dielectric powder (A), aromatic phosphorus compound (B), thermosetting resin (C) and the above-mentioned components as needed are mixed and fully stirred. At this time, in order to uniformly dissolve or disperse each component, known treatments such as stirring, mixing, and kneading can be performed. Specifically, by using a stirring tank equipped with a stirrer with appropriate stirring capacity for stirring and dispersing treatment, the dispersibility of the dielectric powder (A) in the resin composition and the filler blended as needed can be improved. The above-mentioned stirring, mixing, and kneading treatment can be appropriately performed using a device for the purpose of mixing, such as a ball mill, a bead mill, or a known device such as a mixing device of a revolution or autogenous type.

[0336] In addition, when preparing the resin composition, a solvent can be used as needed to prepare a resin varnish. The resin varnish can be obtained by a known method. The resin varnish can be obtained, for example, by adding 10 to 900 parts by mass of an organic solvent to 100 parts by mass of a component in the resin composition from which the organic solvent has been removed, and performing the aforementioned known treatments (stirring, mixing, and kneading treatments, etc.). The type of solvent is not particularly limited as long as it is a type of solvent that can dissolve the resin in the resin composition. Specific examples thereof are as described above.

[0337] [use]

[0338] The resin composition of the present embodiment can be suitably used as a raw material for a cured product, a prepreg, a film-like underfill, a resin sheet, a laminate, a build-up material, a non-conductive film, a metal foil-clad laminate, a printed circuit board, and a fiber-reinforced composite material, or can be suitably used in the manufacture of a semiconductor device. These are described below.

[0339] [cured material]

[0340] The cured product is obtained by curing the resin composition of the present embodiment. As a method for manufacturing a cured product, for example, the resin composition of the present embodiment can be melted or dissolved in a solvent (solvent), flowed into a mold, and cured under normal conditions using heat, light, etc. to obtain it. During thermal curing, from the viewpoint of efficiently curing and preventing the degradation of the obtained cured product, the curing temperature is preferably within the range of 120 to 300°C.

[0341] [Prepreg]

[0342] The prepreg of the present embodiment contains a substrate, and a resin composition of the present embodiment impregnated or coated on the substrate. For example, the resin composition of the present embodiment (for example, uncured state (A stage)) can be impregnated or coated on the substrate, and then dried at 120 to 220 ° C for about 2 to 15 minutes to semi-cured (B stage), thereby obtaining the prepreg of the present embodiment. At this time, the amount of the resin composition (also including the cured product of the resin composition) attached to the substrate, that is, the amount of the resin composition (including dielectric powder (A) and fillers mixed as needed) relative to the total amount of the semi-cured prepreg is preferably in the range of 20 to 99% by mass. It should be noted that the semi-cured state (B stage) refers to the state that the components contained in the resin composition do not actively start to react (curing), but the resin composition is in a dry state, that is, the state where the solvent is volatilized to the extent of no adhesion by heating, and also includes a state where it will not cure even if it is not heated and only the solvent evaporates. In the present embodiment, the minimum melt viscosity of the semi-cured state (B stage) is usually less than 20,000 Pa·s. The lower limit of the minimum melt viscosity is, for example, above 10 Pa·s. It should be noted that, in the present embodiment, the minimum melt viscosity is measured by the following method. That is, 1 g of resin powder collected from the resin composition is used as a sample, and the minimum melt viscosity is measured using a rheometer (ARES-G2 (trade name), TA Instruments). Here, a disposable plate with a plate diameter of 25 mm is used to measure the minimum melt viscosity of the resin powder in a range of above 40°C and below 180°C, at a heating rate of 2°C / min, a frequency of 10.0 rad / sec, and a strain of 0.1%.

[0343] As a substrate, as long as it is a substrate for various printed circuit board materials, there is no particular limitation. As the material of the substrate, for example, glass fiber (for example, E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass and NE-glass, etc.), inorganic fibers other than glass fiber (for example, quartz, etc.), organic fibers (for example, polyimide, polyamide, polyester, liquid crystal polyester and polytetrafluoroethylene, etc.) can be cited. As the form of the substrate, there is no particular limitation, and it can be cited: woven fabric, non-woven fabric, roving, short glass fiber mat, and surface mat, etc. These substrates can be used alone or in combination with more than two kinds. Among these substrates, from the viewpoint of dimensional stability, it is preferred to implement a woven fabric with super fiber opening treatment and filling treatment, and from the viewpoint of moisture absorption and heat resistance, it is preferably a glass fabric after surface treatment using a silane coupling agent, etc., which has been treated with epoxy silane and amino silane. From the viewpoint of having excellent dielectric properties, glass fibers such as E-glass, L-glass, NE-glass, and Q-glass are preferred.

[0344] [Resin sheet]

[0345] The resin sheet of the present embodiment contains the resin composition of the present embodiment. The resin sheet can be a resin sheet with a support body containing a support body and a layer formed by the resin composition of the present embodiment disposed on the surface of the support body. The resin sheet can be used as a laminated film or a dry film solder resist. There is no particular limitation on the manufacturing method of the resin sheet, for example, the following method can be cited: a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied (coated) to the support body and dried to obtain a resin sheet.

[0346] Examples of the support include polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, release film having a release agent coated on the surface of these films, organic film substrates such as polyimide film, conductor foils such as copper foil and aluminum foil, glass plates, SUS plates, and plate-like materials such as FRP, but are not particularly limited.

[0347] As a coating method (coating method), for example, the following method can be cited: a solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied to a support using a rod coater, a die coater, a scraper, a Baker applicator, etc. In addition, after drying, the support can be peeled off or etched from a resin sheet with a support laminated with a support and a resin composition, thereby making a single-layer sheet (resin sheet). In addition, the solution obtained by dissolving the resin composition of the present embodiment in a solvent can be supplied to a mold having a sheet-shaped film cavity and dried, etc., so that a single-layer sheet (resin sheet) can be obtained without using a support.

[0348] It should be noted that in the preparation of the single-layer sheet or the resin sheet with a support of the present embodiment, the drying conditions when removing the solvent are not particularly limited. From the viewpoint of easily removing the solvent in the resin composition and inhibiting the progress of curing during drying, it is preferably carried out at a temperature of 20 to 200°C for 1 to 90 minutes. In addition, in the single-layer sheet or the resin sheet with a support, the resin composition can be used in an uncured state after only the solvent is dried, and can also be used in a semi-cured (B-stage) state as needed. In addition, the thickness of the resin layer of the single-layer sheet or the resin sheet with a support of the present embodiment can be adjusted according to the concentration of the solution of the resin composition of the present embodiment and the coating thickness, and is not particularly limited. From the viewpoint of easily removing the solvent during drying, it is preferably 0.1 to 500 μm.

[0349] [Laminated board]

[0350] The laminate of the present embodiment contains one or more of the group consisting of the prepreg and resin sheet of the present embodiment. For prepreg and resin sheet, when stacking more than 2 kinds, the resin composition used in each prepreg and resin sheet can be the same or different. In addition, when using both prepreg and resin sheet, the resin composition used in them can be the same or different. In the laminate of the present embodiment, one or more of the group consisting of prepreg and resin sheet can be semi-cured state (B stage), or can be fully cured state (C stage).

[0351] [Metal foil-clad laminate]

[0352] The metal foil-clad laminate of the present embodiment includes the laminate of the present embodiment and a metal foil disposed on one surface or both surfaces of the laminate.

[0353] Furthermore, the metal foil-clad laminate may include at least one prepreg according to the present embodiment and a metal foil laminated on one or both surfaces of the prepreg.

[0354] Furthermore, the metal foil-clad laminate may include at least one resin sheet of the present embodiment and a metal foil laminated on one surface or both surfaces of the resin sheet.

[0355] In the metal foil clad laminate of the present embodiment, the resin compositions used in the prepregs and the resin sheets may be the same or different, and when both the prepregs and the resin sheets are used, the resin compositions used in these may be the same or different. In the metal foil clad laminate of the present embodiment, one or more selected from the group consisting of the prepregs and the resin sheets may be in a semi-cured state or in a fully cured state.

[0356] In the metal foil clad laminate of the present embodiment, the metal foil is laminated on one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment, wherein the metal foil is preferably laminated in a manner that contacts the surface of one or more selected from the group consisting of the prepreg of the present embodiment and the resin sheet of the present embodiment. "The metal foil is laminated in a manner that contacts the surface of one or more selected from the group consisting of the prepreg and the resin sheet" means that there is no layer such as an adhesive layer between the prepreg or the resin sheet and the metal foil, and the prepreg or the resin sheet is in direct contact with the metal foil. As a result, there is a tendency that the metal foil peel strength of the metal foil clad laminate is improved and the insulation reliability of the printed circuit board is improved.

[0357] The metal foil clad laminate of the present embodiment may have one or more prepregs and / or resin sheets of the present embodiment overlapped, and metal foil disposed on one or both sides of the prepregs and / or resin sheets. As a method for manufacturing the metal foil clad laminate of the present embodiment, for example, the following method can be cited: overlap one or more prepregs and / or resin sheets of the present embodiment, dispose metal foil on one or both sides thereof and perform laminate molding. As a molding method, the method commonly used when molding laminates and multilayer boards for printed circuit boards can be cited. More specifically, the following method can be cited: using a multi-stage punching machine, a multi-stage vacuum punching machine, a continuous molding machine, an autoclave molding machine, etc., at a temperature of about 180 to 350°C, a heating time of about 100 to 300 minutes, and a surface pressure of 20 to 100 kgf / cm 2 The laminate molding is performed under the conditions of about 1:1.

[0358] In addition, by combining the prepreg and / or resin sheet of the present embodiment with a circuit board for the inner layer obtained separately and performing stacking molding, a multilayer board can also be made. As a manufacturing method for a multilayer board, for example, by configuring a copper foil with a thickness of about 35 μm on both sides of the prepreg and / or resin sheet of the present embodiment overlapping more than one sheet, after stacking and forming a copper foil-clad laminate using the above-mentioned molding method, an inner layer circuit is formed, and the circuit is subjected to blackening treatment to form an inner layer circuit board, and then, the inner layer circuit board and the prepreg and / or resin sheet of the present embodiment are alternately configured piece by piece, and copper foil is further configured in the outermost layer, and stacking molding is preferably performed under vacuum under the above-mentioned conditions to obtain a multilayer board. The metal foil-clad laminate of the present embodiment can be suitably used as a printed circuit board.

[0359] (metal foil)

[0360] The metal foil is not particularly limited, and examples thereof include gold foil, silver foil, copper foil, tin foil, nickel foil, and aluminum foil. Among them, copper foil is preferred. As the copper foil, there is no particular limitation as long as it is a copper foil commonly used for printed circuit board materials, and examples thereof include rolled copper foil and electrolytic copper foil. Among them, electrolytic copper foil is preferred from the viewpoint of copper foil peel strength and the formability of fine wiring. The thickness of the copper foil is not particularly limited, and may be about 1.5 to 70 μm.

[0361] [Printed Circuit Board]

[0362] The printed circuit board of the present embodiment has an insulating layer and a conductor layer disposed on one or both sides of the insulating layer, and the insulating layer contains a cured product of the resin composition of the present embodiment. The insulating layer preferably contains at least one of a layer (a layer containing a cured product) formed by the resin composition of the present embodiment and a layer (a layer containing a cured product) formed by a prepreg. Such a printed circuit board can be manufactured according to a conventional method, and its manufacturing method is not particularly limited, for example, the above-mentioned metal foil-clad laminate can be used to manufacture. An example of a method for manufacturing a printed circuit board is shown below.

[0363] First, prepare the above-mentioned metal foil-clad laminate. Then, the surface of the metal foil-clad laminate is subjected to etching treatment and the inner layer circuit is formed to make an inner substrate. On the inner layer circuit surface of the inner substrate, a surface treatment for improving bonding strength is performed as needed, and then the required number of prepregs are overlapped on the inner layer circuit surface, and then the metal foil for the outer layer circuit is stacked on its outside, and heated and pressed to form an integral body. In this way, a multilayer laminate having an insulating layer formed between the metal foil for the inner layer circuit and the outer layer circuit and consisting of a cured product of the resin composition of the present embodiment can be manufactured. Then, after the opening processing for through holes and vias is performed for the multilayer laminate, a plated metal coating that conducts the metal foil for the inner layer circuit and the outer layer circuit is formed on the wall surface of the hole, and then the metal foil for the outer layer circuit is subjected to etching treatment to form an outer layer circuit, thereby manufacturing a printed circuit board.

[0364] The printed wiring board obtained in the above manufacturing example has the following structure: it has an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer contains the cured product of the resin composition of this embodiment. That is, the prepreg of this embodiment (containing a substrate and the cured product of the resin composition of this embodiment impregnated or coated on the substrate) and the layer of the resin composition of the metal foil-clad laminate of this embodiment (the layer containing the cured product of the resin composition of this embodiment) are composed of the insulating layer containing the cured product of the resin composition of this embodiment.

[0365] [Semiconductor devices]

[0366] The semiconductor device can be manufactured by mounting a semiconductor chip on the conductive part of the printed circuit board of this embodiment. Here, the conductive part refers to the part of the multilayer printed circuit board that transmits electrical signals, and its position can be the surface or the embedded part. In addition, the semiconductor chip is not particularly limited as long as it is a circuit element using semiconductor as a material.

[0367] The method for mounting semiconductor chips when manufacturing semiconductor devices is not particularly limited as long as the semiconductor chips can function effectively. Specifically, the following methods are mentioned: wire bonding mounting method, flip chip mounting method, mounting method using solderless build-up layer (BBUL), mounting method using anisotropic conductive film (ACF), mounting method using non-conductive film (NCF), etc.

[0368] [Example]

[0369] The present embodiment will be described in more detail below using examples and comparative examples. The present embodiment is not limited in any way by the following examples.

[0370] [Measurement method of relative dielectric constant (Dk) and dielectric loss tangent (Df)]

[0371] The relative dielectric constant (Dk) and dielectric loss tangent (Df) of the dielectric powder (strontium titanate) were measured by the cavity resonator method in the following manner.

[0372] First, a sample (S) for measurement is obtained by filling 200 mg of dielectric powder in a PTFE (polytetrafluoroethylene) tube (inner diameter: 1.5 mm, manufactured by NICHIAS Co., Ltd.). A network analyzer (Network Analyzer, Agilent 8722ES (trade name), manufactured by Agilent Technologies Co., Ltd.) is used for the sample (S) for measurement to measure the relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10 GHz. It should be noted that the measurement of the relative dielectric constant (Dk) and dielectric loss tangent (Df) is carried out under an environment of temperature 23°C ± 1°C and humidity 50% RH (relative humidity) ± 5% RH.

[0373] Similarly, a PTFE (polytetrafluoroethylene) tube (inner diameter: 1.5 mm, manufactured by Nichias Corporation) itself was used as a sample (B) as a blank group, and the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the sample (B) at 10 GHz were measured.

[0374] Based on these measurement results, the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the dielectric powder at 10 GHz were calculated using the following Bruggeman formula (ii).

[0375] Formula (ii): f a ×[(ε a -ε d ) / (ε a +2ε d )]+f b ×[(ε b -ε d ) / (ε b +2ε d )]+f c ×[(ε c -ε d ) / (ε c +2ε d )]=0

[0376] It should be noted that f in formula (ii) a is the volume fraction (vol%) of PTFE in the sample for measurement, f b is the volume fraction (vol%) of air in the sample for measurement, f c is the volume fraction (vol%) of the dielectric powder in the sample for measurement, ε a is the complex dielectric constant of PTFE, ε b is the complex permittivity of air, ε c is the complex dielectric constant of the dielectric powder, ε d is the complex dielectric constant of the sample used for measurement.

[0377] Specifically, first assume that in sample (B), the volume fraction of air is f bB is 46 (vol%), the volume fraction of PTFE is f aB The complex dielectric constant ε is expressed as real and imaginary parts as "ε = ε'-iε", Dk is expressed as ε', and Df is expressed as ε" / ε'. Therefore, the complex dielectric constant ε of sample (B) (containing PTFE and air) is calculated based on the measurement results (Dk and Df) of sample (B). dB Then, assuming the real part is 1.0 and the imaginary part is 0, the complex dielectric constant ε of air is bB is 1.0, so by aB 、f bB , ε dB , and ε bB Substitute into equation (ii) to calculate the complex dielectric constant ε of PTFE a .

[0378] Then, in the measurement sample (S) (containing PTFE, air, and dielectric powder), the volume fraction f of the dielectric powder is cS(vol%) is calculated using the inner diameter and length of the PTFE tube, the mass difference before and after dielectric powder filling, and the specific gravity of the dielectric powder. Assuming that the volume fraction of PTFE is f aS is 54 (vol%), using the calculated volume fraction f cS , calculate the volume fraction of air f bS Then, similarly to sample (B), the complex dielectric constant ε of sample (S) (containing PTFE, air, and dielectric powder) was calculated from the measurement results (Dk and Df) of the measurement sample (S). dS Assuming the complex dielectric constant of air ε b = 1.0, using the ε calculated from sample (B) a , and f aS 、f bS 、f cS , and ε dS , and use formula (ii) to calculate the complex dielectric constant ε of the dielectric powder c . By calculating ε c Calculate the Dk and Df of the dielectric powder.

[0379] [Method for measuring average particle size]

[0380] The average particle size (D50) of the dielectric powder (strontium titanate) was calculated by measuring the particle size distribution using a laser diffraction-scattering particle size distribution measuring apparatus (Microtrac (registered trademark) MT3300EXII (trade name), Microtrac BEL Co., Ltd.) under the following measurement conditions using a laser diffraction-scattering method.

[0381] (Measurement conditions of laser diffraction-scattering particle size distribution measuring device)

[0382] (Strontium Titanate)

[0383] Solvent: methyl ethyl ketone, solvent refractive index: 1.33, particle refractive index: 2.41, transmittance: 85±5%.

[0384] [Synthesis Example 1] Synthesis of 1-naphthol aralkyl type cyanate compound (SN495V-CN)

[0385] 300 g (1.28 mol in terms of OH group) of 1-naphthol aralkyl type phenol resin (SN495V (trade name), OH group (hydroxyl) equivalent: 236 g / eq., Nippon Steel Chemical Co., Ltd.) and 194.6 g (1.92 mol) of triethylamine (1.5 mol per 1 mol of hydroxyl group) were dissolved in 1800 g of dichloromethane to prepare solution 1. 125.9 g (2.05 mol) of cyanogen chloride (1.6 mol per 1 mol of hydroxyl group), 293.8 g of dichloromethane, 194.5 g (1.92 mol) of 36% hydrochloric acid (1.5 mol per 1 mol of hydroxyl group) and 1205.9 g of water were added to solution 1 over 30 minutes while stirring and maintaining the liquid temperature at -2 to -0.5°C. After the injection of solution 1 is completed, the mixture is stirred at the same temperature for 30 minutes, and then a solution (solution 2) obtained by dissolving 65 g (0.64 mol) of triethylamine (0.5 mol relative to 1 mol of hydroxyl group) in 65 g of dichloromethane is injected over 10 minutes. After the injection of solution 2 is completed, the mixture is stirred at the same temperature for 30 minutes to terminate the reaction. Then, the reaction solution is allowed to stand to separate the organic phase from the aqueous phase, and the obtained organic phase is washed 5 times with 1300 g of water. The conductivity of the wastewater after the fifth washing was 5 μS / cm, confirming that the ionic compounds that can be removed by water-based washing were fully removed. The washed organic phase was concentrated under reduced pressure, and finally concentrated to dryness at 90°C for 1 hour to obtain the target 1-naphthol aralkyl type cyanate compound (SN495V-CN, cyanate group equivalent: 261 g / eq., R in the above formula (10) 3 All of them are hydrogen atoms, and n3 is an integer of 1 to 10) (orange viscous material) 331g. The infrared absorption spectrum of the obtained SN495V-CN shows 2250cm -1 The absorption of the cyanate group was not shown, and the absorption of the hydroxyl group was not shown.

[0386] [Example 1]

[0387] 25 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 30 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 10 parts by mass of bis(3-ethyl-5-methyl-4-maleimidophenyl)methane (BMI-70 (trade name), K.I. Chemical Industry Co., Ltd.), 20 parts by mass of a biphenyl aralkyl type epoxy resin (NC-3000FH (trade name), epoxy equivalent: 328 g / eq., manufactured by Nippon Kayaku Co., Ltd.), and naphthalene type epoxy resin (EPICLON (registered trademark) EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., manufactured by DIC Corporation) were added. Co., Ltd.), 5 parts by mass of 1,3-phenylenebis(2,6-di(xylyl)phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.), 10 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), 300 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), manufactured by BYK-Chemie Japan Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), and octanoic acid manganese (Nikka 0.5 parts by mass of OCTHIX MANGANESE (trade name, manufactured by Nippon Chemical Industry Co., Ltd.) and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0388] The obtained resin varnish was impregnated and coated on E glass cloth (1031NT S640 (trade name), Arisawa Manufacturing Co., Ltd.) having a thickness of 0.094 mm, and heated and dried at 130° C. for 3 minutes to obtain a prepreg having a thickness of 0.1 mm.

[0389] Then, electrolytic copper foils (3EC-M3-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) with a thickness of 12 μm were placed on the upper and lower surfaces of the obtained prepreg and the surface pressure was 30 kgf / cm 2 The laminate was then vacuum pressed at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.124 mm. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation method. The results are shown in Table 1.

[0390] [Example 2]

[0391] A resin varnish was obtained in the same manner as in Example 1 except that 25 parts by mass of a biphenyl aralkyl maleimide compound (MIR-3000-70MT (trade name)) was used instead of 25 parts by mass, and 15 parts by mass of 1,3-phenylene bis(2,6-di(xylyl)phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.) was used instead of 10 parts by mass.

[0392] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0393] [Comparative Example 1]

[0394] 25 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 40 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 10 parts by mass of bis(3-ethyl-5-methyl-4-maleimidephenyl)methane (BMI-70 (trade name), K.I. Chemical Industry Co., Ltd.), 20 parts by mass of a biphenyl aralkyl type epoxy resin (NC-3000FH (trade name), epoxy equivalent: 328 g / eq., manufactured by Nippon Kayaku Co., Ltd.), and 10 parts by mass of a naphthalene-type Epoxy resin (EPICLON (registered trademark) EXA-4032-70M (trade name), epoxy equivalent: 150 g / eq., manufactured by DIC Corporation) 5 parts by mass, strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.) 300 parts by mass, a wetting and dispersing agent (BYK (registered trademark) -W903 (trade name), BYK-Chemie 3 parts by mass of methyl ethyl ketone (manufactured by Japan Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by mass of manganese octoate (Nikkaocthix Manganese (trade name), manufactured by Nippon Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0395] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0396] [Example 3]

[0397] 30 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 35 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 15 parts by mass of an indane type maleimide compound (NE-X-9470S (trade name), DIC Corporation), 1,3-phenylene bis(2,6-di(xylyl) phosphate) (PX-20 0 (trade name), Daihachi Chemical Industry Co., Ltd.), 20 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), 300 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), manufactured by BYK-Chemie Japan Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by mass of manganese octoate (NIKKA OCTHIX MANGANESE (trade name), manufactured by Nippon Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0398] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0399] [Example 4]

[0400] A resin varnish is obtained in the same manner as in Example 3, except that 30 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1 is replaced by 45 parts by mass, 35 parts by mass of the biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name)) is replaced by 25 parts by mass, and 15 parts by mass of the indane type maleimide compound (NE-X-9470S (trade name)) is replaced by 10 parts by mass.

[0401] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0402] [Example 5]

[0403] 45 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 50 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 5 parts by mass of 1,3-phenylene bis(2,6-di(xylyl)phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.), 300 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), and a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK-Chemie 3 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by mass of manganese octoate (Nikka OCTHIX MANGANESE (trade name), manufactured by Nippon Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0404] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0405] [Comparative Example 2]

[0406] 40 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 40 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 20 parts by mass of an indane type maleimide compound (NE-X-9470S (trade name), DIC Corporation), 300 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), and a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK-Chemie 3 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by mass of manganese octoate (Nikka OCTHIX MANGANESE (trade name), manufactured by Nippon Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0407] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0408] [Example 6]

[0409] A resin varnish was obtained in the same manner as in Example 5, except that 45 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1 was replaced with 40 parts by mass, and 5 parts by mass of 1,3-phenylene bis(2,6-di(xylyl) phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.) was replaced with 10 parts by mass.

[0410] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0411] [Example 7]

[0412] A resin varnish was obtained in the same manner as in Example 5, except that 45 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1 was replaced by 30 parts by mass, and 5 parts by mass of 1,3-phenylene bis(2,6-di(xylyl) phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.) was replaced by 20 parts by mass.

[0413] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0414] [Example 8]

[0415] A resin varnish was obtained in the same manner as in Example 7 except that 20 parts by mass of condensed phosphate (SR-3000 (trade name), Daihachi Chemical Industry Co., Ltd.) was used instead of 20 parts by mass of 1,3-phenylenebis(2,6-di(xylyl)phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.).

[0416] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0417] [Comparative Example 3]

[0418] 50 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 50 parts by mass of a biphenyl aralkyl type maleimide compound (MIR-3000-70MT (trade name), Nippon Kayaku Co., Ltd.), 300 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), 3 parts by mass of a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), manufactured by BYK-Chemie Japan Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), and manganese octanoate (NIKKA OCTHIX MANGANESE (trade name, manufactured by Nippon Chemical Industry Co., Ltd.) 0.5 parts by mass and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0419] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0420] [Example 9]

[0421] 30 parts by mass of the 1-naphthol aralkyl type cyanate compound (SN495V-CN) obtained in Synthesis Example 1, 50 parts by mass of an indane type maleimide compound (NE-X-9470S (trade name), DIC Corporation), 20 parts by mass of 1,3-phenylenebis(2,6-di(xylyl)phosphate) (PX-200 (trade name), Daihachi Chemical Industry Co., Ltd.), 300 parts by mass of strontium titanate (SrTiO3, an oxide with a perovskite structure, average particle size (D50): 0.3 μm, relative dielectric constant (Dk): 21, dielectric loss tangent (Df): 0.007, ST-03 (trade name), manufactured by Sakai Chemical Industry Co., Ltd.), and a wetting and dispersing agent (BYK (registered trademark)-W903 (trade name), BYK-Chemie 3 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.1 parts by mass of 2,4,5-triphenylimidazole (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.5 parts by mass of manganese octoate (Nikka OCTHIX MANGANESE (trade name), manufactured by Nippon Chemical Industry Co., Ltd.), and 100 parts by mass of methyl ethyl ketone were mixed to obtain a resin varnish.

[0422] Using this resin varnish, a prepreg and a metal foil-clad laminate were obtained in the same manner as in Example 1. The physical properties of the obtained prepreg and metal foil-clad laminate were measured according to the evaluation methods. The measurement results are shown in Table 1.

[0423] [Evaluation method]

[0424] (1) Relative dielectric constant (Dk) and dielectric loss tangent (Df)

[0425] Four prepregs obtained in the examples and comparative examples were stacked, and electrolytic copper foils (3EC-M3-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) with a thickness of 12 μm were placed on the upper and lower surfaces, and the surface pressure was 30 kgf / cm 2 And the temperature is 220 ℃, vacuum pressing is implemented for 120 minutes and stacking molding is performed to obtain a metal foil laminate (double-sided copper-clad laminate) with a thickness of 0.424mm. The copper foil on both sides of the metal foil laminate is completely etched to obtain an unclad plate with a thickness of 0.4mm with all the copper foil on both sides removed. The unclad plate is cut into a size of 1mm×65mm (miniaturization) to obtain a sample for measurement. Using the sample for measurement and using a network analyzer (Network Analyzer, Agilent (registered trademark) 8722ES (trade name), Agilent Technologies Co., Ltd.), the relative dielectric constant (Dk) and dielectric loss tangent (Df) at 10GHz are measured respectively. It should be noted that the determination of the relative dielectric constant (Dk) and dielectric loss tangent (Df) is carried out under a temperature of 23℃±1℃ and a humidity of 50%RH±5%RH.

[0426] (2) Copper foil peel strength

[0427] Four prepregs obtained in the examples and comparative examples were stacked, and electrolytic copper foils (3EC-M3-VLP (trade name), manufactured by Mitsui Mining & Smelting Co., Ltd.) with a thickness of 12 μm were placed on the upper and lower surfaces of the prepregs. The prepregs were then placed under a surface pressure of 30 kgf / cm 2 The laminate was formed by vacuum pressing at 220°C for 120 minutes to obtain a metal foil-clad laminate (double-sided copper-clad laminate) with a thickness of 0.424 mm. The copper foil peel strength (copper foil adhesion, kgf / cm) was measured using the metal foil-clad laminate (10 mm×100 mm×0.424 mm) in accordance with JIS C6481.

[0428] (3) Hygroscopic heat resistance evaluation

[0429] The metal foil-clad laminates obtained in Examples and Comparative Examples were cut into a size of 50 mm×50 mm (miniaturized), and the copper foil on one side was completely removed by etching, and the copper foil on half of the other side was removed by etching to prepare measurement samples.

[0430] The obtained measurement sample was treated for 3 hours at 121°C and in the presence of saturated steam at 2 atmospheres using a pressure cooker tester (PC-3 model (trade name), Hirayama Manufacturing Co., Ltd.), and then immersed in a solder bath at 260°C for 60 seconds to visually observe whether there was any abnormal change in appearance.

[0431] Each measurement was performed on 4 sheets, and the evaluation was "A" when no abnormality was observed in all 4 sheets, and the evaluation was "C" when one sheet of the 4 sheets had an abnormal appearance. In addition, in the sample after immersion, for example, when swelling occurred on the surface or back of the copper foil, it was judged to be abnormal in appearance. In Tables 1 and 2, "PCT 3h" indicates the result after 3 hours of treatment using a pressure cooker tester.

[0432] (4) Heat resistance of copper-containing solder (thermal properties)

[0433] The metal foil-clad laminate obtained in the embodiment and the comparative example is cut into a size of 50 mm × 50 mm (miniaturized) to obtain a sample for measurement. Similarly, a total of 3 samples for measurement are prepared. Each sample for measurement is floated in a solder tank at 260°C for 30 minutes in a manner that only one side of the sample contacts the solder. After 30 minutes, the sample is taken out from the solder tank, and the side of these samples in contact with the solder is visually observed to see if there is any change in appearance. The results of observing the three samples separately are evaluated as "A" when there is no appearance abnormality in all samples, and "C" is evaluated when more than one sample has an appearance abnormality. It should be noted that in the sample, for example, the situation where bulging is observed at the interface between the metal foil and the insulating layer is judged as an appearance abnormality.

[0434] [Table 1]

[0435]

[0436] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-57895) filed on March 31, 2022, and the contents are incorporated herein by reference.

[0437] [Industrial Applicability]

[0438] The resin composition of the present invention has a high dielectric constant and a low dielectric loss tangent, and has excellent moisture absorption heat resistance, a high glass transition temperature, a low thermal expansion coefficient, and good coating properties and appearance. Therefore, the resin composition of the present invention can be suitably used as a raw material for a cured product, a prepreg, a film-like bottom filler, a resin sheet, a laminate, a laminated material, a non-conductive film, a metal foil laminate, a printed circuit board, and a fiber-reinforced composite material, or suitably used in the manufacture of a semiconductor device.

Claims

1. A resin composition comprising a dielectric powder (A), an aromatic phosphorus compound (B), and a thermosetting resin (C).

2. The resin composition according to claim 1, wherein The dielectric powder (A) includes one or more selected from the group consisting of titanium dioxide, barium titanate, calcium titanate, and strontium titanate.

3. The resin composition according to claim 1, wherein The average particle size of the dielectric powder (A) is 0.1 to 5 μm.

4. The resin composition according to claim 1, wherein The content of the dielectric powder (A) is 50 to 500 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

5. The resin composition according to claim 1, wherein The aromatic phosphorus compound (B) comprises at least one selected from the group consisting of a phosphaphenanthrene compound, an aromatic phosphorus compound represented by the following formula (1), an aromatic phosphorus compound represented by the following formula (2), an aromatic phosphorus compound represented by the following formula (3), and an aromatic phosphorus compound represented by the following formula (4); In formula (1), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, X represents a divalent organic group, m each independently represents 0 or 1, and n represents 0 to 5; wherein, in formula (1), at least one R is an aryl group having 6 to 30 carbon atoms; In formula (2), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, X represents a divalent organic group, m each independently represents 0 or 1, and n represents 0 to 5; wherein, in formula (2), at least one R is an aryl group having 6 to 30 carbon atoms; In formula (3), A each independently represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and n represents an integer of 3 to 15; In formula (4), A represents a hydrogen atom, a hydroxyl group, a cyano group, an amino group, a carboxyl group, a glycidyloxy group, a p-hydroxyphenyldimethyl group, a p-glycidyloxyphenyldimethyl group, a p-hydroxyphenylsulfone group, a p-glycidyloxyphenylsulfone group, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms, and R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms.

6. The resin composition according to claim 5, wherein The aromatic phosphorus compound represented by the formula (1) comprises at least one selected from the group consisting of an aromatic phosphorus compound represented by the following formula (6) and an aromatic phosphorus compound represented by the following formula (8); In formula (6), R each independently represents a hydrogen atom, an alkyl group having 1 to 30 carbon atoms, or an aryl group having 6 to 30 carbon atoms; In the formula (8), R represents an alkyl group having 1 to 4 carbon atoms, l represents an integer of 3 to 11, m represents an integer of 0 to 22, and n represents an integer of 1 to 10.

7. The resin composition according to claim 1, wherein The content of the aromatic phosphorus compound (B) is 1 to 40 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

8. The resin composition according to claim 1, wherein The thermosetting resin (C) includes one or more selected from the group consisting of cyanate compounds, maleimide compounds, epoxy compounds, phenol compounds, modified polyphenylene ether compounds, alkenyl-substituted nadic imide compounds, oxetane resins, benzoxazine compounds, and compounds having a polymerizable unsaturated group.

9. The resin composition according to claim 8, wherein The maleimide compound comprises one or more selected from the group consisting of bis(4-maleimidephenyl)methane, 2,2-bis(4-(4-maleimidephenoxy)-phenyl)propane, bis(3-ethyl-5-methyl-4-maleimidephenyl)methane, a maleimide compound represented by the following formula (11), a maleimide compound represented by the following formula (12), and a maleimide compound represented by the following formula (13); In formula (11), R 1 Each independently represents a hydrogen atom or a methyl group, and n1 is an integer from 1 to 10; In formula (12), R 2 Each independently represents a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or a phenyl group, and n2 is an average value and represents 1<n2≤5; In formula (13), Ra each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group; q represents an integer of 0 to 4; when q is an integer of 2 to 4, Ra may be the same or different in the same ring; Rb each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group; r represents an integer of 0 to 3; when r is 2 or 3, Rb may be the same or different in the same ring; n is the average number of repeating units and represents a value of 0.95 to 10.

0.

10. The resin composition according to claim 8, wherein The content of the maleimide compound is 15 to 85 parts by mass based on 100 parts by mass of the resin solid content in the resin composition. 11 . The resin composition according to claim 1 , further comprising a filler different from the dielectric powder (A).

12. The resin composition according to claim 11, wherein The filler includes one or more selected from the group consisting of silica, alumina, talc, aluminum nitride, boron nitride, boehmite, aluminum hydroxide, zinc molybdate, silicone rubber powder, and silicone composite powder.

13. The resin composition according to claim 11, wherein The content of the filler is 50 to 300 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

14. The resin composition according to claim 1, which is used for a printed circuit board. 15 . A prepreg comprising a substrate and the resin composition according to claim 1 impregnated or coated on the substrate. 16 . A resin sheet comprising the resin composition according to claim 1 .

17. A laminate comprising the prepreg according to claim 15. 18 . A laminate comprising the resin sheet according to claim 16 . 19 . A metal foil-clad laminate comprising the laminate according to claim 17 and a metal foil disposed on one or both surfaces of the laminate. 20 . A metal foil-clad laminate comprising the laminate according to claim 18 and a metal foil disposed on one or both surfaces of the laminate.

21. A printed circuit board comprising an insulating layer and a conductor layer disposed on one or both sides of the insulating layer, The insulating layer contains a cured product of the resin composition according to any one of claims 1 to 14.