Quantum dot preparation method
By mixing quantum dot precursors at low temperatures through rapid heating and cooling methods, quantum dots with high efficiency and excellent stability are solved, and the problems of complex preparation methods and low performance in the prior art are achieved, and simplified process and performance improvement are achieved .
Patent Information
- Application Number
- CN202280094579.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2022-05-13
- Publication Date
- 2024-11-22
AI Technical Summary
The existing quantum dot preparation methods are complex, the synthesis time is long, it is difficult to control the emission wavelength, the thermal stability and quantum efficiency are low, and the performance deteriorates during the multi-step process.
Mix precursor solutions such as indium oxide clusters and trialkylphosphine at 20°C to 130°C, quickly heat up to 300°C and cool to form quantum dots with uniform nuclei, simplify the process and reduce steps, avoid centrifugal purification, by adjusting before Body ratio controls wavelength and performance.
High quantum efficiency, excellent optical and thermal stability are achieved, synthesis time is shortened, production process is simplified, costs are reduced, and the uniformity and optical durability of quantum dots are improved through rapid cooling and heat treatment.
Smart Images

Figure CN119013373A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for preparing quantum dots and quantum dots prepared thereby, and more particularly to a method for preparing quantum dots capable of obtaining quantum dots with shortened reaction time, easy large-scale production, high quantum efficiency, and improved optical and thermal stability. Background Art
[0002] Quantum dots are semiconductor materials with a nano-sized crystal structure that have high color purity, excellent light stability and thermal stability, and easy control of the band gap compared to organic materials. Since these quantum dots have a large surface area per unit volume due to their small size and exhibit a quantum confinement effect, quantum dots have physical and chemical properties that are different from those of the semiconductor material itself. Quantum dots absorb light from an excitation source, enter an energy excited state, and emit energy corresponding to the energy band gap of the quantum dots. Since quantum dots have luminescent properties, can control the energy band gap by controlling the size and composition of nanocrystals, and have high color purity, quantum dots have been developed for various applications such as display devices, energy devices, or bioluminescent devices.
[0003] When quantum dots are applied to devices, the efficiency is reduced due to corrosion and oxidation of quantum dots by high frequency, heat, moisture, etc. Therefore, the conventional quantum dots generally mentioned are mainly used in a core-shell structure in which the shell is coated on the surface of the core. Therefore, when the shell is coated on the surface of the core, it has the following advantages: improving the phenomenon of quantum dots being corroded by heat or moisture, and improving optical durability by acting as an energy barrier to limit the charge formed by applying light.
[0004] Generally, the method for preparing quantum dots having a core-shell structure uses a method of preliminarily synthesizing a core by injecting an anion precursor solution into a high-temperature cation precursor solution at a high temperature, and then secondarily forming a shell by injecting a solution constituting a shell component. At this time, quantum dots having a core-shell or multi-shell structure can be prepared according to the number of times the solution constituting the shell component is added.
[0005] However, due to the series of processes of preparing each precursor solution and synthesizing multiple solutions in steps, the above-mentioned quantum dot preparation method has the disadvantages of complex synthesis method and increased synthesis time. In addition, quantum dots with core-shell structure can usually control the emission wavelength by adjusting the particle size of the core, but since the reaction rate of synthesizing the core is very fast, it is difficult to control the emission wavelength. In addition, there is the following problem: in the process of forming the core-shell structure through multiple steps, when lattice mismatch occurs between the core and the shell, the thermal stability and quantum efficiency of the quantum dots will be reduced. Summary of the invention
[0006] [Technical issues]
[0007] The object of the present invention is to provide a method for preparing quantum dots which can be easily mass-produced in a short time.
[0008] Another object of the present invention is to provide a method for preparing quantum dots, which can achieve high quantum efficiency by having a narrow full width at half maximum.
[0009] Another object of the present invention is to provide a method for preparing quantum dots with excellent photostability and thermal stability.
[0010] Still another object of the present invention is to provide a method for preparing quantum dots, which can variously adjust emission wavelengths by easily controlling reactions.
[0011] The objects of the present invention are not limited to the above objects, and other objects not mentioned above will be apparent to those skilled in the art through the following description.
[0012] [Technical solution]
[0013] One aspect of the present invention provides a method for preparing quantum dots, comprising: preparing a first solution containing at least one first cation precursor and a second solution containing at least one first anion precursor; mixing the first solution and the second solution at 20°C to 130°C to prepare a first mixture; raising the temperature of the first mixture to a high temperature of 300°C within 1 minute; and cooling the first mixture with the raised temperature to 100°C or lower within 1 minute to form a core, wherein the first cation precursor includes an indium oxide cluster (In-Oxo cluster).
[0014] Details of other embodiments are included in the detailed description and accompanying drawings of the invention.
[0015] [Advantageous Effects]
[0016] According to the preparation method of the present invention, quantum dots capable of achieving high quantum efficiency can be obtained by having a narrow full width at half maximum.
[0017] According to the preparation method of the present invention, quantum dots having excellent photostability and thermal stability can be obtained by using a synthesis technique using high-temperature heat treatment.
[0018] According to the preparation method of the present invention, the core is used without centrifugation, and the reaction time is short, so large-scale production can be achieved in a short time using a small-scale continuous production method.
[0019] According to the preparation method of the present invention, since the reaction can be easily controlled and the emission wavelength can be adjusted in various ways, there is an effect of minimizing the defect rate.
[0020] The effects according to the present invention are not limited to the above-exemplified contents, and more various effects are included in this specification. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a flow chart schematically illustrating a nucleus formation process in a quantum dot preparation method according to an embodiment of the present invention.
[0022] Figure 2 is a flow chart schematically illustrating a shell formation process in a method for preparing quantum dots according to an embodiment of the present invention.
[0023] Figure 3 is a schematic diagram for describing a method for preparing quantum dots according to an embodiment of the present invention.
[0024] Figure 4 is a schematic diagram for describing a method for preparing quantum dots according to an embodiment of the present invention. DETAILED DESCRIPTION
[0025] From the embodiments described in detail below with reference to the accompanying drawings, the advantages and features of the present invention and the methods for implementing the present invention will be more clearly understood. However, the present invention is not limited to the following embodiments, but can be implemented in various different forms. The embodiments are provided only to improve the disclosure of the present invention and to provide the category of the present invention to those of ordinary skill in the art to which the present invention belongs.
[0026] The shapes, sizes, ratios, angles, quantities, etc. shown in the drawings for describing the embodiments of the present invention are merely examples, and the present invention is not limited thereto. In this specification, the same reference numerals represent the same components. In addition, when describing the present invention, when it is determined that it will unnecessarily obscure the subject matter of the present invention, the detailed explanation of the known related art will be omitted. The terms "including", "having" and "consisting of..." used herein are generally intended to allow the addition of other components, unless these terms are used together with the word "only". When a component is expressed in the singular, the singular may include the plural form unless otherwise expressly stated.
[0027] Even if not explicitly stated, components are interpreted as including ordinary margins of error.
[0028] When terms such as “on,” “above,” “below,” and “next to” are used to describe the positional relationship between two parts, one or more other parts may be located between the two parts unless these terms are used together with “close to” or “directly.”
[0029] When an element or layer is referred to as being “on” another element or layer, it can be directly on the other element or layer, or intervening elements or layers may be present.
[0030] Although the terms "first", "second", etc. are used to describe various components, these components are not limited by these terms. These terms are only used to distinguish one element or component from another element or component. Therefore, the first component to be mentioned below can be the second component in the technical concept of the present invention.
[0031] In this specification, the same reference numerals denote the same components.
[0032] Since the size and thickness of each component shown in the drawings are represented for convenience of explanation, the present invention is not necessarily limited to the shown size and thickness of each component.
[0033] The features of the various embodiments of the present invention may be partially or completely coupled or combined with each other, and may be technically interlocked and operated in various ways, and the embodiments may be performed independently or in association with each other.
[0034] Hereinafter, the present invention will be described with reference to the accompanying drawings.
[0035] Figure 1 is a flow chart schematically illustrating a nucleus formation process in a quantum dot preparation method according to an embodiment of the present invention.
[0036] refer to Figure 1 , a method for preparing quantum dots according to an embodiment of the present invention includes preparing a first solution containing at least one first cation precursor and a second solution containing at least one first anion precursor (S110); mixing the first solution and the second solution at 20°C to 130°C to prepare a first mixture (S120); raising the temperature of the first mixture to a high temperature of 300°C within 1 minute (S130); and cooling the first mixture with the raised temperature to 100°C or less within 1 minute to form a core (S140), wherein the first cation precursor includes an indium oxide cluster (In-Oxo cluster).
[0037] Hereinafter, the quantum dot preparation method of the present invention will be described step by step in detail.
[0038] First, a first solution containing at least one first cation precursor and a second solution containing at least one first anion precursor are prepared ( S110 ).
[0039] At this time, at least one of the first solution and the second solution may include two or more precursors. For example, the first solution may include two types of cationic precursors, and the second solution may also include two types of anionic precursors, but is not limited thereto.
[0040] The first cation precursor includes an indium oxide cluster (In-Oxo cluster). A cluster structure refers to a structure in which three or more atoms of the same or similar element are combined to form a single substance, and an active metal oxide such as an indium oxide cluster (In-Oxo) can be synthesized by reacting an active metal precursor with a carboxylic acid. Specifically, the indium oxide cluster (In-Oxo) can be formed by reacting an active metal precursor such as indium (III) acetate and a carboxylate such as oleic acid.
[0041] The first solution may include one or more first cation precursors, and thus, the first cation precursor may also include cadmium (Cd), mercury (Hg), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) or strontium (Sr).
[0042] Specifically, the first cationic precursor can be further selected from oxides, peroxides, sulfates, halides, oleates, perchlorates, carboxylates, acetates, phosphates, acetylacetonates, cyanides, carbonates or nitrates of cadmium (Cd), mercury (Hg), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) or strontium (Sr), but is not limited thereto.
[0043] In addition, the first cation precursor may also include zinc oxide clusters (Zn-Oxo clusters). Similar to indium oxide (In-Oxo), active metal oxides such as zinc oxide clusters (Zn-Oxo) can be synthesized by reacting active metal precursors with carboxylic acids. Specifically, zinc oxide clusters (Zn-Oxo) can be formed by reacting active metal precursors such as zinc acetate (Zn acetate) and carboxylates such as oleic acid.
[0044] The first anion precursor may be a compound containing sulfur (S), selenium (Se), phosphorus (P), tellurium (Te), arsenic (As), nitrogen (N), or antimony (Sb).
[0045] For example, the first anion precursor can be selected from sulfur, trialkylphosphine sulfide, trialkenylphosphine sulfide, alkylaminosulfide, alkenylaminosulfide, alkylthiol, selenium, trialkylphosphine selenide, trialkenylphosphine selenide, alkylaminoselenide, alkenylaminoselenide, trialkylphosphine telluride, trialkenylphosphine telluride, alkylaminotelluride, alkynylaminotelluride, alkylphosphine, tri(trialkylsilyl)phosphine, tri(dialkylsilyl)phosphine, tri(dialkylamino)phosphine, arsenic oxide, arsenic chloride, arsenic sulfate, arsenic bromide, arsenic iodide, nitric oxide, nitric acid and ammonium nitrate, but is not limited thereto. More specifically, the first anion precursor can include tri(trimethylsilyl)phosphine (TMSP).
[0046] The preparation of the first solution can also include mixing the first cation precursor and unsaturated fatty acids, and then raising the temperature of the mixture to form a more suitable first cation precursor. By comprising an unsaturated fatty acid ligand with a long chain length, the first cation precursor prepared above can maintain a more stable dispersed form. For example, the unsaturated fatty acid can be selected from myristic acid, oleic acid, stearic acid, lauric acid and palmitic acid, and in view of the dispersion stability, size distribution and luminescent properties of quantum dots, oleic acid can be preferably used, but is not limited thereto.
[0047] The preparation of the first solution includes preparing indium oxide clusters (In-Oxo). Specifically, the preparation of indium oxide clusters (In-Oxo) may include mixing indium acetate (indium (III) acetate) and oleic acid, raising the temperature of the mixed solution to 200°C under vacuum, then converting the pressure to normal pressure, and then adding octadecene (ODE) and synthesizing at 260°C to 300°C for 1 hour or more. Therefore, the first solution includes indium oxide clusters, but is not limited thereto.
[0048] In addition, the preparation of the first solution may further include preparing zinc oxide clusters (Zn-Oxo). Specifically, the preparation of zinc oxide clusters (Zn-Oxo) may include mixing dehydrated zinc acetate (dehydrated Zn acetate) and oleic acid, raising the temperature to 190°C under vacuum and converting the pressure to normal pressure, then adding octadecene (ODE) and synthesizing at 300°C to 315°C for 1 hour or more, so the first solution may also include zinc oxide clusters.
[0049] By considering the emission wavelength of the quantum dots finally formed, the composition ratio of the indium oxide clusters and the zinc oxide clusters in the first solution can be appropriately controlled. For example, the molar ratio of the indium oxide clusters and the zinc oxide clusters can be 1:1 to 1:0.4. More specifically, based on the case where the anion precursor such as phosphorus (p) is 1, the molar ratio of the indium oxide clusters and the zinc oxide clusters can be 1.2:1.2 to 1.8:0.8, but is not limited thereto.
[0050] The preparation of the second solution can also include mixing anion precursors and trialkylphosphines, and then raising the temperature of the mixture to form a more suitable first anion precursor. The anion precursor prepared in this way has better dispersion stability by comprising a long-chain trialkylphosphine ligand. For example, the trialkylphosphine can be selected from trihexylphosphine, trioctylphosphine and tridecylphosphine, and trioctylphosphine is preferably used in view of dispersion stability, but is not limited thereto.
[0051] Next, the first solution and the second solution are mixed at 20° C. to 130° C. to prepare a first mixture ( S120 ).
[0052] Specifically, the first solution containing the first cation precursor and the second solution containing the first anion precursor may be mixed at a relatively low temperature of 20° C. to 130° C. (more preferably, 80° C. to 120° C.). At this time, by mixing the first solution and the second solution at a relatively low temperature, the chemical reaction between the cation precursor and the anion precursor may be suppressed.
[0053] The solvent can mix the first cation precursor of the first solution and the first anion precursor of the second solution, and any non-reactive solvent can be appropriately selected and used without particular limitation. Specifically, the solvent can be a primary alkylamine having 6 to 22 carbon atoms, such as hexadecylamine, a secondary alkylamine having 6 to 23 carbon atoms, such as dioctylamine, a tertiary alkylamine having 6 to 40 carbon atoms, such as trioctylamine; a nitrogen-containing heterocyclic compound, such as pyridine, an aliphatic hydrocarbon (alkane, alkene, alkyne, etc.) having 6 to 40 carbon atoms, such as hexadecane, octadecane, octadecene and squalane, an aromatic hydrocarbon having 6-30 carbon atoms, such as phenyldodecane, phenyltetradecane and phenylhexadecane, a phosphine substituted by an alkyl having 6 to 20 carbon atoms, such as trioctylphosphine, a phosphine oxide substituted by an alkyl having 6 to 22 carbon atoms, such as trioctylphosphine oxide, an aromatic ether having 12 to 22 carbon atoms, such as phenyl ether and benzyl ether, and a combination thereof, but not limited thereto. Preferably, the solvent may be an aliphatic hydrocarbon having 6 to 40 carbon atoms, such as octadecene and squalane.
[0054] As another example, the solvent may be pre-added in the first solution preparation step and / or the second solution preparation step. Specifically, for example, when preparing the first solution, indium acetate and oleic acid may be mixed, the temperature may be raised to 200° C., and then the solvent may be added.
[0055] Next, the temperature of the first mixture is rapidly increased to 300° C. to 350° C. at a rate of 3° C. / sec to 10° C. / sec within 1 minute ( S130 ).
[0056] In step S130, the temperature of the first mixture is rapidly increased to 300° C. to 350° C. or higher within 120 seconds, preferably within 60 seconds. In this case, there are advantages of greatly shortening the synthesis time and facilitating large-scale production. In addition, the quantum dots or cores prepared by rapidly increasing the temperature have the advantages of uniform particle size distribution, narrow half-maximum full width, and excellent quantum efficiency.
[0057] As another example, in step S130, the rapid increase in temperature may be completed within a range of 15 to 80 seconds (preferably 30 to 60 seconds). Within this range, there are advantages in both productivity and quantum dot quality.
[0058] In step S130, the heating rate may be 3°C / sec to 10°C / sec, preferably 3°C / sec to 8°C / sec. In this case, the synthesis time is greatly shortened, and the size of the obtained quantum dots becomes uniform, thereby exhibiting high quantum efficiency.
[0059] More specifically, for example, in step S130 , the temperature of the first mixture at 80° C. to 120° C. may be quickly increased to 300° C. within 120 seconds, preferably within 60 seconds.
[0060] The rapid increase in temperature can be performed using a rapid heating device. For example, the first mixture can be rapidly heated using the radiant heat generated by a lamp. At this time, a halogen lamp, a tungsten halogen lamp, or a xenon arc lamp can be used to rapidly increase the temperature of the first mixture.
[0061] The temperature of the first mixture may be increased to 300° C. or higher, preferably 300° C. to 350° C. If the increased temperature is lower than 300° C., quantum dots may not be stably synthesized, the reaction time may become very long, and the particle size distribution may increase. If the temperature exceeds 350° C., the purity of the quantum dots may be reduced due to reaction with trace amounts of oxygen or moisture present in the reactor or other side reactions.
[0062] Next, although Figure 1 Although not shown in the schematic flow chart of , the first mixture is heat-treated at 300° C. or higher for 1 to 10 seconds while maintaining the elevated temperature to prepare quantum dots.
[0063] When the temperature of the first mixture is rapidly raised to the reaction temperature, the first cation precursor and the first anion precursor in the solution rapidly react with each other and grow to prepare quantum dot cores having uniform shapes. In particular, the indium oxide clusters contained in the first solution have the advantage of excellent optical durability of quantum dots because the core distribution is more uniform and the peak-to-valley (PV) ratio is 0.6 or less.
[0064] As with rapid heating, heat treatment is also performed by radiant heat generated by the lamp of the rapid heating device. Heat treatment can be performed at 300°C or higher for 1 to 10 seconds, within which the quantum dot synthesis time can be significantly shortened to obtain quantum dots with small size distribution and excellent optical efficiency. As the heat treatment time increases, the particle size increases due to inter-particle aggregation, the size distribution increases, and the half-peak full width increases.
[0065] In the quantum dot preparation method according to an embodiment of the present invention, at least one of the first solution and the second solution includes two or more precursors, and the first solution may include indium oxide clusters and zinc oxide clusters to form quantum dots including at least three or more elements (such as indium (In), zinc (Zn) and phosphorus (P)).
[0066] Next, although Figure 1 Although not shown, a heat treatment process may be additionally performed by mixing the first mixture at a raised temperature with trioctylphosphine (TOP) and then maintaining the mixture at a temperature of 300° C. or higher for 10 seconds or longer. This process is not a necessary process for improving the reactivity of the surface of the synthesized core, but is intended to improve the reactivity and enable the subsequent shell synthesis process to proceed smoothly.
[0067] Next, the first mixture with the increased temperature is cooled to 100°C or less within 1 minute to form a core (S140). That is, a step of rapidly cooling the product after the heat treatment is also included. Rapid cooling can be performed by removing the heat source and cooling to room temperature, and in some cases, rapid cooling can be performed by air cooling or water cooling. Specifically, the first mixture that is rapidly heated to 300°C or more can be directly transferred to a cooling tank filled with cooling water and rapidly cooled to 100°C or less within 1 minute.
[0068] The first mixture including the core prepared by step S140 includes indium oxide clusters, and thus can be used as the core solution itself in the subsequent quantum dot shell formation step without the need for a separate purification process such as centrifugation after cooling to room temperature. Since a separate purification process such as centrifugation is not required, the process can be simplified, raw materials can be reduced, and processing time can be shortened, which has a favorable effect on the productivity of quantum dots.
[0069] In addition, despite Figure 1 Although not shown in the figure, the size of the core can be controlled by additionally adding the first cation precursor and the first anion precursor to the core prepared by step S140. Specifically, the method may further include the following steps: further adding the first sub-solution containing the first cation precursor and the second sub-solution containing the first anion precursor to the core prepared by the above step S140 at room temperature to prepare a first sub-mixture, rapidly raising the temperature of the first sub-mixture to 300° C. to 350° C. within 1 minute, heat-treating the first sub-mixture with the raised temperature for 10 seconds to 5 minutes, and cooling the heat-treated first sub-mixture to 100° C. or less within 1 minute.
[0070] At this time, the preparation of the first sub-mixture, the rapid increase of the temperature of the first sub-mixture, and the cooling of the first sub-mixture may be performed in substantially the same manner as steps S120, S130, and S140, respectively, and thus repeated descriptions are omitted.
[0071] The first sub-solution and the second sub-solution may be the same as the first solution and the second solution prepared in step S110, but are not limited thereto. For example, the first sub-solution and the second sub-solution may contain a first cation precursor and a first anion precursor, respectively, but the contents thereof may be different from each other.
[0072] At the same time, the first sub-mixture with the increased temperature is heat-treated for 10 seconds to 5 minutes so that the preformed nuclei can grow additionally. Unlike the step of forming nuclei through the initial steps S110 to S140, forming nuclei by additionally agglomerating particles on the surface of the preformed nuclei requires sufficient heat treatment time.
[0073] The size and wavelength of the core prepared by this additional process can be changed. In addition, the following steps can be repeated: preparing the first sub-mixture, rapidly increasing the temperature of the first sub-mixture, heat treating the first sub-mixture, and cooling the first sub-mixture. The size and wavelength of the core prepared by the repeated process can be appropriately adjusted.
[0074] Figure 2 is a flow chart schematically illustrating a shell formation process in a method for preparing quantum dots according to an embodiment of the present invention. Figure 2 Shown by Figure 1 The method for preparing quantum dots according to the illustrated embodiment is a process for forming a shell in the core of the quantum dots prepared.
[0075] refer to Figure 2 , the method for preparing quantum dots according to an embodiment of the present invention includes the following steps: preparing a third solution containing at least one second cation precursor and a fourth solution containing at least one second anion precursor (S210), mixing the third solution, the fourth solution and the solution containing the core at 20°C to 100°C to prepare a second mixture (S220), quickly increasing the temperature of the second mixture to 350°C to 370°C within 1 minute (S230), and cooling the second mixture with the increased temperature to 100°C or less within 1 minute to form a shell on the surface of the core (S240).
[0076] Hereinafter, the quantum dot preparation method of the present invention will be described step by step in detail.
[0077] First, a third solution containing at least one second cation precursor and a fourth solution containing at least one second anion precursor are prepared ( S210 ).
[0078] At this time, at least one of the third solution and the fourth solution may include two or more precursors. For example, the third solution may include two types of cationic precursors, and the fourth solution may also include two types of anionic precursors, but is not limited thereto.
[0079] The second cation precursor may include zinc (Zn), cadmium (Cd), mercury (Hg), indium (In), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe), or strontium (Sr).
[0080] Specifically, the second cation precursor can be selected from zinc (Zn), cadmium (Cd), mercury (Hg), indium (In), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) or strontium (Sr) oxide, peroxide, sulfate, halide, oleate, perchlorate, carboxylate, acetate, phosphate, acetylacetonate, cyanide, carbonate or nitrate, but is not limited thereto. More specifically, the second cation precursor can include zinc oleate (Zn-OA).
[0081] The second anion precursor may include sulfur (S), selenium (Se), phosphorus (P), tellurium (Te), arsenic (As), nitrogen (N), or antimony (Sb).
[0082] For example, the second anion precursor can be selected from sulfur, trialkylphosphine sulfide, trialkenylphosphine sulfide, alkylaminosulfide, alkenylaminosulfide, alkylthiol, selenium, trialkylphosphine selenide, trialkenylphosphine selenide, alkylaminoselenide, alkenylaminoselenide, trialkylphosphine telluride, trialkenylphosphine telluride, alkylaminotelluride, alkynylaminotelluride, alkylphosphine, tri(trialkylsilyl)phosphine, tri(dialkylsilyl)phosphine, tri(dialkylamino)phosphine, arsenic oxide, arsenic chloride, arsenic sulfate, arsenic bromide, arsenic iodide, nitric oxide, nitric acid and ammonium nitrate, but is not limited thereto. More specifically, the second anion precursor can include trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP).
[0083] The preparation of the third solution can also include mixing the second cation precursor and unsaturated fatty acids, and then raising the temperature of the mixture to form a more suitable second cation precursor. By comprising a long-chain unsaturated fatty acid part, the second cation precursor of the above preparation can keep a more stable dispersed form. For example, the unsaturated fatty acids can be selected from myristic acid, oleic acid, stearic acid, lauric acid and palmitic acid, and in view of the dispersion stability, size distribution and luminescent properties of quantum dots, oleic acid can be preferably used, but is not limited thereto.
[0084] The preparation of the third solution includes preparing zinc oleate (Zn-OA). Specifically, the preparation of zinc oleate (Zn-OA) may include the following steps: mixing zinc acetate dihydrate and oleic acid, then raising the temperature of the mixture to 190° C. under vacuum, raising the temperature to 260° C. by adding trioctylamine (TOA), and then cooling the mixture, so that the third solution includes zinc oleate (ZnOA), but is not limited thereto.
[0085] By considering the emission wavelength of the quantum dots finally formed, the composition ratio of zinc (Zn) and oleic acid in the third solution can be appropriately controlled. For example, the molar ratio of zinc and oleic acid can be 1:1.3 to 1:1.7, preferably 1:1.5, but not limited thereto.
[0086] The preparation of the 4th solution can also include mixing anion precursor and trialkylphosphine, and then raising the temperature of the mixture to form more suitable anion precursor. The anion precursor prepared in this way has better dispersion stability by comprising long-chain trialkylphosphine ligand. For example, the trialkylphosphine can be selected from trihexylphosphine, trioctylphosphine and tridecylphosphine, and considering dispersion stability etc., trioctylphosphine can be preferably used, but is not limited to this.
[0087] Specifically, the fourth solution is prepared by mixing selenium, sulfur and trioctylphosphine and then raising the temperature to 100° C. to 150° C., wherein the fourth solution includes trioctylphosphine sulfide and trioctylphosphine selenide, but is not limited thereto.
[0088] By considering the emission wavelength of the quantum dots finally formed, the composition ratio of sulfur (S) and selenium (Se) in the fourth solution can be appropriately controlled. For example, the molar ratio of sulfur and selenium can be 1:1 to 1:2.5, preferably 1:1.4 to 1:2.0, but is not limited thereto.
[0089] Next, it includes preparing a second mixture by mixing the third solution and the fourth solution with the solution containing the core at 20° C. to 100° C. ( S220 ).
[0090] Specifically, the third solution containing the second cation precursor and the fourth solution containing the second anion precursor may be mixed at a relatively low temperature of 20° C. to 100° C. (more preferably 80° C. to 100° C.). At this time, by mixing the third solution, the fourth solution, and the synthesized core solution at a relatively low temperature, the chemical reaction between the cation precursor and the anion precursor may be suppressed.
[0091] The solvent can mix the second cation precursor of the third solution and the third anion precursor of the fourth solution, and any non-reactive solvent can be appropriately selected and used without particular limitation. Specifically, the solvent can be a primary alkylamine having 6 to 22 carbon atoms, such as hexadecylamine; a secondary alkylamine having 6 to 22 carbon atoms, such as dioctylamine; a tertiary alkylamine having 6 to 40 carbon atoms, such as trioctylamine; a nitrogen-containing heterocyclic compound, such as pyridine; an aliphatic hydrocarbon (alkane, alkene, alkyne, etc.) having 6 to 40 carbon atoms, such as hexadecane, octadecane, octadecene and squalane; an aromatic hydrocarbon having 6 to 30 carbon atoms, such as phenyldodecane, phenyltetradecane and phenylhexadecane; a phosphine substituted with an alkyl having 6 to 22 carbon atoms, such as trioctylphosphine; a phosphine oxide substituted with an alkyl having 6 to 22 carbon atoms, such as trioctylphosphine oxide; an aromatic ether having 12 to 22 carbon atoms, such as phenyl ether and benzyl ether; and combinations thereof, but not limited thereto. Preferably, the solvent may be an aliphatic hydrocarbon having 6 to 40 carbon atoms, such as octadecene and squalane.
[0092] As another example, the solvent may be added in advance in the third solution preparation step and / or the fourth solution preparation step. Specifically, for example, when preparing the third solution, zinc acetate and oleic acid may be mixed, and then the temperature may be raised to 190° C., and then the solvent may be added.
[0093] Next, the temperature of the second mixture is rapidly increased to 350° C. to 400° C. within 1 minute ( S230 ).
[0094] In step S230, the temperature of the second mixture is rapidly raised to 350° C. to 400° C. or 350° C. to 370° C. within 120 seconds, preferably within 60 seconds. In this case, there are advantages of greatly shortening the synthesis time and facilitating large-scale production. In addition, the quantum dots prepared by rapidly raising the temperature have the advantages of uniform particle size distribution, narrow half-maximum full width and excellent quantum efficiency.
[0095] As another example, in step S230, the rapid increase in temperature may be completed within a range of 15 to 80 seconds (preferably 30 to 60 seconds), within which there are advantages in both productivity and quantum dot quality.
[0096] More specifically, for example, in step S230 , the temperature of the second mixture at 20° C. to 100° C. may be rapidly increased to 350° C. to 370° C. within 60 seconds.
[0097] The rapid increase in temperature can be carried out using a rapid heating device. For example, the second mixture can be rapidly heated using the radiant heat generated by a lamp. At this time, a halogen lamp, a tungsten halogen lamp, or a xenon arc lamp can be used to rapidly increase the temperature of the second mixture.
[0098] The temperature of the second mixture may be increased to 350° C. or higher, preferably 350° C. to 370° C. If the increased temperature is lower than 350° C., quantum dots may not be stably synthesized, the reaction time may become very long, and the particle size distribution may increase. If the temperature exceeds 370° C., the purity of the quantum dots may be reduced due to reaction with trace amounts of oxygen or moisture present in the reactor or other side reactions.
[0099] Next, although Figure 2 Although not shown in the schematic flow chart of , the second mixture is heat-treated at 350° C. to 400° C. for 30 seconds to 5 minutes while maintaining the elevated temperature to prepare quantum dots.
[0100] When the temperature of the second mixture is rapidly increased to reach the reaction temperature, the second cation precursor and the second anion precursor in the solution rapidly react with each other and grow to prepare quantum dots including a shell having an alloy shape. The quantum dots having an alloy shape have the advantage of excellent optical durability of quantum dots because the quantum dots have no shell boundaries and the shells are uniformly distributed to minimize lattice constant mismatch.
[0101] As with rapid heating, heat treatment is also performed by radiant heat generated by the lamp of the rapid heating device. Heat treatment can be performed at 350°C to 370°C for 30 seconds to 5 minutes, within which the quantum dot synthesis time can be significantly shortened to obtain quantum dots with small size distribution and high optical efficiency. As the heat treatment time increases, the particle size increases due to inter-particle aggregation, and the size distribution increases to increase the half-peak full width.
[0102] In the method for preparing quantum dots according to an embodiment of the present invention, since at least one of the third solution and the fourth solution includes two or more precursors, quantum dots are formed by including a shell consisting of at least three or more elements. For example, the quantum dots prepared by the preparation method according to an embodiment of the present invention have a single shell shape consisting of three or more elements (such as Zn-Se-S).
[0103] Next, the second mixture with the increased temperature is cooled to 100°C or less within 1 minute to form a shell on the core surface (S240). That is, the step of rapidly cooling the product after the heat treatment is also included. Rapid cooling can be performed by removing the heat source and cooling to room temperature, and in some cases, rapid cooling can be performed by air cooling or water cooling. Specifically, the second mixture whose temperature is rapidly increased to 350°C to 370°C can be directly moved to a cooling tank filled with cooling water after the heat treatment step, and rapidly cooled to 100°C or less within 1 minute.
[0104] The product cooled to room temperature can be washed and purified to obtain quantum dots with the desired purity. Washing and purification can include adding a non-solvent to the resultant to separate the quantum dots. The non-solvent is a polar solvent mixed with the organic solvent used in the reaction, but may not disperse the quantum dots, and can be acetone, ethanol, butanol, isopropanol, ethylene glycol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), ether or formaldehyde, but is not limited thereto. In addition, purification can include separating the quantum dots by methods such as centrifugation, precipitation, chromatography or distillation. In addition, the quantum dots can be redispersed in a solvent after purification.
[0105] In the method for preparing quantum dots according to an embodiment of the present invention, since the first solution uses indium oxide clusters and zinc oxide clusters as the first cationic precursors, the first solution containing the first cationic precursor and the second solution containing the first anionic precursor are first mixed at a low temperature to prepare a first mixture, and then the first mixture reacts rapidly in a short time through rapid heating and heat treatment to form quantum dots with uniform cores.
[0106] Unlike the conventional preparation method of injecting an anion precursor solution into a cationic precursor solution at a temperature of 100° C. or higher, and then reacting at 200° C. to 280° C. for a period of time to prepare uniformly distributed cores, the quantum dot preparation method according to an embodiment of the present invention can prepare quantum dots by mixing the cationic precursor and the anionic precursor at a low temperature, rapidly heating to 300° C. or higher, and then rapidly cooling, thereby having the advantages of shortening the reaction time and the cooling time and facilitating large-scale production.
[0107] In addition, the conventional quantum dot preparation method using the high temperature injection method can prepare quantum dots containing three or more elements by one reaction, but there is a problem that the energy cost consumed by heating the reaction solution to a high temperature of 300°C or higher increases rapidly as the scale of synthesis increases. The quantum dot preparation method according to an embodiment of the present invention provides the advantage of mass production of quantum dots with a relatively small amount of heat treatment by rapidly heating and heat-treating a precursor solution using radiant heat generated by a lamp.
[0108] In addition, unlike the conventional quantum dot preparation method having a core-shell structure (in which a core is formed and then obtained through a purification process such as centrifugation), in the quantum dot preparation method according to an embodiment of the present invention, the core solution prepared without centrifugation is used as is to simplify the process and minimize waste liquid, thereby having the effect of reducing costs and shortening process time, which is advantageous in terms of quantum dot productivity.
[0109] In addition, compared with quantum dots having a traditional core-shell structure, the quantum dots prepared by the method for preparing quantum dots according to an embodiment of the present invention have a narrow half-maximum full width. When the cationic precursor includes indium oxide clusters and zinc oxide clusters, the first mixture can be quickly heated and quickly cooled to prepare a uniform core, thereby reducing lattice fatigue and narrowing the half-maximum full width. In addition, even in the process of forming a shell on the core surface, a uniform alloy shell can be formed by mixing the cationic precursor and the anionic precursor at a low temperature, and then performing a rapid heating and rapid cooling process to narrow the half-maximum full width. In particular, during the shell formation process, the ratio of zinc (Zn) and oleic acid (OA) is adjusted to 1: 1.5 to narrow the half-maximum full width. Therefore, the method for preparing quantum dots according to an embodiment of the present invention can have a high quantum efficiency.
[0110] In addition, the quantum dots prepared by the method for preparing quantum dots according to the embodiment of the present invention may ensure optical stability and thermal stability by performing a heat treatment process at a high temperature of 350° C. or higher.
[0111] In addition, in the prior art, since the wavelength of the core determines the wavelength of the final quantum dot, if the wavelength does not match, it is necessary to synthesize the core first, so there is a problem of increased cost and increased defect rate. In contrast, the method for preparing quantum dots according to an embodiment of the present invention can not only adjust the ratio of the indium oxide cluster (In-Oxo) and the zinc oxide cluster (Zn-Oxo) of the core, but also adjust the ratio of zinc (Zn) and oleic acid (OA) of the shell, or the ratio of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (Se-TOP) to control the wavelength. That is, a single core can be used to synthesize quantum dots of various wavelength ranges, and on the contrary, cores of various wavelengths can also be used to synthesize quantum dots of the same wavelength range. Therefore, even if the wavelength formed in the core does not match, the wavelength can be controlled during the shell formation process to have the effect of minimizing defect rate, reducing cost and shortening processing time, which is very advantageous in terms of productivity. Example 1-1: Synthesis of red fluorescent quantum dot cores
[0112] Figure 3 Schematic diagram for describing a method for preparing quantum dots according to an embodiment of the present invention. Figure 3 , examples of the present invention will be described.
[0113] First, 63 g (216.0 mmol) of indium (III) acetate and 183 g (648.0 mmol) of oleic acid were mixed in a 2 L container, heated to 200 ° C under vacuum, then changed to normal pressure, octadecene (ODE) was added, and synthesized at 260 ° C to 300 ° C for 1 hour or more to prepare a first cationic precursor of an indium oxide cluster.
[0114] 200 g (57.6 mmol) of the prepared indium oxide cluster solution was added to a 1 L quartz container, and 48 g (38.4 mmol) of TMSP (20 wt % in TOP) was added at 130° C. to prepare a first mixture. At this time, the molar ratio of indium (In) to phosphorus (P) of the first mixture was 1.5:1.
[0115] Next, the first mixture of the first cation precursor and the first anion precursor is rapidly heated to 300° C. at a rate of about 200° C. per minute using radiant heat, and then the heat-treated first mixture is rapidly cooled to 100° C. or less within 1 minute to form quantum dot cores. Example 1-2: Synthesis of red fluorescent quantum dot cores
[0116] In the quantum dot preparation method according to Example 1-2, 100 g (28.8 mmol) of indium oxide cluster solution and 36 g (28.8 mmol) of TMSP (20 wt % in TOP) are further added to the solution containing the quantum dot core prepared in Example 1-1, and the mixture is rapidly heated to 300° C. by using radiant heat at a rate of approximately 200° C. per minute, and then the heat-treated mixture is rapidly cooled to 100° C. or less within 1 minute to form a quantum dot core. Example 1-3: Synthesis of red fluorescent quantum dot cores
[0117] In the method for preparing quantum dots according to Example 1-3, 100 g (28.8 mmol) of an indium oxide cluster solution and 36 g (28.8 mmol) of TMSP (20 wt % in TOP) were further added to the solution containing the quantum dot cores prepared in Example 1-2, and the mixture was rapidly heated to 300° C. by increasing the temperature at a rate of about 200° C. per minute using radiant heat, and then reacted for 1 minute while maintaining the same temperature. Thereafter, the heat-treated mixture was rapidly cooled to 100° C. or less within 1 minute to form a quantum dot core. Example 1-4: Synthesis of red fluorescent quantum dot cores
[0118] In the quantum dot preparation method according to Example 1-4, 100 g (28.8 mmol) of indium oxide cluster solution and 36 g (28.8 mmol) of TMSP (20 wt % in TOP) were further added to the solution containing the quantum dot core prepared in Example 1-3, and rapidly heated to 300° C. by increasing the temperature at a rate of about 200° C. per minute using radiant heat, and then reacted for 1 minute while maintaining the same temperature. Thereafter, the heat-treated mixture was rapidly cooled to 100° C. or less within 1 minute to form a quantum dot core. Example 1-5: Synthesis of red fluorescent quantum dot cores
[0119] In the quantum dot preparation method according to Example 1-5, 50 g (14.4 mmol) of indium oxide cluster solution and 18 g (14.4 mol) of TMSP (20 wt% in TOP) were further added to the solution containing the quantum dot core prepared in Example 1-4, and rapidly heated to 300° C. by increasing the temperature at a rate of about 200° C. per minute using radiant heat, and then reacted for 1 minute while maintaining the same temperature. Thereafter, the heat-treated mixture was rapidly cooled to 100° C. or less within 1 minute to form a quantum dot core. Example 1-6: Synthesis of red fluorescent quantum dot cores
[0120] In the quantum dot preparation method according to Example 1-6, 50 g (14.4 mmol) of indium oxide cluster solution and 18 g (14.4 mol) of TMSP (20 wt % in TOP) were further added to the solution containing the quantum dot core prepared in Example 1-5, and rapidly heated to 300° C. at a rate of about 200° C. per minute by using radiant heat, and then reacted for 1 minute while maintaining the same temperature. Thereafter, the heat-treated mixture was rapidly cooled to 100° C. or less within 1 minute to form a quantum dot core. Example 2-1: Synthesis of green fluorescent quantum dot cores
[0121] First, 63 g (216.0 mmol) of indium (III) acetate and 183 g (648.0 mmol) of oleic acid were mixed in a 2 L container, heated to 200 ° C under vacuum, then changed to normal pressure, octadecene (ODE) was added, and synthesized at 260 ° C to 300 ° C for 1 hour or more to prepare a first cationic precursor of an indium oxide cluster.
[0122] Next, 47 g (216.0 mmol) of zinc acetate dihydrate and 122 g (432.0 mmol) of oleic acid were mixed in a 1 L container, heated to 190 ° C under vacuum, then changed to normal pressure, octadecene (ODE) was added, and synthesized at 300 ° C to 315 ° C for 1 hour or more to prepare a first cationic precursor of a zinc oxide cluster.
[0123] 180 g (51.8 mmol) of the prepared indium oxide cluster solution and 43 g (23.0 mmol) of the zinc oxide cluster solution were mixed in a 1 L quartz container, heated to 100° C. under a N2 atmosphere, and 36 g (28.8 mmol) of TMSP (20 wt % in TOP) was added to prepare a first mixture. At this time, the molar ratio of indium (In): zinc (Zn): phosphorus (P) of the first mixture was 1.8:0.8:1.
[0124] Next, the first mixture of the first cation precursor and the first anion precursor is rapidly heated to 300° C. at a rate of about 200° C. per minute using radiant heat, and then reacted for 0 to 10 seconds while maintaining the same reaction temperature. Thereafter, the heat-treated first mixture is rapidly cooled to 100° C. or less within 1 minute to form a core solution. Example 2-2: Synthesis of green fluorescent quantum dot cores
[0125] The method for preparing quantum dots according to Example 2-2 is substantially the same as the method for preparing quantum dots according to Example 2-1 in other configurations except that the synthesis ratio of the indium oxide clusters and the zinc oxide clusters is different, and thus repeated descriptions are omitted.
[0126] In the quantum dot preparation method according to Example 2-2, an indium oxide cluster solution and a zinc oxide cluster solution are mixed in a 1L quartz container so that the molar ratio of indium (In): zinc (Zn): phosphorus (P) is 1.8:1.2:1, heated to 100°C under a N2 atmosphere, and TMSP (20 wt% in TOP) is added to prepare a first mixture. Example 2-3: Synthesis of green fluorescent quantum dot cores
[0127] The method for preparing quantum dots according to Example 2-3 is substantially the same as the method for preparing quantum dots according to Example 2-1 in other configurations except that the synthesis ratio of the indium oxide clusters and the zinc oxide clusters is different, and thus repeated descriptions are omitted.
[0128] In the quantum dot preparation method according to Example 2-3, the indium oxide cluster solution and the zinc oxide cluster solution were mixed in a 1L quartz container so that the molar ratio of indium (In): zinc (Zn): phosphorus (P) was 1.5:0.8:1, heated to 100°C under a N2 atmosphere, and TMSP (20 wt% in TOP) was added to prepare a first mixture. Example 2-4: Synthesis of Green Fluorescent Quantum Dot Cores
[0129] The method for preparing quantum dots according to Example 2-4 is substantially the same as the method for preparing quantum dots according to Example 2-1 in other configurations except that the synthesis ratio of the indium oxide clusters and the zinc oxide clusters is different, and thus repeated descriptions are omitted.
[0130] In the quantum dot preparation method according to Example 2-4, the indium oxide cluster solution and the zinc oxide cluster solution were mixed in a 1L quartz container so that the molar ratio of indium (In): zinc (Zn): phosphorus (P) was 1.2:0.8:1, heated to 100°C under a N2 atmosphere, and TMSP (20 wt% in TOP) was added to prepare a first mixture. Example 2-5: Synthesis of Green Fluorescent Quantum Dot Cores
[0131] The method for preparing quantum dots according to Example 2-5 is substantially the same as the method for preparing quantum dots according to Example 2-1 in other configurations except that the synthesis ratio of the indium oxide clusters and the zinc oxide clusters is different, and thus repeated descriptions are omitted.
[0132] In the quantum dot preparation method according to Example 2-5, the indium oxide cluster solution and the zinc oxide cluster solution were mixed in a 1L quartz container so that the molar ratio of indium (In): zinc (Zn): phosphorus (P) was 1.2:1.2:1, heated to 100°C under a N2 atmosphere, and TMSP (20 wt% in TOP) was added to prepare a first mixture. Comparative Example 1: Synthesis of core prepared by conventional method
[0133] The quantum dot preparation method according to Comparative Example 1 is a conventional method, except that indium oleate (In-OA) solution and zinc oleate (Zn-OA) solution are used as the first cation precursor instead of indium oxide cluster solution and zinc oxide cluster solution and only a different synthesis ratio is used. The other configurations are basically the same as the quantum dot preparation method according to Example 2-1, so the repeated description will be omitted.
[0134] In the quantum dot preparation method according to Comparative Example 1, an indium oleate solution and a zinc oleate solution were mixed in a 1 L quartz container so that the molar ratio of indium (In): zinc (Zn): phosphorus (P) was 1.5:0.8:1, heated to 100° C. under a N2 atmosphere, and TMSP (20 wt % in TOP) was added to prepare a first mixture. Experimental Example 1-Performance Evaluation
[0135] The wavelength (core λ) and PV (peak-to-valley) values of the cores prepared according to the preparation methods of Examples 1-1 to 2-5 and Comparative Example 1 were measured. The detailed results are shown in Tables 1 and 2 below. Table 1 describes the measurement of the cores of the red fluorescent quantum dots prepared in Examples 1-1 to 1-6, while Table 2 describes the measurement of the cores of the green fluorescent quantum dots prepared in Examples 2-1 to 2-5 and Comparative Example 1.
[0136] [Table 1]
[0137] First, the core of the red fluorescent quantum dots prepared according to the preparation method of Examples 1-1 to 1-6 uses indium oxide clusters (In Oxo clusters) as cationic precursors and TMSP as anionic precursors. At this time, referring to Table 1, it can be confirmed that due to the uniform distribution of the core, the cores prepared according to the preparation methods of Examples 1-1 to 1-6 all have excellent P / V (peak-to-valley) values of 0.6 or less. In addition, by differently controlling the molar ratio of indium (In): phosphorus (P) and the amount of precursor added, the core wavelength (core λ) has different values. That is, it can be confirmed that the wavelength can be controlled by the ratio of indium oxide clusters and TMSP, the amount of precursor added, and the number of precursor additions. Therefore, it can be seen that the quantum dots prepared according to the preparation methods of Examples 1-1 to 1-6 can easily control the wavelength, thereby ensuring quality stability and having excellent reproducibility.
[0138] [Table 2]
[0139] The core prepared according to the preparation method of Examples 2-1 to 2-5 is obtained by mixing a cation precursor and an anion precursor including an indium oxide cluster and a zinc oxide cluster at a low temperature, rapidly heating the mixture to 300°C or higher within 1 minute, and then rapidly cooling the heated mixture. Referring to Table 2, due to the uniform distribution of the core, the cores prepared according to the preparation methods of Examples 2-1 to 2-5 all have a good P / V (peak-to-valley) value of 0.6 or less. In particular, it can be confirmed that even if the ratio of indium (In): zinc (Zn): phosphorus (P) is the same as that of Example 2-3, the core prepared according to the preparation method of Comparative Example 1, i.e., prepared by a conventional method, has a P / V value of 0.71, so Examples 2-1 to 2-5 of the present invention using an indium oxide cluster solution and a zinc oxide cluster solution are excellent. In addition, by differently controlling the ratio of indium (In): zinc (Zn): phosphorus (P), the core wavelength (core λ) has different values. That is, it can be confirmed that the wavelength can be controlled according to the amount and molar ratio of the oxygen cluster precursor added. Therefore, it can be seen that the quantum dots prepared according to the preparation methods of Examples 2-1 to 2-5 can easily control the wavelength, thereby ensuring quality stability and having excellent reproducibility. Example 3: Synthesis of a shell on the surface of a green fluorescent quantum dot core
[0140] Figure 4 Schematic diagram for describing a method for preparing quantum dots according to an embodiment of the present invention. Figure 4 , examples of the present invention will be described.
[0141] First, 2063 g (9396.0 mmol) of zinc acetate dihydrate and 3981 g (14094.0 mmol) of oleic acid were mixed in a 20 L container, heated to 190 ° C and stirred under vacuum, and then 3608 g of trioctylamine (TOA) was added, heated to 260 ° C and cooled to prepare a second cationic precursor of zinc oleate (Zn-OA). At this time, the molar ratio of zinc (Zn) to oleic acid (OA) in zinc oleate (Zn-OA) was 1:1.5.
[0142] Next, 948 g (12000.0 mmol) of selenium (Se) powder and 5485 g (6.6 L) of trioctylphosphine (TOP) were mixed in a 10 L container, heated to 250 ° C in vacuum under N2 atmosphere, stirred until completely dissolved, and then cooled to prepare the second anion precursor (Se-TOP) of trioctylphosphine selenide.
[0143] Next, 769.68 g (24000.0 mmol) of sulfur (S) powder and 10637 g (12.8 L) of trioctylphosphine (TOP) were mixed in a 30 L container, heated to 150° C. in vacuum under N2 atmosphere, stirred until completely dissolved, and then cooled to prepare a second anion precursor of trioctylphosphine sulfide (S-TOP).
[0144] In addition, 273 g (313.2 mmol of Zn) of zinc oleate (Zn OA) with a zinc (Zn): oleic acid (OA) ratio of 1:1.5 and 4 g of trioctylphosphine (TOP) were mixed with 35 g of the core solution of Example 2-2 with indium (In): zinc (Zn): phosphorus (P) ratio of 1.8:1.2:1 in a 1L quartz container, stirred, and then 21 g (39.1 mmol) of pre-prepared trioctylphosphine selenide and 27 g (56.7 mmol) of trioctylphosphine sulfide were added at room temperature of 20°C to 24°C to prepare a second mixture.
[0145] Next, the second mixture of the core solution obtained in Example 2-2, the second cation precursor, and the second anion precursor was quickly heated to 370° C. by using radiant heat to increase the temperature by about 200° C. per minute, and then reacted for 30 seconds to 5 minutes while maintaining the temperature at 350° C. to 370° C. Thereafter, the heat-treated second mixture was quickly cooled to 100° C. or less within 1 minute to obtain quantum dots having a ZnSeS shell formed on the surface of the InZnP core. Comparative Example 2-1: Synthesis of a shell on the core surface of a green fluorescent quantum dot
[0146] The quantum dot manufacturing method according to Comparative Example 2-1 is substantially the same as the quantum dot manufacturing method according to Example 3 in other configurations except that the synthesis ratio of zinc (Zn) and oleic acid (OA) is different, and thus repeated descriptions are omitted.
[0147] In Comparative Example 2-1, 2063 g (9396.0 mmol) of zinc acetate dihydrate and 5308 g (18792.0 mmol) of oleic acid were mixed in a 20 L container, heated to 190° C. and stirred under vacuum, and then 3608 g of trioctylamine (TOA) was added, heated to 260° C. and cooled to prepare a second cationic precursor of zinc oleate (Zn-OA). At this time, the molar ratio of zinc (Zn) to oleic acid (OA) in zinc oleate (Zn-OA) was 1:2. Comparative Example 2-2: Synthesis of a shell on the core surface of green fluorescent quantum dots
[0148] The quantum dot manufacturing method according to Comparative Example 2-2 is substantially the same as the quantum dot manufacturing method according to Example 3 in other configurations except that the synthesis ratio of zinc (Zn) and oleic acid (OA) is different, and thus repeated descriptions are omitted.
[0149] In Comparative Example 2-2, zinc acetate dihydrate and oleic acid were mixed in a 20 L container so that the molar ratio of zinc (Zn) to oleic acid (OA) of zinc oleate (Zn-OA) was 1:1, heated to 190° C. and stirred under vacuum, and then 3608 g of trioctylamine (TOA) was added, heated to 260° C. and cooled to prepare a second cationic precursor of zinc oleate (Zn-OA). Comparative Example 2-3: Synthesis of a shell on the core surface of a green fluorescent quantum dot
[0150] The quantum dot manufacturing method according to Comparative Example 2-3 is substantially the same as the quantum dot manufacturing method according to Example 2-1 in other configurations except for the heating rate of the second mixture, and thus repeated descriptions are omitted.
[0151] In Comparative Example 2-3, the second mixture in which the core solution, the second cation precursor, and the second anion precursor were mixed was slowly heated to 370° C. by increasing the temperature by about 15° C. per minute using heat conduction, and then reacted for 30 seconds to 5 minutes while maintaining the temperature at 350° C. to 370° C. Thereafter, the heat-treated second mixture was rapidly cooled to 100° C. or less within 1 minute to obtain quantum dots having a shell formed on the core surface. Experimental Example 2-Performance Evaluation
[0152] The maximum peak wavelength (PL Max), full width at half maximum (FWHM) and quantum efficiency (QY) of the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-1 and 2-2 were measured. The specific results are shown in Table 3 below.
[0153] [Table 3]
[0154] Except for the different molar ratios of zinc (Zn) and oleic acid (OA), the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-1 and 2-2 have the same other configurations. Referring to Table 3, according to the preparation method of Example 3, the quantum dots having a molar ratio of zinc (Zn) and oleic acid (OA) of 1:1.5 have a narrow full width at half maximum (FWHM) of 34nm and a high quantum efficiency (QY) of 95%. In contrast, according to the preparation method of Comparative Example 2-1, the quantum dots having a molar ratio of zinc (Zn) and oleic acid (OA) of 1:2 have a quantum efficiency (QY) of 96%, similar to Example 2-2, but a full width at half maximum (FWHM) of 37nm. In addition, according to the preparation method of Comparative Example 2-2, the quantum dots having a molar ratio of zinc (Zn) and oleic acid (OA) of 1:1 have a full width at half maximum (FWHM) of 33nm, similar to Example 2-1, but a lower quantum efficiency (QY) of 84%. Therefore, it can be confirmed that the molar ratio of zinc (Zn) and oleic acid (OA) in zinc oleate (ZnOA), which is the second cation precursor required in the process of forming a shell on the core surface, is preferably 1:1.5.
[0155] In addition, since the molar ratio of zinc (Zn) and oleic acid (OA) is controlled differently, the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-1 and 2-2 have different maximum peak wavelengths (PL Max). That is, it can be confirmed that the wavelength can be controlled according to the addition amount and molar ratio of the second cationic precursor composed of zinc acetate and oleic acid. Therefore, even if the core wavelength range is fixed by a single core, various wavelengths can be synthesized by adjusting the ratio of zinc (Zn) and oleic acid (OA). In other words, a single core can be used to synthesize quantum dots of various wavelength ranges, and on the contrary, cores in various wavelength ranges can also be used to synthesize quantum dots of the same wavelength range, thereby minimizing the defect rate. Experimental Example 3-Performance Evaluation
[0156] The maximum peak wavelength (PLMax), full width at half maximum (FWHM) and quantum efficiency (QY) of the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-3 were measured. The specific results are shown in Table 4 below.
[0157] [Table 4] Example Example 3 (200°C / min) Comparative Example 2-3 (15°C / min) PL Max(nm) 530 532 FWHM(nm) 34 37 QY(%) 95 91
[0158] Except for the different heating rates of the second mixture, the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-3 have the same other configurations. That is, Example 3 is a quantum dot that reacts by rapidly heating the second mixture to 370°C by using radiant heat to increase the temperature by about 200°C per minute, while Comparative Example 2-3 is a quantum dot that reacts by slowly heating the second mixture to 370°C by using heat conduction to increase the rate by about 15°C per minute. Referring to Table 4, the quantum dots rapidly heated at a heating rate of 200°C / min in Example 3 have a narrow full width at half maximum (FWHM) of 34nm and a high quantum efficiency (QY) of 95%. In contrast, the quantum dots slowly heated at a heating rate of 15°C / min in Comparative Examples 2-3 not only have a wide full width at half maximum (FWHM) of 37nm, but also have a low quantum efficiency (QY) of 91%. Therefore, it can be confirmed that when the second mixture is quickly heated using radiant heat, excellent quantum dots with narrow full width at half maximum (FWHM) and high quantum efficiency (QY) can be obtained. In addition, the quantum dots prepared according to the preparation methods of Example 3 and Comparative Examples 2-3 have different maximum peak wavelength (PLMax) values because the heating rate of the second mixture is set differently. That is, it can be confirmed that the wavelength can be controlled according to the heating rate of the second mixture. Therefore, even if the core wavelength range is fixed by a single core, various wavelengths can be synthesized by controlling the heating rate. That is, the wavelength of the quantum dots prepared by the preparation method according to one embodiment of the present invention can be controlled not only by the content ratio of the precursor, but also by heating rate, reaction rate, reaction time, etc. Example 4-1: Synthesis of a shell on the surface of a green fluorescent quantum dot core
[0159] The quantum dot manufacturing method according to Example 4-1 is substantially the same as the quantum dot manufacturing method according to Example 3 in other configurations except for the core solution, and thus repeated descriptions are omitted.
[0160] In Example 4-1, 273 g (313.2 mmol of Zn) of zinc oleate (Zn OA) with a zinc (Zn): oleic acid (OA) ratio of 1:1.5 and 4 g of trioctylphosphine (TOP) were mixed with 34.6 g of the core solution of Example 1-1 with a indium (In): zinc (Zn): phosphorus (P) ratio of 1.8:0.8:1 in a 1L quartz container, stirred, and then 21 g (39.1 mmol) of pre-prepared trioctylphosphine selenide (Se-TOP) and 27 g (56.7 mmol) of trioctylphosphine sulfide (S-TOP) were added at room temperature of 20°C to 24°C to prepare a second mixture. Example 4-2: Synthesis of a shell on the surface of a green fluorescent quantum dot core
[0161] Except for the different synthesis ratio of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP), the quantum dot preparation method according to Example 4-2 is basically the same as the quantum dot preparation method according to Example 4-1 in other configurations, so the repeated description is omitted.
[0162] In the quantum dot preparation method according to Comparative Example 4-2, a second mixture was prepared by adding trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP) so that the molar ratio of selenium (Se):sulfur (S) was 1.0:1.96. Example 4-3: Synthesis of a shell on the surface of a green fluorescent quantum dot core
[0163] Except for the different synthesis ratio of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP), the quantum dot preparation method according to Example 4-3 is basically the same as the quantum dot preparation method according to Example 4-1 in other configurations, so the repeated description is omitted.
[0164] In the quantum dot preparation method according to Example 4-3, a second mixture was prepared by adding trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP) so that the molar ratio of selenium (Se):sulfur (S) was 1.0:2.45. Example 4-4: Synthesis of a shell on the surface of a green fluorescent quantum dot core
[0165] Except for the different synthesis ratio of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP), the quantum dot preparation method according to Example 4-4 is basically the same as the quantum dot preparation method according to Example 4-1 in other configurations, so the repeated description is omitted.
[0166] In the quantum dot preparation method according to Example 4-4, a second mixture was prepared by adding trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP) so that the molar ratio of selenium (Se):sulfur (S) was 1.5:1.45. Experimental Example 4-Performance Evaluation
[0167] The maximum peak wavelength (PL Max), full width at half maximum (FWHM) and quantum efficiency (QY) of the quantum dots prepared according to the preparation methods of Examples 4-1 to 4-4 were measured. The specific results are shown in Table 5 below.
[0168] [Table 5]
[0169] Except for the different molar ratios of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP) as anion precursors required for the process of forming a shell on the core surface, the quantum dots prepared according to the preparation methods of Examples 4-1 to 4-4 have the same other configurations. Referring to Table 5, since the ratio of selenium (Se): sulfur (S) is adjusted differently, the quantum dots prepared according to the preparation methods of Examples 4-1 to 4-4 have different maximum peak wavelengths (PL Max). That is, it can be confirmed that the wavelength can be controlled according to the addition amount and molar ratio of the second anion precursor composed of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP). Therefore, in the quantum dots according to the preparation methods of Examples 4-1 to 4-4, even if the core wavelength range is fixed by a single core, various wavelengths can be synthesized by adjusting the ratio of selenium (Se) and sulfur (S). That is, a single core can be used to synthesize quantum dots of various wavelength ranges, and conversely, cores in various wavelength ranges can also be used to synthesize quantum dots of the same wavelength range, thereby minimizing the defect rate. The display device according to various embodiments of the present invention can be described as follows.
[0170] The method for preparing quantum dots according to an embodiment of the present invention includes preparing a first solution containing at least one first cationic precursor and a second solution containing at least one first anionic precursor; mixing the first solution and the second solution at 20°C to 130°C to prepare a first mixture; raising the temperature of the first mixture to a high temperature of 300°C to 350°C within 1 minute; and cooling the first mixture with the raised temperature to 100°C or lower within 1 minute to form a core, wherein the first cationic precursor may include an indium oxide cluster (In-Oxo cluster).
[0171] According to another feature of the present invention, indium oxide clusters (In-Oxo clusters) can be prepared by the following steps: mixing indium acetate and oleic acid, raising the temperature of the mixed solution to 200°C under vacuum, then converting the pressure to normal pressure, and then adding octadecene (ODE) and synthesizing at 260°C to 300°C for 1 hour or more.
[0172] According to another feature of the present invention, the first cation precursor may further include zinc oxide clusters (Zn—Oxo clusters).
[0173] According to another feature of the present invention, zinc oxide clusters (Zn-Oxo clusters) can be prepared by mixing zinc acetate (Zn acetate) and oleic acid, raising the temperature of the mixed solution to 190°C under vacuum, then converting the pressure to normal pressure, and then adding octadecene (ODE) and synthesizing at 300°C to 315°C for 1 hour or more.
[0174] According to another feature of the present invention, preparing the first mixture may further include controlling the wavelength range of the quantum dots by adjusting the ratio of indium oxide clusters (In-Oxo clusters) and zinc oxide clusters (Zn-Oxo clusters).
[0175] According to another feature of the present invention, the first cation precursor may also include at least one of cadmium (Cd), mercury (Hg), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) and strontium (Sr).
[0176] According to another feature of the present invention, the method may further include heat-treating the first mixture at 300° C. or higher for 1 to 10 seconds between the rapid increase in temperature of the first mixture and the rapid cooling of the first mixture.
[0177] According to another feature of the present invention, the rapid temperature raising step and the heat treatment step may be performed by radiant heat using a quartz container and a halogen lamp.
[0178] According to another feature of the present invention, the method may further include mixing trioctylphosphine (TOP) with the heat-treated first mixture and heat-treating the mixture at 300° C. or higher for 10 seconds or longer to increase the surface reactivity of the core.
[0179] According to another feature of the present invention, the method may also include preparing a first sub-mixture by additionally adding a first sub-solution containing a first cation precursor and a second sub-solution containing a first anion precursor to a solution containing a core at room temperature, raising the temperature of the first sub-mixture to a high temperature of 300°C to 350°C within 1 minute, heat-treating the first sub-mixture with the raised temperature for 10 seconds to 5 minutes, and cooling the heat-treated first sub-compound to 100°C or less within 1 minute.
[0180] According to another feature of the present invention, the method may further include repeatedly preparing the first sub-mixture, rapidly increasing the temperature of the first sub-mixture, heat-treating the first sub-mixture, and cooling the first sub-mixture.
[0181] According to another feature of the present invention, the method may also include preparing a third solution containing at least one second cation precursor and a fourth solution containing at least one second anion precursor, mixing the third solution and the fourth solution with the solution containing the core at 20°C to 100°C to prepare a second mixture, rapidly raising the temperature of the second mixture to a high temperature of 350°C to 400°C within 1 minute, and cooling the second mixture with the raised temperature to 100°C or lower within 1 minute to form a shell on the surface of the core.
[0182] According to another feature of the present invention, the third solution may contain zinc oleate (Zn-OA), and the fourth solution may contain trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP).
[0183] According to another feature of the present invention, the method may further include controlling the wavelength range of the quantum dots by adjusting the molar ratio of zinc (Zn) to oleate (OA) in the third solution within a range of 1:1.3 to 1:1.7.
[0184] According to another feature of the present invention, the method may further include controlling the wavelength range of the quantum dots by adjusting the ratio of trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP) in the fourth solution.
[0185] According to another feature of the present invention, the method may further include heat treating the second mixture at 350° C. to 370° C. for 30 seconds to 5 minutes between rapid temperature increase of the second mixture and rapid cooling of the second mixture.
[0186] According to another feature of the present invention, the second cation precursor may include at least one of zinc (Zn), cadmium (Cd), mercury (Hg), indium (In), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) and strontium (Sr).
[0187] According to another feature of the present invention, the first anion precursor and the second anion precursor may include at least one of sulfur (S), selenium (Se), phosphorus (P), tellurium (Te), arsenic (As), nitrogen (N), and antimony (Sb).
[0188] Although the embodiments of the present invention have been described in detail with reference to the accompanying drawings, the present invention is not limited thereto and can be embodied in many different forms without departing from the technical concept of the present invention. Therefore, the various embodiments disclosed in the present invention are not intended to limit the technical spirit, but to describe the present invention, and the technical spirit of the present invention is not limited by the following embodiments. Therefore, it should be understood that the above-mentioned embodiments are illustrative in all aspects and do not limit the present invention. The scope of protection of the present invention should be interpreted based on the attached claims, and all technical ideas within their equivalent ranges should be interpreted as falling within the scope of the present invention.
[0189] [Sequence Listing Free Text]
[0190] [National R&D project supporting this invention]
[0191] [Project unique number] 1425157068
[0192] [Project Number]S3165227
[0193] [Department Name] Ministry of Small, Medium Enterprises and Entrepreneurship (MSS)
[0194] [Name of project management (special) agency] Korea Small and Medium Enterprise Technology and Information Promotion Agency
[0195] [Research Project Name] Entrepreneurship Growth Technology Development (Special Project, R&D)
[0196] [Research Topic Name] Development of high-efficiency and environmentally friendly mass production technology for InP quantum dots with a quantum efficiency of 90%
[0197] [Contribution] 1 / 1
[0198] [Project implementing agency name] DCT Co., Ltd.
[0199] [Study period] November 1, 2021 to October 31, 2023.
Claims
1. A method for preparing quantum dots, comprising: preparing a first solution comprising at least one first cation precursor and a second solution comprising at least one first anion precursor; preparing a first mixture by mixing the first solution and the second solution at 20° C. to 130° C.; Raising the temperature of the first mixture to a high temperature of 300° C. to 350° C. within 1 minute; as well as cooling the first mixture having an elevated temperature to 100° C. or less within 1 minute to form a core, The first cation precursor includes indium oxide clusters (In-Oxo clusters).
2. The method for preparing quantum dots according to claim 1, wherein the indium oxide cluster (In-Oxo cluster) is prepared by the following steps: Mixing indium acetate (In acetate) and oleic acid; raising the temperature of the mixed solution to 200° C. under vacuum, and then converting the pressure to normal pressure; and Octadecene (ODE) was added and synthesized at 260° C. to 300° C. for 1 hour or more.
3. The method for preparing quantum dots according to claim 1, wherein the first cation precursor further comprises zinc oxide clusters (Zn-Oxo clusters).
4. The method for preparing quantum dots according to claim 3, wherein the zinc oxide cluster (Zn-Oxo cluster) is prepared by the following steps: Mixing zinc acetate (Zn acetate) and oleic acid; raising the temperature of the mixed solution to 190° C. under vacuum, and then converting the pressure to normal pressure; and Octadecene (ODE) was added and synthesized at 300° C. to 315° C. for 1 hour or more.
5. The method for preparing quantum dots according to claim 3, wherein the preparation of the first mixture further comprises controlling the wavelength range of the quantum dots by adjusting the ratio of the indium oxide clusters (In-Oxo clusters) and the zinc oxide clusters (Zn-Oxo clusters).
6. The method for preparing quantum dots according to claim 3, wherein the first cationic precursor also includes at least one of cadmium (Cd), mercury (Hg), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) and strontium (Sr).
7. The method for preparing quantum dots according to claim 1, further comprising: Between the rapid heating of the first mixture and the rapid cooling of the first mixture, the first mixture is heat-treated at a temperature of 300° C. or higher for 1 second to 10 seconds. 8 . The method for preparing quantum dots according to claim 7 , wherein the rapid temperature increase step and the heat treatment step are performed by using a quartz container and radiant heat of a halogen lamp.
9. The method for preparing quantum dots according to claim 7, further comprising: Trioctylphosphine (TOP) is mixed with the heat-treated first mixture, and the mixture is heat-treated at a temperature of 300° C. or higher for 10 seconds or longer to increase the surface reactivity of the core.
10. The method for preparing quantum dots according to claim 1, further comprising: preparing a first sub-mixture by additionally adding a first sub-solution containing the first cation precursor and a second sub-solution containing the first anion precursor to a solution containing the core at room temperature; Raising the temperature of the first sub-mixture to a high temperature of 300° C. to 350° C. within 1 minute; heat-treating the first sub-mixture at an elevated temperature for 10 seconds to 5 minutes; and The heat-treated first sub-mixture is cooled to 100° C. or less within 1 minute.
11. The method for preparing quantum dots according to claim 10, further comprising: The preparing of the first submixture, the rapid temperature increase of the first submixture, the heat treatment of the first submixture, and the cooling of the first submixture are repeated.
12. The method for preparing quantum dots according to claim 1, further comprising: preparing a third solution containing at least one second cation precursor and a fourth solution containing at least one second anion precursor; mixing the third solution and the fourth solution with the solution containing the core at 20° C. to 100° C. to prepare a second mixture; Rapidly heating the second mixture to a high temperature of 350° C. to 400° C. within 1 minute; as well as The heated second mixture is cooled to 100° C. or less within 1 minute to form a shell on the surface of the core.
13. The method for preparing quantum dots according to claim 12, wherein the third solution contains zinc oleate (Zn-OA), and The fourth solution contains trioctylphosphine selenide (Se-TOP) and trioctylphosphine sulfide (S-TOP).
14. The method for preparing quantum dots according to claim 13, further comprising: The wavelength range of the quantum dots is controlled by adjusting the molar ratio of zinc (Zn) to oleate (OA) of the third solution within a range of 1:1.3 to 1:1.
7.
15. The method for preparing quantum dots according to claim 13, further comprising: The wavelength range of the quantum dots is controlled by adjusting the ratio of trioctylphosphine selenide (Se-TOP) to trioctylphosphine sulfide (S-TOP) in the fourth solution.
16. The method for preparing quantum dots according to claim 12, further comprising: Between the rapid heating of the second mixture and the rapid cooling of the second mixture, the second mixture is heat-treated at 350° C. to 370° C. for 30 seconds to 5 minutes.
17. The method for preparing quantum dots according to claim 12, wherein the second cation precursor comprises at least one of zinc (Zn), cadmium (Cd), mercury (Hg), indium (In), magnesium (Mg), aluminum (Al), manganese (Mn), copper (Cu), gallium (Ga), tin (Sn), barium (Ba), iron (Fe) and strontium (Sr).
18. The method for preparing quantum dots according to claim 12, wherein the first anion precursor and the second anion precursor include at least one of sulfur (S), selenium (Se), phosphorus (P), tellurium (Te), arsenic (As), nitrogen (N) and antimony (Sb).