Multilayer ceramic capacitor

By configuring a glass film and a sintered layer on the metal layer of the external electrode, and setting gaps in the sintered layer, and then covering the sintered layer with a coating film, the problem of easy cracking of the external electrode is solved, and the moisture resistance reliability of the multilayer ceramic capacitor is improved.

CN119013747APending Publication Date: 2024-11-22MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034085.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-02
Filing Date
2023-04-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors have insufficient moisture resistance and reliability of their external electrodes, mainly because the external electrodes are prone to cracking.

Method used

A glass film and a sintered layer are disposed on the metal layer of the external electrode, and voids are set in the sintered layer. A coating film covers the sintered layer, and the coating material fills the voids, forming a glass film covering the metal layer. The voids are formed by controlling the sintering temperature and time to reduce stress.

Benefits of technology

It effectively suppressed the generation of cracks in the external electrodes and improved the moisture resistance reliability of the multilayer ceramic capacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013747A_ABST
    Figure CN119013747A_ABST
Patent Text Reader

Abstract

Provided is a multilayer ceramic capacitor capable of suppressing the occurrence of cracks in an external electrode and improving moisture resistance reliability. An external electrode of a multilayer ceramic capacitor (1) is provided with: metal layers (41a, 41b) disposed on a first end surface (E1) and a second end surface (E2) so as to cover an internal electrode led out to the first end surface (E1) and an internal electrode led out to the second end surface (E2); glass films (42a, 42b) which are disposed on the first end surface (E1) and the second end surface (E2) and are disposed around the metal layers (41a, 41b) so as to be adjacent to the metal layers (41a, 41b); a sintered layer (43a, 43b) that contains glass and a metal and is disposed so as to cover the metal layer (41a, 41b); and plating films (44a, 44b) disposed so as to cover the sintered layers (43a, 43b), the sintered layers (43a, 43b) having voids, and a plating material being present in at least a portion of the voids.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a laminated ceramic capacitor. Background Art

[0002] A multilayer ceramic capacitor is known that includes a laminated body in which dielectric layers and internal electrodes are alternately laminated, and an external electrode that is electrically connected to the internal electrode and is provided on a surface of the laminated body.

[0003] Patent Document 1 describes a method for forming external electrodes in a multilayer ceramic capacitor.

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-266208 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] A multilayer ceramic capacitor having external electrodes has a problem of insufficient moisture resistance reliability. One of the causes of insufficient moisture resistance reliability is cracks in the external electrodes.

[0009] An object of the present invention is to provide a multilayer ceramic capacitor that can suppress the occurrence of cracks in external electrodes and has improved moisture-resistant reliability.

[0010] Technical solutions to solve problems

[0011] The multilayer ceramic capacitor of the present invention comprises:

[0012] A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and

[0013] a pair of external electrodes provided on the surface of the stack and electrically connected to the internal electrodes led out to the surface of the stack;

[0014] The laminated body has:

[0015] The first main surface and the second main surface are opposed to each other in a thickness direction which is a lamination direction of the dielectric layer and the internal electrode;

[0016] The first end surface and the second end surface are opposed to each other in a longitudinal direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and

[0017] The first side surface and the second side surface are opposed to each other in a width direction perpendicular to the thickness direction and the length direction.

[0018] The external electrode comprises:

[0019] a metal layer disposed on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface;

[0020] A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer;

[0021] a sintered layer comprising glass and metal and configured to cover the metal layer; and

[0022] a coating film configured to cover the sintered layer,

[0023] The sintered layer has voids,

[0024] A plating material exists in at least a portion of the void.

[0025] Effects of the Invention

[0026] According to the present invention, it is possible to provide a multilayer ceramic capacitor which can suppress the occurrence of cracks in external electrodes and has improved moisture-resistant reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a perspective view of a multilayer ceramic capacitor of the present invention.

[0028] Figure 2 yes Figure 1 Line II cross-sectional view.

[0029] Figure 3 yes Figure 1 Cross-sectional view along line III-III.

[0030] Figure 4 yes Figure 1 Sectional view along line II-II.

[0031] Figure 5 yes Figure 1 Sectional view along line IV-IV. DETAILED DESCRIPTION

[0032] Hereinafter, an example of an embodiment of the present invention will be described with reference to the accompanying drawings. In addition, in each figure, the same reference numerals are attached to the same or corresponding parts.

[0033] <Outline of Multilayer Ceramic Capacitors>

[0034] based on Figure 1 The outline of the appearance of the multilayer ceramic capacitor 1 will be described. Figure 1 1 is a perspective view showing a multilayer ceramic capacitor 1 according to the present embodiment.

[0035] like Figure 1 As shown, the multilayer ceramic capacitor 1 includes a multilayer body 2 and external electrodes 4 (4a, 4b). The external electrodes 4 include a first external electrode 4a and a second external electrode 4b.

[0036] <Definition of direction>

[0037] exist Figures 1 to 5 , the L direction, the W direction, and the T direction are shown. The L direction is the length direction L of the multilayer ceramic capacitor 1. The W direction is the width direction W of the multilayer ceramic capacitor 1. The T direction is the stacking direction of the multilayer ceramic capacitor 1, that is, the thickness direction T.

[0038] thus, Figure 2 as well as Figure 4 The section shown is called the LT section. Figure 3 as well as Figure 5 The section shown is called the WT section.

[0039] The length direction L, the width direction W, and the thickness direction T do not necessarily need to be orthogonal to each other. The length direction L, the width direction W, and the thickness direction T may be intersecting to each other.

[0040] <Outer Shape of Laminated Body>

[0041] like Figure 1 As shown, the shape of the stacked body 2 is a substantially rectangular parallelepiped shape.

[0042] The laminate has two end surfaces, two main surfaces, and two side surfaces.

[0043] The end faces are faces facing each other in the longitudinal direction L. The main faces are faces facing each other in the thickness direction T. The side faces are faces facing each other in the width direction W.

[0044] The two end faces are referred to as the first end face E1 and the second end face E2. The two principal faces are referred to as the first principal face M1 and the second principal face M2. The two side faces are referred to as the first side face S1 and the second side face S2.

[0045] The corners and ridges of the laminate 2 are preferably rounded. The corners are the portions where three surfaces of the laminate 2 intersect. The ridges are the portions where two surfaces of the laminate 2 intersect.

[0046] <Size of laminated body>

[0047] The size of the laminated body 2 can be set, for example, as follows.

[0048] The length L of the laminate 2 can be 200 μm to 2000 μm. The length in the thickness direction of the laminate 2 can be 100 μm to 1000 μm. The length in the width direction W of the laminate 2 can be 100 μm to 1000 μm.

[0049] The length of each portion of the laminate 2 can be measured using a micrometer or an optical microscope.

[0050] <Internal structure of laminate>

[0051] based on Figure 2 as well as Figure 3 , the internal structure of the stacked body 2 is described.

[0052] Figure 2 yes Figure 1 FIG. 1 is a cross-sectional view of the multilayer ceramic capacitor taken along line II shown in FIG. Figure 3 yes Figure 1 FIG. 1 is a cross-sectional view of the multilayer ceramic capacitor taken along line III-III shown in FIG.

[0053] like Figure 2 As shown, the laminate 2 includes a plurality of dielectric layers 7 ( 7 a , 7 b ) and a plurality of internal electrodes 8 ( 8 a , 8 b ). The plurality of dielectric layers 7 and the plurality of internal electrodes 8 are stacked in the thickness direction T on one another.

[0054] <Dielectric Layer>

[0055] like Figure 2 As shown, the dielectric layer 7 includes an outer dielectric layer 7a and an inner dielectric layer 7b.

[0056] <Outer Dielectric Layer>

[0057] The outer dielectric layers 7a are the dielectric layers 7 located on the first and second principal surfaces M1 and M2 of the laminate 2. That is, the outer dielectric layers 7a are the dielectric layers 7 located on both outer sides in the thickness direction T of the laminate 2.

[0058] Specifically, the outer dielectric layer 7 a is the dielectric layer 7 located between the first main surface M1 and the internal electrode 8 closest to the first main surface M1 , and between the second main surface M2 and the internal electrode 8 closest to the second main surface M2 .

[0059] <Inner Dielectric Layer>

[0060] The inner dielectric layer 7 b is the dielectric layer 7 located between the internal electrodes 8 .

[0061] Specifically, the inner dielectric layer 7b is the dielectric layer 7 located between a first inner electrode 8a and a second inner electrode 8b described below.

[0062] <Internal Electrode>

[0063] like Figure 2 As shown, the internal electrode 8 includes a first internal electrode 8a and a second internal electrode 8b. The first internal electrode 8a is an internal electrode connected to the first external electrode 4a. The second internal electrode 8b is an internal electrode connected to the second external electrode 4b.

[0064] The first inner electrode 8a extends from the first end surface E1 toward the second end surface E2. The second inner electrode 8b extends from the second end surface E2 toward the first end surface E1.

[0065] <Opposing portion and lead portion>

[0066] The first internal electrode 8a and the second internal electrode 8b each have an opposing portion and a lead portion.

[0067] The opposing portion is a portion where the first internal electrode 8a and the second internal electrode 8b oppose each other.

[0068] The lead portion is a portion led out from the opposing portion to the end faces E1 and E2 of the laminate 2. Specifically, the lead portion of the first internal electrode 8a is a portion led out from the opposing portion to the first end face E1 of the laminate 2. The lead portion of the second internal electrode 8b is a portion led out from the opposing portion to the second end face E2 of the laminate 2.

[0069] The facing portion of the first internal electrode 8a and the facing portion of the second internal electrode 8b face each other via the inner dielectric layer 7b, thereby forming capacitance at the facing portions. Thus, the multilayer ceramic capacitor 1 functions as a capacitor.

[0070] <Lengthwise Gap>

[0071] like Figure 2 As shown, the region from the front end of the first inner electrode 8a on the second end face E2 side to the second end face E2 is defined as the longitudinal gap LG. Similarly, the region from the front end of the second inner electrode 8b on the first end face E1 side to the first end face E1 is defined as the longitudinal gap LG.

[0072] The length of the longitudinal direction L of the longitudinal gap LG can be set to, for example, 5 μm or more and 30 μm or less.

[0073] <Gap in Width Direction>

[0074] like Figure 3 As shown, the region from the end of the internal electrode 8 in the width direction W to the first side surface S1 is defined as the width direction gap WG. Similarly, the region from the end of the internal electrode 8 in the width direction W to the second side surface S2 is defined as the width direction gap WG.

[0075] The length of the width direction W of the width direction gap WG can be set to, for example, 5 μm or more and 30 μm or less.

[0076] <Number of Dielectric Layers>

[0077] The number of dielectric layers 7 stacked in the stacked body 2 can be, for example, 10 or more and 1000 or less. The number of dielectric layers 7 includes the number of outer dielectric layers 7a and the number of inner dielectric layers 7b.

[0078] <Thickness of Dielectric Layer>

[0079] The thickness of the outer dielectric layer 7 a among the dielectric layers 7 can be set to, for example, 10 μm or more and 100 μm or less. The thickness of the inner dielectric layer 7 b can be set to, for example, 0.3 μm or more and 5.0 μm or less.

[0080] <Material for Dielectric Layer>

[0081] The material of the dielectric layer 7 can be, for example, a dielectric ceramic including BaTiO 3 , CaTiO 3 , SrTiO 3 , or CaZrO 3 .

[0082] The material of the dielectric layer 7 may be a material obtained by adding a Mn compound, a Fe compound, a Cr compound, a Co compound, a Ni compound, or the like to the above-mentioned dielectric ceramic.

[0083] <Number of Internal Electrodes>

[0084] The number of the internal electrodes 8 can be set, for example, to not less than 10 and not more than 1000. The number of the internal electrodes 8 includes the number of the first internal electrodes 8a and the number of the second internal electrodes 8b.

[0085] <Thickness of Internal Electrode>

[0086] The thickness of the internal electrode 8 can be set to, for example, 0.3 μm or more and 5.0 μm or less. When the thickness of the internal electrode 8 is 0.5 μm or more, a plated film easily grows when a metal layer is formed by plating. The metal layer will be described later.

[0087] <Material of Internal Electrode>

[0088] The material of the internal electrode 8 can be, for example, metals such as Ni, Cu, Ag, Pd, and Au, alloys of Ni and Cu, alloys of Ag and Pd, etc. In addition, the material of the internal electrode 8 may include dielectric particles of the same composition as the ceramic included in the dielectric layer 7 .

[0089] <External Electrode>

[0090] As based on Figure 1 As described above, the external electrodes include the first external electrode 4 a and the second external electrode 4 b .

[0091] <First External Electrode>

[0092] like Figure 1 As shown, the first external electrode 4 a is an external electrode disposed on the first end surface E1 of the stacked body 2 .

[0093] The first external electrode 4 a extends from the first end surface E1 to a part of both main surfaces and a part of both side surfaces.

[0094] The portion of the first external electrode 4a disposed on the first end surface E1 of the stacked body 2 is referred to as the end surface external electrode 4Ea. The portion of the first external electrode 4a disposed on a portion of the first principal surface M1 or a portion of the second principal surface M2 is referred to as the principal surface external electrode 4Ma. The portion of the first external electrode 4a disposed on a portion of the first side surface S1 or a portion of the second side surface S2 is referred to as the side surface external electrode 4Sa.

[0095] like Figure 2 As shown, the first external electrode 4a and the first internal electrode 8a are electrically connected.

[0096] <Second External Electrode>

[0097] The second external electrode 4 b is an external electrode disposed on the second end surface E2 of the stacked body 2 .

[0098] The second external electrode 4b has the same structure as the first external electrode 4a.

[0099] That is, the second outer electrode 4 b extends from the second end surface E2 to a part of both main surfaces and a part of both side surfaces.

[0100] The portion of the second external electrode 4b disposed on the second end surface E2 of the stack 2 is referred to as the end surface external electrode 4Eb. The portion of the second external electrode 4b disposed on a portion of the first principal surface M1 or a portion of the second principal surface M2 is referred to as the principal surface external electrode 4Mb. The portion of the second external electrode 4b disposed on a portion of the first side surface S1 or a portion of the second side surface S2 is referred to as the side surface external electrode 4Sb.

[0101] like Figure 2 As shown, the second outer electrode 4b is electrically connected to the second inner electrode 8b.

[0102] <Layer Structure of External Electrode>

[0103] based on Figure 2 The layer structure of the external electrode 4 will be described.

[0104] like Figure 2 As shown, the first external electrode 4a includes a metal layer 41a, a glass film 42a, a sintered layer 43a, and a plated film 44a. The second external electrode 4b includes a metal layer 41b, a glass film 42b, a sintered layer 43b, and a plated film 44b.

[0105] Each layer of the external electrode 4 will be described by taking the first external electrode 4 a as an example.

[0106] In addition, each layer of the second external electrode 4b has the same structure as each layer of the first external electrode 4. Therefore, the description about the first external electrode 4a is also appropriate for the second external electrode 4b.

[0107] <Metal Layer>

[0108] The end portion of the first internal electrode 8a is exposed from the end surface E1. The metal layer 41a is a metal layer provided on the first end surface E1 so as to cover the exposed end portion of the first internal electrode 8a.

[0109] The metal layer 41a is formed of, for example, a material containing at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The metal layer 41a may be formed of, for example, an alloy such as an alloy of Cu and Ni or an alloy of Ag and Pd.

[0110] A part of the material forming the metal layer 41a may diffuse into the first internal electrode 8a which is in contact with the metal layer 41a. The material forming the metal layer 41a and the material forming the first internal electrode 8a are mixed together, thereby improving the bonding strength between the metal layer 41a and the first internal electrode 8a.

[0111] The metal layer 41 a can be formed by, for example, plating.

[0112] <Thickness of Metal Layer>

[0113] Figure 2 The thickness of the metal layer 41a is indicated by d1.

[0114] The thickness d1 of the metal layer 41 a can be set to, for example, 0.1 μm or more and 15.0 μm or less.

[0115] When the thickness d1 of the metal layer 41a is less than 0.1 μm, the continuity of the metal layer 41a tends to decrease. Therefore, the bonding strength between the metal layer 41a and the first internal electrode 8a may decrease. In addition, the conductivity of the metal layer 41a may decrease.

[0116] When the thickness d1 of the metal layer 41a exceeds 15.0 μm, the internal stress in the metal layer 41a tends to increase, so that the metal layer 41a may be separated from the first internal electrode 8a.

[0117] <Burn layer>

[0118] The sintered layer 43a is a layer arranged to cover at least a portion of the metal layer 41a. The sintered layer 43a includes glass and metal.

[0119] The sintered layer 43a is formed of a material including at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The sintered layer 43a may be a single layer or may include a plurality of layers.

[0120] The sintered layer 43a can be formed, for example, as follows. That is, first, a conductive paste is applied on the metal layer 41a. The conductive paste contains glass and metal. Next, the applied conductive paste is fired. In this way, the sintered layer 43a can be formed.

[0121] This firing or sintering can be performed simultaneously with the firing of the laminate 2. Alternatively, the sintering layer 43a can be fired after the laminate 2 is fired.

[0122] The sintered layer 43a will be described in more detail later.

[0123] <Glass Film>

[0124] The glass film 42a is a film mainly made of glass and is disposed around the metal layer 41a.

[0125] like Figure 2 As shown, the glass film 42a is disposed around the metal layer 41a so as to be adjacent to the metal layer 41a and surround the metal layer 41a. Specifically, the glass film 42a is in contact with the end 5 of the metal layer 41a.

[0126] The glass film 42a extends from a portion of the first end face E1 to a portion of the first main face M1 of the laminate 2. Similarly, the glass film 42a extends from a portion of the first end face E1 to a portion of the second main face M2 of the laminate 2.

[0127] In addition, although Figure 2 Although not shown, the glass film 42 a extends from a portion of the first end surface E1 of the stacked body 2 to a portion of the first side surface S1 and a portion of the second side surface S2 .

[0128] The glass film 42a is formed together with the sintered layer 43 in the process of forming the sintered layer 43a. In the process of forming the sintered layer 43a, a conductive paste is applied to the first end surface E1. The conductive paste contains glass.

[0129] The glass moves to the exposed portion of the dielectric layer 7 during the sintering process. The exposed portion of the dielectric layer 7 is a portion where the metal layer 41a is not arranged in the laminate 2. The glass moves to a portion of the first end face E1, a portion of the first main face M1, a portion of the second main face M2, a portion of the first side face S1, and a portion of the second side face S2. In this way, the glass moved to the exposed portion of the dielectric layer 7 forms a glass film 42a after the sintering is completed.

[0130] As described above, the glass contained in the conductive paste moves to the exposed portion of the dielectric layer 7 during sintering. Therefore, the glass content of the glass film 42a becomes higher than the glass content of the sintered layer 43a.

[0131] In particular, it is preferred that the surface of the sintered layer 43a has a low glass content.

[0132] This is because the adhesion of the plating film 44a described later to the surface of the sintered layer 43a is improved. In addition, this is because the adhesion between the surface of the sintered layer 43a and the plating film 44a is improved.

[0133] Here, in the sintered layer 43a, a portion containing metal is referred to as a metal portion. Also, in the sintered layer 43a, a portion containing glass is referred to as a glass portion.

[0134] On the surface of the sintered layer 43a on the plating film 44a side, the area of ​​the metal portion is preferably larger than 10 times the area of ​​the glass portion.

[0135] Thereby, the adhesion of the plated film 44a to the sintered layer 43a can be sufficiently improved. In addition, the adhesion between the sintered layer 43a and the plated film 44a can be sufficiently improved.

[0136] The glass film 42a is not necessarily formed only of glass. The glass film 42a may contain other materials such as metal materials in addition to glass. However, the ratio of glass contained in the glass film 42a is preferably high. This is because the higher the ratio of glass, the higher the effect of suppressing the intrusion of moisture into the interior of the laminate 2, etc., which will be described later.

[0137] As described above, the glass film 42a is arranged to be in contact with the end 5 of the metal layer 41a and adjacent to the metal layer 41a so as to surround the periphery of the metal layer 41a. In other words, the end 5 of the metal layer 41a is buried and sealed by the glass film 42a.

[0138] This can suppress the intrusion of moisture from the periphery of the metal layer 41 a into the interface between the dielectric layer 7 and the internal electrode 8 .

[0139] From the viewpoint of suppressing moisture intrusion, it is preferred that the glass film 42a is in continuous contact with the end portion 5 around the entire periphery of the metal layer 41a, thereby covering the entire periphery of the metal layer 41a.

[0140] Whether the glass film 42 a is formed on the surface of the laminate 2 can be determined by appropriately polishing the laminate 2 and performing elemental analysis on the portion using a field emission wavelength dispersive X-ray spectrometer.

[0141] <Plating film>

[0142] The plated film 44a is a film containing metal formed by plating and is arranged to cover the sintered layer 43a.

[0143] The plated film 44a is formed of a material containing at least one metal selected from Cu, Ni, Ag, Pd, Au, etc. The plated film 44a may be formed of an alloy such as an alloy of Ag and Pd. In addition, the plated film 44a does not contain glass.

[0144] The plating film 44a includes a lower plating film and an upper plating film. The upper plating film is a plating film formed on the lower plating film.

[0145] The lower plating film is formed of a material containing at least one metal selected from the group consisting of Cu, Ni, Ag, Pd, an alloy of Ag and Pd, and Au, for example.

[0146] The upper plating film is formed using Sn as a material, for example.

[0147] By using Sn as the material of the upper plating film, the wettability of the solder to the first external electrode 4 a can be improved.

[0148] The thickness of the upper plating film can be set to, for example, 1 μm or more and 10 μm or less. In addition, the thickness of the plating films 44 a and 44 b can also be set to, for example, 1 μm or more and 10 μm or less.

[0149] The above description of the first external electrode 4a is also applicable to the second external electrode 4b because the first external electrode 4a and the second external electrode 4b are the same except that the first external electrode 4a and the second external electrode 4b are provided on different surfaces.

[0150] Therefore, the metal layer 41b, the glass film 42b, the sintered layer 43b, and the plated film 44b in the second external electrode 4b are the same as the components described in relation to the first external electrode 4a.

[0151] <Size of Multilayer Ceramic Capacitors>

[0152] The length L of the entire multilayer ceramic capacitor 1 including the laminate 2 and the external electrodes 4 can be set to, for example, 0.2 mm or more and 2.0 mm or less. The length T of the entire multilayer ceramic capacitor 1 in the thickness direction can be set to, for example, 0.1 mm or more and 1.2 mm or less. The length W of the entire multilayer ceramic capacitor 1 in the width direction can be set to, for example, 0.1 mm or more and 1.2 mm or less.

[0153] <Details of External Electrodes>

[0154] based on Figure 2 , the external electrode 4 is described in detail.

[0155] As mentioned earlier, Figure 2 yes Figure 1 Here, the II-line cross-sectional view is a LT cross-sectional view at the center position in the width direction W of the multilayer ceramic capacitor 1 .

[0156] exist Figure 3 The center position in the width direction W is shown in FIG. Figure 3 The position of the line I is the center position of the multilayer ceramic capacitor 1 in the width direction W. Figure 3 yes Figure 1 III-III section view. Figure 3 WT is a diagram showing a cross section of the multilayer ceramic capacitor 1 .

[0157] Will Figure 2 The LT cross section at the center position in the width direction W of the multilayer ceramic capacitor 1 shown is set to be a 1 / 2 LT cross section.

[0158] Hereinafter, the external electrode 4 will be described by taking the first external electrode 4a as an example. In addition, the second external electrode 4b has the same structure as the first external electrode 4a. Therefore, the following description is also appropriate for the second external electrode 4b.

[0159] <Metal layer and glass film>

[0160] At the first end face E1, Figure 2 As shown, the metal layer 41a is arranged on substantially the entire area of ​​the first end surface E1. However, a glass film 42a is arranged in the vicinity of the first main surface M1 and the vicinity of the second main surface M2 in the first end surface E1 instead of the metal layer 41a. The glass film 42a is in contact with the end 5 of the metal layer 41a.

[0161] In addition, although Figure 2 Although not shown, the glass film 42a is also disposed in the first end surface E1, in the vicinity of the first side surface S1 and in the vicinity of the second side surface S2. The glass film 42a is also in contact with the end portion 5 of the metal layer 41a.

[0162] As described above, the glass film 42a is arranged to cover the periphery of the metal layer 41a.

[0163] More specifically, the glass film 42a on the first end face E1 extends from the end 5 of the metal layer 41a to a part of the first main face M1 and a part of the second main face M2.

[0164] In addition, although not shown in Figure 2 , the glass film 42a extends from the end 5 of the metal layer 41a to a part of the first side face S1 and a part of the second side face S2.

[0165] That is, the glass film 42a is arranged to cover the ridge line part of the laminate 2 between the first end face, the two main faces and the two side faces.

[0166] <Sintered layer>

[0167] The sintered layer 43a is arranged in the entire area of the first end face E1 at the central position in the 1 / 2LT cross-section, that is, in the central position in the width direction W. In addition, the sintered layer 43a extends from the first end face E1 to a part of the first main face M1 and a part of the second main face M2. Moreover, although not shown in Figure 2 , the sintered layer 43a extends from the first end face E1 to a part of the first side face S1 and a part of the second side face S2.

[0168] In addition, the sintered layer 43a is arranged to cover the entire metal layer 41a and the glass film 42a. Therefore, at the central position in the width direction W of the multilayer ceramic capacitor 1, neither the metal layer 41a nor the glass film 42a is exposed from the sintered layer 43a.

[0169] <Plated film>

[0170] The plated film 44a is arranged to cover the entire sintered layer 43a. That is, the plated film 44a is arranged on the first end face E1 and a part of the two main faces beyond the range where the sintered layer 43a is arranged. In addition, although not shown in Figure 2 , the plated film 44a is also arranged on a part of the two side faces in the same way as the two main faces.

[0171] <WT cross-section>

[0172] The arrangement of the first external electrode 4a will be described based on the WT cross-sectional view of the multilayer ceramic capacitor 1.

[0173] As described above, Figure 3 is Figure 1 the III-III line cross-sectional view. Figure 3 is a view showing the WT cross-section at the line L1 of Figure 2 .

[0174] As Figure 3 As shown, on the outside of the stacked body 2 , the glass film 42 a is arranged so as to surround the entire periphery of the stacked body 2 .

[0175] Furthermore, on the outer side of the glass film 42a, the sintered layer 43a is arranged so as to surround the entire periphery of the glass film 42a.

[0176] Furthermore, on the outer side of the sintered layer 43a, the plating film 44a is arranged so as to surround the entire periphery of the sintered layer 43a.

[0177] <Voids in the Burnt Layer>

[0178] based on Figure 2 The voids 6 of the sintered layer 43a will be described. Figure 2 1 is a diagram showing a 1 / 2LT cross section of the multilayer ceramic capacitor 1 .

[0179] In the multilayer ceramic capacitor 1 of the present embodiment, the voids 6 are formed in the sintered layer 43 a .

[0180] The gap 6 is a portion of the sintered layer 43a that is not filled with glass or metal. The glass and metal here refer to the glass and metal contained in the conductive paste used to form the sintered layer 43a.

[0181] <Position of the gap>

[0182] like Figure 2 As shown, the void 6 is formed throughout the sintered layer 43a in the thickness direction.

[0183] However, the void 6 is preferably formed at least in a portion close to the metal layer 41 a.

[0184] Specifically, it is preferable that at least one of the voids 6 is formed in a range closer to the metal layer 41 a than ½ of the thickness d2 of the sintered layer 43 a from the surface of the sintered layer 43 a .

[0185] in addition, Figure 2 The distance d2 shown shows the thickness d2 of the sintered layer 43a. Figure 2 The distance d3 shown shows the thickness from the surface of the metal layer 41a to 1 / 2 of the thickness d2 of the sintered layer 43a.

[0186] Preferably, at least one of the gaps 6 is located within a range of a distance d3 from the surface of the metal layer 41 a .

[0187] The thickness d2 of the sintered layer 43 a can be set to, for example, 1.0 μm or more and 100.0 μm or less. This thickness is the thickness of the thickest portion of the sintered layer 43 a.

[0188] <Filling of plating material>

[0189] The plating film 44a is formed outside the sintered layer 43a. Therefore, the plating material exists in at least a part of the gap 6. This is because the plating material enters the gap 6 when the plating film 44a is formed.

[0190] <Ratio of voids>

[0191] The ratio of the voids 6 in the sintered layer 43a is not particularly limited, but is preferably within the following range.

[0192] As described above, the plating material exists in at least a part of the voids 6. Therefore, the ratio of the voids 6 in the sintered layer 43a is defined by the area ratio of the plating material in the WT cross section.

[0193] Specifically, in the sintered layer 43a of the first end surface E1, a surface parallel to the first end surface E1 at a position ¾ of the thickness d2 of the sintered layer 43a from the surface of the sintered layer 43a is observed.

[0194] That is, a WT cross section at a position 1 / 2 of d3 from the surface of the metal layer 41 a is observed.

[0195] Furthermore, in the WT cross section, the ratio of the area of ​​the plating material to the entire area of ​​the sintered layer 43 a is preferably greater than or equal to 20% and less than or equal to 90%.

[0196] <1 / 2LT section and side LT section>

[0197] based on Figure 4 as well as Figure 5 The external electrode 4 in the vicinity of the width direction gap WG will be described.

[0198] Figure 4 yes Figure 1 Sectional view along line II-II. Figure 5 yes Figure 1 Sectional view along line IV-IV.

[0199] In the multilayer ceramic capacitor 1 of the present embodiment, the external electrodes 4 are arranged differently at the center position in the width direction W and at the position close to the side surface in the width direction W. In other words, the shape of the external electrodes 4 is different. Figure 3 LT section at line I and Figure 3 The LT profile at line II is different.

[0200] The aforementioned based on Figure 2 The description of the LT cross section is about the central position in the width direction W. Figure 4 The position close to the side surface in the width direction W will be described.

[0201] Figure 41 is a diagram showing a cross section taken along line LT at the end surface of the internal electrode 8 on the first side surface S1 side. Figure 4 It is shown Figure 3 Figure 1 is a diagram of the LT cross section at line II.

[0202] Hereinafter, the position of the end surface of the internal electrode 8 on the first side surface S1 side is referred to as a side end position.

[0203] As mentioned above, Figure 2 The LT cross section at the center of the width direction W shown is set to a 1 / 2LT cross section. Figure 4 The LT cross section at the side end position shown is set as the side end LT cross section.

[0204] like Figure 4 As shown, in Figure 4 In the side LT section, Figure 2 Compared with the 1 / 2LT cross section, the thickness of the sintered layer 43a on the first end surface E1 is thinner.

[0205] Figure 4 The distance d2 and the distance d3 shown are Figure 2 The distance d2 and the distance d3 shown are the same.

[0206] like Figure 2 As shown in FIG. 1 , the thickness of the sintered layer 43a is d2 at the center position in the width direction W. Figure 4 As shown, at the side end position, the thickness of the sintered layer 43a is thinner than d3 which is half of d2.

[0207] Thus, the sintered layer 43a is not formed with a uniform thickness on the surface of the metal layer 41a.

[0208] The thickness of the sintered layer 43a is thicker near the center of the metal layer 41a than near the end of the metal layer 41a. In other words, the thickness of the sintered layer 43a decreases from near the center of the metal layer 41a toward the end of the metal layer 41a.

[0209] <Ridge Line>

[0210] The thickness of the sintered layer 43a decreases from the vicinity of the center of the metal layer 41a toward the ridgeline of the laminate 2. Furthermore, the thickness of the sintered layer 43a also decreases from the vicinity of the center of the metal layer 41a toward the corner of the laminate 2.

[0211] First, the reduction toward the ridge portion will be described.

[0212] The thickness of the sintered layer 43a decreases toward the four ridges of the first end face E1. The four ridges are ridges formed by the first end face E1 and the first principal surface M1, the first end face E1 and the second principal surface M2, the first end face E1 and the first side surface S1, and the first end face E1 and the second side surface S2. In addition, as mentioned above, the ridge is a portion where two faces of the stacked body 2 intersect.

[0213] And, the film thickness of the sintered layer 43a also decreases from the vicinity of the center of the first end face E1 toward the four corners of the first end face E1. The so-called four corners are the corners formed by the first end face E1, the first principal surface M1 and the first side surface S1, the first end face E1, the first principal surface M1 and the second side surface S2, the first end face E1, the second principal surface M2 and the first side surface S1, and the first end face E1, the second principal surface M2 and the second side surface S2. In addition, as mentioned above, the so-called corner is the part where the three faces of the stacked body 2 intersect.

[0214] <Exposure of Metal Layer>

[0215] In this way, since the film thickness of the sintered layer 43a decreases toward the four corners, the end portions 5 of the metal layer 41a are exposed from the sintered layer 43a at the side end positions.

[0216] Figure 4 FIG. 4 shows a state where the end portion 5 of the metal layer 41a is not covered by the sintered layer 43a at two locations in the thickness direction T. Figure 4 The remaining two corners not shown are also not covered by the sintered layer 43a.

[0217] Hereinafter, the multilayer ceramic capacitor 1 will be described based on the WT cross section.

[0218] Figure 5 yes Figure 1 Sectional view along line IV-IV. Figure 5 Show Figure 4 WT section at line L2.

[0219] like Figure 5 As shown in FIG. 1 , the sintered layer 43a is disposed around the metal layer 41a. However, the sintered layer 43a is not disposed near the four corners of the metal layer 41a.

[0220] Thus, the four end portions 5 of the metal layer 41 a are exposed from the sintered layer 43 a near the four corners where the end surface, the main surface, and the side surface intersect.

[0221] <Effect>

[0222] The multilayer ceramic capacitor 1 of the present embodiment can suppress the occurrence of cracks in the external electrodes 4. Furthermore, the multilayer ceramic capacitor 1 of the present embodiment is a multilayer ceramic capacitor 1 having improved moisture resistance reliability.

[0223] <Conventional Multilayer Ceramic Capacitors>

[0224] In the past, in a laminated ceramic capacitor having a metal layer disposed on the external electrode, cracks sometimes occurred in the metal layer. As a cause of cracks in the metal layer, stress applied from other components can be cited. As the other component, there is a sintered layer. The sintered layer is a layer disposed in contact with the metal layer.

[0225] Due to changes in ambient temperature or humidity, stress may be generated in the sintered layer. This stress is applied to the metal layer, causing cracks in the metal layer.

[0226] When cracks are generated in the metal layer, the function of the metal layer to suppress water intrusion is destroyed.

[0227] In addition, the suppression of moisture intrusion is not easily replaced by other layers such as the sintered layer because the film density of other layers is inferior to that of the metal layer.

[0228] Therefore, it is desired to suppress the occurrence of cracks.

[0229] <Voids in the Burnt Layer>

[0230] In the multilayer ceramic capacitor 1 of the present embodiment, the sintered layer 43a has the voids 6. Since the sintered layer 43a has the voids 6, the stress of the sintered layer 43a can be reduced. As a result, the occurrence of cracks in the metal layer 41a can be suppressed.

[0231] In particular, when at least one of the voids 6 is located closer to the metal layer 41a than 1 / 2 of the thickness d2 of the sintered layer 43a from the surface of the sintered layer 43a, the occurrence of cracks in the metal layer 41a can be further suppressed.

[0232] This is because the gap 6 is located near the metal layer 41a, so that the stress applied to the metal layer 41a from the sintered layer 43a can be easily relieved.

[0233] Furthermore, when the void 6 is located near the metal layer 41 a , the stress of the sintered layer 43 a can be further reduced.

[0234] As described later, the sintered layer 43a is formed by firing the conductive paste. In the over-fired sintered layer 43a, it is easy to generate a large stress. In addition, during the sintering process, along with the sintering, the void 6 is easy to disappear from the part near the metal layer 41a in the sintered layer 43a.

[0235] Here, in the multilayer ceramic capacitor 1 of the present embodiment, the void 6 exists in the portion of the sintered layer 43a close to the metal layer 41a. That is, the sintered layer 43a is not over-sintered. Therefore, it is difficult for a large stress to be generated in the sintered layer 43a. As a result, it is possible to further suppress the generation of cracks in the metal layer 41a.

[0236] <Exposure of Metal Layer>

[0237] In the multilayer ceramic capacitor 1 of the present embodiment, at least a portion of the metal layer 41 a is exposed from the sintered layer 43 a .

[0238] Specifically, when the metal layer 41a is viewed from the longitudinal direction L, the sintered layer 43a is not disposed near the four corners thereof. As a result, the vicinities of the four corners of the metal layer 41a are exposed from the sintered layer 43a.

[0239] In the multilayer ceramic capacitor 1 of the present embodiment, at least a portion of the metal layer 41 a is exposed from the sintered layer 43 a , so that the occurrence of cracks in the metal layer 41 a can be further suppressed.

[0240] Since the metal layer 41a is exposed from the sintered layer 43a, the stress received by the exposed portion of the metal layer 41a from the sintered layer 43a is weakened. Therefore, it is possible to suppress the occurrence of cracks in the metal layer 41a.

[0241] In addition, the exposed portion of the metal layer 41a is the portion where the sintered layer 43a is interrupted. Since there is an interrupted portion in the sintered layer 43a, the bonding in the surface direction of the sintered layer 43a becomes weaker. As a result, the stress of the sintered layer 43a is reduced. As a result, it is possible to suppress the generation of cracks in the metal layer 41a.

[0242] <Method for Manufacturing Multilayer Ceramic Capacitor>

[0243] An overview of a general method for manufacturing the multilayer ceramic capacitor 1 will be described.

[0244] (1) Ceramic green sheets for dielectric layer 7 and conductive paste for internal electrode 8 are prepared.

[0245] (2) Forming an internal electrode pattern on a ceramic green sheet. The pattern can be formed by printing a conductive paste in a predetermined pattern on the ceramic green sheet. This printing can be performed by, for example, screen printing, gravure printing, or the like.

[0246] (3) Stacking a plurality of ceramic green sheets for outer dielectric layers on which no internal electrode pattern is formed. Stacking ceramic green sheets on which internal electrode patterns are printed in sequence. Stacking a plurality of ceramic green sheets for outer dielectric layers on top. In this way, a laminated sheet is produced.

[0247] (4) The laminated sheets are pressed in the thickness direction by isostatic pressing or the like. Thus, a laminated block is produced.

[0248] (5) Cut the laminated block into a given size. Thus, laminated chips are cut out.

[0249] (6) The corners and edges of the stacked small pieces are rounded by barrel grinding or the like.

[0250] (7) The stacked small pieces are fired to obtain a fired stacked body.

[0251] (8) A metal layer is formed on the end surface of the fired laminate. Specifically, the metal layer is formed on the end surface so as to cover the internal electrode led out to the end surface of the laminate. The metal layer can be formed by plating, for example.

[0252] Plating can be performed by electrolytic plating or electroless plating. As a plating process, for example, barrel plating can be used.

[0253] (9) A conductive paste for a sintered layer is applied onto the metal layer.

[0254] (10) The conductive paste is dried and then sintered.

[0255] Thus, sintered layers 43a and 43b are formed. In addition, glass contained in the conductive paste for sintered layers 43a and 43b moves to the surface of dielectric layer 7. The moved glass moves to the surface of dielectric layer 7. The moved glass becomes glass films 42a and 42b.

[0256] (11) Forming a plated film on the sintered layers 43a and 43b. Specifically, first, Ni plating is performed so as to cover the sintered layers 43a and 43b. Thus, a lower plated film is formed. Sn plating is performed thereon. Thus, an upper plated film is formed.

[0257] <Characteristics of the manufacturing method>

[0258] The multilayer ceramic capacitor 1 of the present embodiment has the following features in the manufacturing method in addition to the above-described general multilayer ceramic capacitor manufacturing method.

[0259] The sintered layer 43 a of the multilayer ceramic capacitor 1 of the present embodiment has voids 6 .

[0260] In order to form the voids 6, the sintering temperature and sintering time are optimized. Specifically, the sintering is performed at a temperature of 600°C or more and 750°C or less for a period of 5 minutes or more and 15 minutes or less. The temperature is more preferably 650°C or more and 700°C or less. In addition, the time is more preferably less than 15 minutes. In addition, the sintering can be performed in an inert gas atmosphere such as nitrogen.

[0261] The sintering temperature is lower than the general sintering temperature. In addition, the sintering time is shorter than the general sintering time. That is, the sintering is slower than the general sintering.

[0262] By performing firing under such conditions, the voids 6 can be formed in the fired layer 43 a .

[0263] However, the glass film 42a is not formed in the above-mentioned firing.

[0264] As described above, the glass film 42 a is formed by the glass contained in the conductive paste for forming the sintered layer 43 a moving to the exposed portion of the dielectric layer 7 .

[0265] In the above-mentioned firing, since the glass does not move sufficiently, the glass film 42 a is not formed.

[0266] Therefore, in addition to the above-mentioned firing, firing in an air atmosphere is performed.

[0267] This sintering can be performed at 700° C. for 5 minutes in an air atmosphere, for example.

[0268] The sintered layer 43 a can be formed by the sintering in the air atmosphere.

[0269] By firing in the air atmosphere, the metal particles such as Cu contained in the sintered layer 43a are oxidized. Moreover, the glass wets and spreads on the surface of the oxidized metal particles. Thus, the movement of the glass is promoted. Moreover, the glass further wets and spreads on the surface of the dielectric layer 7 formed of BaTiO3 or the like as an oxide, thereby forming a glass film 42a.

[0270] <Method for measuring length>

[0271] The length of each portion of the multilayer ceramic capacitor 1 can be measured by observing the cross section of the multilayer body exposed by grinding with a scanning electron microscope, for example. Each value can be an average value of measured values ​​at a plurality of locations corresponding to the locations to be measured.

[0272] <Moisture Resistance Reliability Test>

[0273] As a durability test, a moisture resistance reliability test was conducted. The samples, test conditions, etc. are as follows.

[0274] (Sample)

[0275] Length in the longitudinal direction L: 0.6 mm

[0276] Length in width direction W: 0.3mm

[0277] Length in thickness direction T: 0.3mm

[0278] Capacitance: 2.2μF

[0279] Thickness of inner dielectric layer 7b: 0.65 μm

[0280] Thickness of internal electrode 8: 0.43 μm

[0281] Number of internal electrodes 8: 280

[0282] Thickness of metal layers 41a, 141b: 5 μm

[0283] (Moisture resistance reliability test)

[0284] Temperature, humidity: 85℃, 85%RH

[0285] Voltage: 6.3V

[0286] Voltage application time: 120 hours

[0287] Judgment criteria: Based on the logarithmic value (log IR) of the insulation resistance (IR) immediately after the start of the moisture resistance reliability test, samples that are lower by two or more digits are judged to have IR deterioration.

[0288] A moisture resistance reliability test was performed using 72 samples according to the embodiment of the present invention and 72 conventional samples.

[0289] The sample of the embodiment is a sample in which the sintered layer 43a has the voids 6. On the other hand, the conventional sample is a sample in which the sintered layer 43a does not have the voids.

[0290] The results of the moisture resistance reliability test are as follows.

[0291] Among the samples of the embodiment, IR degradation was not observed in all 72 samples.

[0292] On the other hand, among the conventional samples, IR degradation was observed in 3 out of 72 samples.

[0293] In conventional samples, cracks may have occurred in the metal layer during the moisture resistance reliability test, resulting in IR degradation.

[0294] On the other hand, in the sample of the embodiment, it is considered that cracks did not occur in the metal layer in the moisture resistance reliability test, and as a result, IR degradation did not occur.

[0295] The above test results show that the multilayer ceramic capacitor of the present embodiment can suppress the occurrence of cracks in the external electrodes and has improved moisture-resistant reliability.

[0296] In addition, the description so far is mainly based on the first external electrode 4a. As mentioned above, the description of the first external electrode 4a is also appropriate for the second external electrode 4b. This is because the first external electrode 4a and the second external electrode 4b are the same only in that the surface on which they are provided is different.

[0297] Furthermore, although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various changes and modifications can be made.

[0298] <1> A multilayer ceramic capacitor, characterized by comprising:

[0299] A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and

[0300] a pair of external electrodes, provided on the surface of the stacked body and electrically connected to the internal electrodes led out to the surface of the stacked body;

[0301] The laminated body has:

[0302] The first main surface and the second main surface are opposed to each other in a thickness direction which is a lamination direction of the dielectric layer and the internal electrode;

[0303] The first end surface and the second end surface are opposed to each other in a longitudinal direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and

[0304] The first side surface and the second side surface are opposed to each other in a width direction perpendicular to the thickness direction and the length direction.

[0305] The external electrode comprises:

[0306] a metal layer disposed on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface;

[0307] A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer;

[0308] a sintered layer comprising glass and metal and configured to cover the metal layer; and

[0309] a coating film configured to cover the sintered layer,

[0310] The sintered layer has voids,

[0311] A plating material exists in at least a portion of the void.

[0312] <2> according to <1> The multilayer ceramic capacitor is characterized in that:

[0313] At least one of the voids is located in a range closer to the metal layer than 1 / 2 of the thickness of the sintered layer from the surface of the sintered layer.

[0314] <3> according to <1> or <2> The multilayer ceramic capacitor is characterized in that:

[0315] At least a portion of the metal layer is exposed from the sintered layer.

[0316] <4> according to <1> to <3> The multilayer ceramic capacitor according to any one of the preceding claims is characterized in that:

[0317] An area ratio of the plating material at a position of 3 / 4 of the thickness of the sintered layer from the surface of the sintered layer at the first end surface or the second end surface is 20% or more and 90% or less.

[0318] <5> according to <1> to <4> The multilayer ceramic capacitor according to any one of the preceding claims is characterized in that:

[0319] The thickness of the metal layer is greater than or equal to 0.1 μm and less than 15.0 μm.

[0320] <6> according to <1> to <5> The multilayer ceramic capacitor according to any one of the preceding claims is characterized in that:

[0321] The sintered layer has a thickness of 1.0 μm or more and 100.0 μm or less.

[0322] <7> according to <1> to <6> The multilayer ceramic capacitor according to any one of the preceding claims is characterized in that:

[0323] A glass film is disposed around the metal layer and in contact with an end portion of the metal layer.

[0324] Description of Reference Numerals

[0325] 1 Multilayer Ceramic Capacitors

[0326] 2 Laminated body

[0327] 4a 1st external electrode

[0328] 4b Second external electrode

[0329] 4Ma, 4Mb Main surface external electrode

[0330] 4Ea, 4Eb End surface external electrode

[0331] 4Sa, 4Sb Side external electrodes

[0332] 41a, 41b metal layer

[0333] 42a, 42b Glass film

[0334] 43a, 43b Sintered layer

[0335] 44a, 44b coating film

[0336] 5 End of the metal layer

[0337] 6. Voids in the burnt layer

[0338] 7a Outer dielectric layer

[0339] 7b Inner dielectric layer

[0340] 8a 1st internal electrode

[0341] 8b Second internal electrode

[0342] M1 1st main surface

[0343] M2 Second main surface

[0344] E1 1st end face

[0345] E2 2nd end face

[0346] S1 Side 1

[0347] S2 Side 2

[0348] L Length direction

[0349] T thickness direction

[0350] W Width direction.

Claims

1. A laminated ceramic capacitor, characterized in that: have: A laminated body in which a plurality of dielectric layers and internal electrodes are alternately laminated; and a pair of external electrodes, provided on the surface of the stacked body and electrically connected to the internal electrodes led out to the surface of the stacked body; The laminated body has: The first main surface and the second main surface are opposed to each other in a thickness direction which is a lamination direction of the dielectric layer and the internal electrode; The first end surface and the second end surface are opposed to each other in a length direction which is a direction in which the pair of external electrodes are opposed to each other, and the external electrodes are provided thereon; and The first side surface and the second side surface are opposed to each other in a width direction perpendicular to the thickness direction and the length direction. The external electrode comprises: a metal layer disposed on the first end surface and the second end surface so as to cover the internal electrode led out to the first end surface and the internal electrode led out to the second end surface; A glass film is disposed on the first end surface and the second end surface and is adjacent to the metal layer and disposed around the metal layer; a sintered layer comprising glass and metal and configured to cover the metal layer; as well as a coating film configured to cover the sintered layer, The sintered layer has voids, A plating material exists in at least a portion of the void.

2. The multilayer ceramic capacitor according to claim 1, wherein: At least one of the voids is located in a range closer to the metal layer than 1 / 2 of the thickness of the sintered layer from the surface of the sintered layer.

3. The multilayer ceramic capacitor according to claim 1 or 2, wherein: At least a portion of the metal layer is exposed from the sintered layer.

4. The multilayer ceramic capacitor according to claim 1 or 2, wherein: An area ratio of the plating material at a position of 3 / 4 of the thickness of the sintered layer from the surface of the sintered layer at the first end surface or the second end surface is 20% or more and 90% or less.

5. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The thickness of the metal layer is greater than or equal to 0.1 μm and less than 15.0 μm.

6. The multilayer ceramic capacitor according to claim 1 or 2, wherein: The sintered layer has a thickness of 1.0 μm or more and 100.0 μm or less.

7. The multilayer ceramic capacitor according to claim 1 or 2, wherein: A glass film is disposed around the metal layer and in contact with an end portion of the metal layer.