Positive electrode for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery

By adding sugar alcohol with carbon atoms of less than 10 to the positive electrode of the non-aqueous electrolyte secondary battery, the endothermic reaction of the hydration reaction suppresses heat generation, the difficulty of heating control in abnormal situations in the prior art is solved. The problem of high capacity and excellent heat suppression effect are achieved.

CN119013802APending Publication Date: 2024-11-22PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027184.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-23
Filing Date
2023-03-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the abnormal situation, the existing nonaqueous electrolyte secondary batteries are difficult to take into account high capacity and excellent heat suppression functions, especially in high capacity batteries, which are prone to cause sharp temperature rises. The prior art still has room for improvement in this regard.

Method used

The sugar alcohol having a carbon atom number of 10 or less is added to the positive electrode of the nonaqueous electrolyte secondary battery, and the content rate is less than 5% relative to the mass of the positive electrode active material, so as to endothermic heat generation by the hydration reaction of the sugar alcohol.

Benefits of technology

It achieves excellent heat generation suppression function when abnormalities occur without reducing the battery capacity, ensuring high capacity and good heat generation control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013802A_ABST
    Figure CN119013802A_ABST
Patent Text Reader

Abstract

A positive electrode for a non-aqueous electrolyte secondary battery according to an embodiment includes a positive electrode core material and a positive electrode mixture layer formed on a surface of the positive electrode core material. The positive electrode contains a sugar alcohol having 10 or less carbon atoms, and the content of the sugar alcohol is less than 5 mass% with respect to the mass of the positive electrode active material contained in the positive electrode mixture layer. The sugar alcohol is included, for example, in the positive electrode mixture layer. When the positive electrode mixture layer has a multilayer structure including a first layer and a second layer, it is preferable that the sugar alcohol content in the second layer is higher than the sugar alcohol content in the first layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a positive electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery using the positive electrode. Background Art

[0002] In recent years, non-aqueous electrolyte secondary batteries such as lithium-ion batteries have been widely used for applications requiring high capacity, such as vehicle-mounted applications and power storage applications. In addition, for non-aqueous electrolyte secondary batteries, a heat suppression function is required when abnormalities occur. The electrode body, which is the main component of the non-aqueous electrolyte secondary battery, has a great influence on these properties, so a lot of research has been done on the positive electrode. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery, in which a porous layer of filler particles containing metal hydroxide is formed between at least one of the positive and negative electrodes constituting the electrode body and the separator. Patent Document 1 records the effect of a battery confirmed to be excellent in safety in a foreign body internal short circuit test.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent No. 5574196 Summary of the invention

[0006] In non-aqueous electrolyte secondary batteries, it is an important issue to improve the heat suppression function when an abnormality occurs. In particular, in high-capacity batteries, a sharp temperature rise is easily caused when an abnormality occurs, so a higher degree of heat suppression function is required. In addition, it is necessary to improve the heat suppression function without causing the capacity of the battery to decrease, but it is not easy to take into account both high capacity and excellent heat suppression function. The prior art including the invention disclosed in patent document 1 still has room for improvement in terms of taking into account both high capacity and excellent heat suppression function.

[0007] The positive electrode for a non-aqueous electrolyte secondary battery disclosed herein is characterized in that it comprises a positive electrode core material and a positive electrode mixture layer formed on the surface of the positive electrode core material, the positive electrode comprises a sugar alcohol having a carbon number of less than 10, and the content of the sugar alcohol is less than 5% by mass relative to the mass of the positive electrode active material contained in the positive electrode mixture layer.

[0008] The nonaqueous electrolyte secondary battery of the present invention is characterized by comprising the above-mentioned positive electrode, a negative electrode, and a nonaqueous electrolyte.

[0009] According to the positive electrode for a nonaqueous electrolyte secondary battery of the present invention, it is possible to provide a nonaqueous electrolyte secondary battery having a high capacity and an excellent function of suppressing heat generation when abnormality occurs. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.

[0011] Figure 2 It is a cross-sectional view of a positive electrode as another example of the embodiment.

[0012] Figure 3 It is a cross-sectional view of a positive electrode as another example of the embodiment. DETAILED DESCRIPTION

[0013] As mentioned above, in non-aqueous electrolyte secondary batteries, it is an important issue to take into account both high capacity and excellent heat suppression function. The present inventors have conducted in-depth research to solve this issue, and successfully achieved a non-aqueous electrolyte secondary battery that ensures high capacity and excellent heat suppression function when abnormalities occur by using a positive electrode containing a sugar alcohol with a carbon number of 10 or less in an amount less than 5% by mass relative to the mass of the positive electrode active material.

[0014] It is believed that the sugar alcohol contained in the positive electrode exhibits a hydration reaction accompanied by endothermic action when an abnormality occurs in the battery. The hydration reaction is a reaction between water and sugar alcohol, and is carried out using water generated by the decomposition of the electrolyte when an abnormality occurs in the battery as an initiator. Therefore, in normal use of the battery, if the content of sugar alcohol is less than 5% by mass relative to the mass of the positive electrode active material, it will not affect the battery performance. Sugar alcohols with a carbon number of less than 10 have a large latent heat, so by adding them to the positive electrode, the heat generation when an abnormality occurs is highly suppressed. It should be noted that the filler of the metal hydroxide disclosed in Patent Document 1 also has a large latent heat, but it is difficult to suppress the heat generation as quickly as sugar alcohols with a carbon number of less than 10.

[0015] Hereinafter, an embodiment of a positive electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery using the positive electrode of the present invention will be described in detail with reference to the accompanying drawings. In addition, a configuration in which a plurality of embodiments and modifications described below are selectively combined is included in the present disclosure.

[0016] Hereinafter, a cylindrical battery in which a wound electrode body 14 is contained in an outer can 16 having a bottomed cylindrical shape is exemplified, but the outer body of the battery is not limited to a cylindrical outer can, and may be, for example, a square outer can (square battery), an outer body composed of a laminate sheet including a metal layer and a resin layer (laminated battery). In addition, the electrode body may also be a laminated electrode body in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated with separators therebetween.

[0017] Figure 1 Schematic diagram of a cross section of a non-aqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1As shown, the nonaqueous electrolyte secondary battery 10 includes a wound electrode body 14, a nonaqueous electrolyte (not shown), and an outer can 16 for storing the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 includes a positive electrode 11, a negative electrode 12, and a separator 13, and has a winding structure in which the positive electrode 11 and the negative electrode 12 are wound in a spiral shape with the separator 13 interposed therebetween. The outer can 16 is a metal container in a bottomed cylindrical shape with one side open in the axial direction, and the opening of the outer can 16 is blocked by a sealing body 17. In the following, for the sake of convenience of description, the sealing body 17 side of the battery is set as the upper side, and the bottom side of the outer can 16 is set as the lower side.

[0018] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substituted substance in which at least a portion of the hydrogen atoms of these solvents are replaced with halogen atoms such as fluorine. As an example of a non-aqueous solvent, ethylene carbonate (EC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and mixed solvents thereof may be cited. The electrolyte salt may be, for example, a lithium salt such as LiPF6. The non-aqueous electrolyte is not limited to a liquid electrolyte, but may also be a solid electrolyte.

[0019] The positive electrode 11, the negative electrode 12, and the separator 13 constituting the electrode body 14 are all strip-shaped long bodies, which are alternately stacked in the radial direction of the electrode body 14 by being wound into a spiral shape. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one circle larger than the positive electrode 11. In other words, the negative electrode 12 is formed to be longer than the positive electrode 11 in the length direction and the width direction (short direction). The separator 13 is formed to be at least one circle larger than the positive electrode 11, and two sheets are arranged in a manner of sandwiching the positive electrode 11. The electrode body 14 has a positive electrode lead 20 connected to the positive electrode 11 by welding or the like, and a negative electrode lead 21 connected to the negative electrode 12 by welding or the like.

[0020] Insulating plates 18 and 19 are disposed above and below the electrode body 14, respectively. Figure 1 In the example shown, the positive electrode lead 20 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode lead 21 extends to the bottom side of the outer can 16 through the outer side of the insulating plate 19. The positive electrode lead 20 is connected to the lower surface of the internal terminal plate 23 of the sealing body 17 by welding or the like, and the top plate of the sealing body 17, that is, the cover 27 electrically connected to the internal terminal plate 23 serves as the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the outer can 16 by welding or the like, and the outer can 16 serves as the negative terminal.

[0021] As described above, the outer can 16 is a metal container in a cylindrical shape with a bottom and an opening on one side in the axial direction. A gasket 28 is provided between the outer can 16 and the sealing body 17 to ensure the airtightness of the battery interior and the insulation between the outer can 16 and the sealing body 17. A groove 22 is formed in the outer can 16, which supports the sealing body 17 by extending a part of the side surface inward. The groove 22 is preferably formed in an annular shape along the circumference of the outer can 16, and supports the sealing body 17 on its upper surface. The sealing body 17 is fixed to the upper part of the outer can 16 through the groove 22 and the open end of the outer can 16 riveted to the sealing body 17.

[0022] The sealing body 17 has a structure in which an internal terminal plate 23, a lower valve body 24, an insulating component 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating component 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and an insulating component 25 is sandwiched between their respective peripheral portions. When an abnormality occurs in the battery and the internal pressure rises, the lower valve body 24 is deformed and broken in a manner of pushing the upper valve body 26 toward the cover 27 side, so that the current path between the lower valve body 24 and the upper valve body 26 is cut off. When the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.

[0023] Hereinafter, the positive electrode 11 , the negative electrode 12 , and the separator 13 , particularly the positive electrode 11 , will be described in detail.

[0024] [positive electrode]

[0025] The positive electrode 11 includes a positive electrode core material 30 and a positive electrode mixture layer 31 formed on the surface of the positive electrode core material 30. The positive electrode core material 30 can use a foil of a metal such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode 11, a film having the metal configured on the surface, etc. An example of the positive electrode core material 30 is a foil of aluminum or aluminum alloy having a thickness of 10 to 20 μm. The positive electrode mixture layer 31 includes a positive electrode active material, a conductive agent, and a binder, and is preferably formed on both sides of the positive electrode core material 30. An example of the thickness of the positive electrode mixture layer 31 is 50 to 150 μm on one side of the positive electrode core material 30.

[0026] The positive electrode 11 can be manufactured by coating a positive electrode mixture slurry containing a positive electrode active material, a conductive agent, a binder, etc. on the positive electrode core material 30, drying the coating, and then compressing to form a positive electrode mixture layer 31 on both sides of the positive electrode core material 30. As described in detail later, the positive electrode 11 contains a sugar alcohol having a carbon number of 10 or less, and the content of the sugar alcohol is less than 5% by mass relative to the mass of the positive electrode active material.

[0027] In the positive electrode mixture layer 31, as a positive electrode active material, a granular lithium metal composite oxide is included. The lithium metal composite oxide is a composite oxide containing metal elements such as Co, Mn, Ni, and Al in addition to Li. The metal element constituting the lithium metal composite oxide is, for example, at least one selected from Mg, Al, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Ge, Y, Zr, Sn, Sb, W, Pb, and Bi. Among them, it is preferred to contain at least one selected from Co, Ni, and Mn. As an example of a preferred composite oxide, a lithium metal composite oxide containing Ni, Co, and Mn and a lithium metal composite oxide containing Ni, Co, and Al can be cited.

[0028] The volume-based median particle size (D50) of the positive electrode active material is, for example, 1 to 25 μm, preferably 3 to 20 μm. D50 refers to the particle size at which the accumulation of frequencies in the volume-based particle size distribution reaches 50% from the smaller particle size, also known as the median diameter. The particle size distribution of the positive electrode active material can be measured using a laser diffraction particle size distribution measuring device (e.g., MT3000II manufactured by MicrotracBEL Co., Ltd.) using water as a dispersion medium. The content of the positive electrode active material is, for example, 90 to 99.5% by mass relative to the mass of the positive electrode mixture layer 31. It should be noted that the average particle size of the positive electrode active material obtained from the SEM image of the positive electrode cross section by the same method as the average particle size of the sugar alcohol described later is substantially the same value as the D50 measured using a laser diffraction particle size distribution measuring device.

[0029] Examples of the conductive agent contained in the positive electrode mixture layer 31 include carbon black such as acetylene black and Ketjen black, graphite, carbon nanotubes (CNTs), carbon nanofibers, and carbon materials such as graphene. The preferred content of the conductive agent varies depending on the type of the conductive agent, and is, for example, 0.1 to 10% by mass relative to the mass of the positive electrode mixture layer 31, and more preferably 0.2 to 5% by mass.

[0030] As the binder contained in the positive electrode mixture layer 31, fluorine-containing resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. In addition, these resins can also be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc. The content rate of the binder is, for example, 0.1 to 10% by mass relative to the mass of the positive electrode mixture layer 31, and more preferably 0.5 to 5% by mass.

[0031] As described above, the positive electrode 11 contains a sugar alcohol having a carbon number of 10 or less. Sugar alcohol is a chain or cyclic polyol in which the carbonyl group of a sugar is reduced, has a large latent heat, and functions as a heat absorber. When an abnormality occurs in the battery, it is important to be able to suppress heat generation, for example, at 150 to 250°C, but if a sugar alcohol having a carbon number of 10 or less is added to the positive electrode 11, effective heat absorption can be achieved at this temperature. It should be noted that when the carbon number of the sugar alcohol exceeds 10, the heat suppression effect when an abnormality occurs in the battery is greatly reduced.

[0032] The content of sugar alcohol is less than 5% by mass relative to the mass of the positive electrode active material contained in the positive electrode mixture layer 31. If the amount of sugar alcohol added is set to 5% or more of the mass of the positive electrode active material, although the heat suppression function when an abnormality occurs is improved, the battery capacity decreases sharply. Sugar alcohol exerts the effect of suppressing heat generation by adding a small amount, and the content of sugar alcohol relative to the mass of the positive electrode active material is preferably 0.5% by mass or more, and more preferably 1% by mass or more. In this case, the heat suppression effect when an abnormality occurs in the battery becomes more significant.

[0033] Sugar alcohol is contained in the positive electrode active material layer 31 together with the positive electrode active material, for example. Sugar alcohol is a particle whose average particle size is smaller than the average particle size of the positive electrode active material, and is dispersed in the positive electrode mixture layer 31. It should be noted that by adding sugar alcohol to the above-mentioned positive electrode mixture slurry, the positive electrode mixture layer 31 can contain sugar alcohol. Sugar alcohol may not be biased to exist in a part of the positive electrode active material layer 31 but may be dispersed in the entire layer. It is preferred that sugar alcohol is contained in each positive electrode mixture layer 31 formed on both sides of the positive electrode core material 30. Sugar alcohol is contained in each positive electrode mixture layer 31 at substantially the same concentration.

[0034] The carbon number of the sugar alcohol is preferably 8 or less, more preferably 6 or less. In addition, the carbon number of the sugar alcohol is preferably 4 or more. When a sugar alcohol having 4 to 6 carbon atoms is added to the positive electrode 11, they function effectively at 150 to 250° C., and the heat generation suppression effect when the battery is abnormal becomes more significant. Specific examples of preferred sugar alcohols include erythritol, threitol, pentaerythritol, xylitol, arabitol, mannitol, sorbitol, galactitol, inositol, and the like.

[0035] The sugar alcohol is preferably a chain molecule having 4 to 6 carbon atoms, and specifically, at least one selected from the group consisting of erythritol, threitol, pentaerythritol, xylitol, mannitol, and sorbitol is preferred. Among them, threitol and mannitol are particularly preferred.

[0036] The average particle size of the sugar alcohol is, for example, 0.05 to 5 μm, preferably 0.1 to 2 μm. If the average particle size of the sugar alcohol is within this range, a more effective endothermic effect is exerted at 150 to 250°C, and the heat suppression effect when an abnormality occurs in the battery becomes more significant compared to the case where the average particle size deviates from this range. The average particle size of the sugar alcohol can be adjusted, for example, by a high shear mixer. In addition, the average particle size of the sugar alcohol is measured by observing the positive electrode cross section using a scanning electron microscope (SEM). Specifically, the diameter of the circumscribed circle of the sugar alcohol particles extracted from the SEM image of the positive electrode cross section is used as the particle size, and the particle sizes of 100 randomly selected particles are averaged to obtain the average particle size of the sugar alcohol.

[0037] Figure 2 FIG. 2 is a cross-sectional view of a positive electrode including a positive electrode mixture layer 31 having a multilayer structure. Figure 2 In the illustrated positive electrode, the positive electrode mixture layer 31 includes a first layer 31a formed on the positive electrode core material 30 side and a second layer 31b formed on the positive electrode core material 30 via the first layer 31a. In this case, the content of sugar alcohol in the second layer 31b is preferably higher than the content of sugar alcohol in the first layer 31a. In other words, the positive electrode mixture layer 31 includes a first layer 31a with a low content of sugar alcohol and a second layer 31b with a higher content of sugar alcohol than the first layer 31a. In this case, it is easy to achieve both high capacity and excellent heat suppression function.

[0038] The content of sugar alcohol in the second layer 31b is, for example, 1.3 times or more of the content of sugar alcohol in the first layer 31a. In this case, the improvement effect of heat suppression becomes more significant. Sugar alcohol may also be contained substantially only in the second layer 31b. In addition, the positive electrode mixture layer 31 has a double-layer structure with different contents of sugar alcohol, but may also have more than three layers. The positive electrode mixture layer 31 may have a concentration gradient in which the content of sugar alcohol is higher as it is farther away from the positive electrode core material 30 side.

[0039] The types and contents of the positive electrode active material, the conductive agent, and the binder may be the same or different in the first layer 31a and the second layer 31b. In the present embodiment, the same type of positive electrode active material, conductive agent, and binder are used in the first layer 31a and the second layer 31b, respectively. In addition, the contents of the conductive agent and the binder relative to the mass of the positive electrode active material are substantially the same in each layer. That is, the first layer 31a and the second layer 31b are layers in which only the contents of the sugar alcohol relative to the mass of the positive electrode active material are different from each other. The types of sugar alcohols may be the same or different in the first layer 31a and the second layer 31b.

[0040] Figure 2The positive electrode exemplified in the example can be made using two positive electrode mixture slurries having different contents of sugar alcohol relative to the mass of the positive electrode active material. After applying the first positive electrode mixture slurry having a small amount of added sugar alcohol on the positive electrode core material 30, the second positive electrode mixture slurry having a large amount of added sugar alcohol is applied on the coating film, thereby forming a positive electrode mixture layer 31 having a double-layer structure including a first layer 31a and a second layer 31b.

[0041] Figure 3 It is a cross-sectional view of a positive electrode including a surface layer 32 containing a sugar alcohol. Figure 3 The positive electrode illustrated in the example includes a surface layer 32 formed on the positive electrode mixture layer 31. The surface layer 32 is a layer having a higher content of sugar alcohol than the positive electrode mixture layer 31. The surface layer 32 is composed of, for example, sugar alcohol and a binder, and can be formed by applying a slurry containing sugar alcohol and a binder to the surface of the positive electrode mixture layer 31. Figure 3 In the example shown, the sugar alcohol may not be substantially contained in the positive electrode mixture layer 31 , but may be substantially contained only in the surface layer 32 .

[0042] The thickness of the surface layer 32 is preferably 50% or less of the thickness of the positive electrode mixture layer 31. Since it is difficult to accurately compare the positive electrode mixture layer 31 and the surface layer 32 by thickness ratio, if the layers are compared by mass ratio, the mass of the surface layer 32 is, for example, 0.1 to 5%, more preferably 0.14 to 1%, of the mass of the positive electrode mixture layer 31. If the mass ratio of the positive electrode mixture layer 31 to the surface layer 32 is within this range, it is easy to achieve both high capacity and excellent heat suppression function.

[0043] [negative electrode]

[0044] The negative electrode 12 includes a negative electrode core material 40 and a negative electrode mixture layer 41 formed on the surface of the negative electrode core material 40. The negative electrode core material 41 can be made of a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, or a film having the metal disposed on the surface. An example of the negative electrode core material 40 is a foil of copper or a copper alloy having a thickness of 5 to 15 μm. The negative electrode mixture layer 41 includes a negative electrode active material, a binder, and a conductive agent as required, and is preferably formed on both sides of the negative electrode core material 40. The thickness of the negative electrode mixture layer 41 is, for example, 30 to 150 μm on one side of the negative electrode core material 40. The negative electrode 12 can be manufactured by coating a negative electrode mixture slurry containing a negative electrode active material, a binder, etc. on the negative electrode core material 40, drying the coating, and then compressing the negative electrode mixture layer 41 to form the negative electrode mixture layer 41 on both sides of the negative electrode core material 40.

[0045] In the negative electrode mixture layer 41, as the negative electrode active material, a carbon-based active material that reversibly stores and releases lithium ions is included. Preferred carbon-based active materials are natural graphites such as flake graphite, massive graphite, and earthy graphite, artificial graphites such as massive artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB), etc. In addition, from the viewpoint of improving the energy density, etc., as the negative electrode active material, a Si-based active material containing Si can be used.

[0046] As an example of the Si-based active material, a silicon alloy, a silicon compound, and a composite material containing Si can be cited. Among them, a composite material containing Si is preferred. A preferred composite material is a composite particle including an ion-conducting layer and Si particles dispersed in the ion-conducting layer. A conductive layer can also be formed on the surface of the composite particle containing Si. An example of the composite particle is a composite particle having an island structure in which fine Si particles are substantially uniformly dispersed in an amorphous silica phase and having the general formula SiO x (0 < x ≤ 2). In addition, the ion-conducting layer can be a silicate phase or an amorphous carbon phase represented by the general formula Li 2z SiO (2+z) (0 < z < 2).

[0047] As the binder contained in the negative electrode mixture layer 41, for example, PAN, polyimide, acrylic resin, polyolefin, styrene-butadiene rubber (SBR), etc. can be used. In addition, CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc. can be included in the negative electrode mixture layer 41. In addition, a conductive agent such as carbon black or CNT can be added to the negative electrode mixture layer 41.

[0048] [Separator]

[0049] The separator 13 uses a porous sheet having ion permeability and insulation. As a specific example of the porous sheet, a microporous film, a woven fabric, a non-woven fabric, etc. can be cited. As the material of the separator 13, polyolefins such as polyethylene and polypropylene, cellulose, etc. are preferred. The separator 13 can have a single-layer structure or a multilayer structure. In addition, a resin layer with high heat resistance such as an aromatic polyamide resin can be formed on the surface of the separator 13.

[0050] A filler layer including an inorganic filler can be formed at the interface between the separator 13 and at least one of the positive electrode 11 and the negative electrode 12. As the inorganic filler, for example, oxides containing metal elements such as Ti, Al, Si, Mg, etc., phosphate compounds, etc. can be cited. The filler layer can be formed by coating a slurry containing the filler on the surface of the positive electrode 11, the negative electrode 12, or the separator 13.

[0051] Examples

[0052] Hereinafter, the present disclosure will be described in further detail by way of examples, but the present disclosure is not limited to these examples.

[0053] <Example 1>

[0054] [Production of positive electrode]

[0055] As the positive electrode active material, LiNi 0.91 Co 0.06 Al 0.03 O2 represents a composite oxide with an average particle size of 5.9 μm. The positive electrode active material, acetylene black, polyvinylidene fluoride and xylitol are mixed in a solid component mass ratio of 100:1:1:1, and N-methyl-2-pyrrolidone (NMP) is used as a dispersion medium to prepare a positive electrode mixture slurry. Next, the positive electrode mixture slurry is applied to both sides of a positive electrode core material composed of aluminum foil, the coating is dried, and compressed using a roller. Then, the positive electrode core material is cut into a specified electrode size to obtain a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode core material. It should be noted that the average particle size of xylitol in the positive electrode mixture layer is 1.8 μm (the average particle size of xylitol used in other embodiments and comparative examples is also the same).

[0056] [Production of negative electrode]

[0057] As the negative electrode active material, 95 parts by mass of graphite and 5 parts by mass of SiO X A mixture of Si-containing materials represented by (X=1). A dispersion of a negative electrode active material, sodium salt of CMC and SBR is mixed at a solid content mass ratio of 100:1:1, and water is used as a dispersion medium to prepare a negative electrode mixture slurry. Next, the negative electrode mixture slurry is applied on a negative electrode core material composed of copper foil, and after the coating is dried and rolled, the negative electrode core material is cut into a specified electrode size to obtain a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode core material.

[0058] [Preparation of non-aqueous electrolyte]

[0059] LiPF 6 was dissolved in a mixed solvent of ethylene carbonate (EC) and dimethyl carbonate (DMC) at a volume ratio of 3:7 (25° C.) to give a concentration of 1 M, thereby preparing a non-aqueous electrolyte solution.

[0060] [Preparation of test battery]

[0061] The positive electrode and negative electrode with lead wires were wound through a separator to prepare a wound electrode body. The electrode body was inserted into an outer body made of aluminum laminate film and vacuum dried at 105°C for 2 hours. Then, a nonaqueous electrolyte was injected into the outer body, and the opening of the outer body was sealed to obtain a test battery (nonaqueous electrolyte secondary battery).

[0062] <Example 2>

[0063] In the preparation of the positive electrode, a test cell was prepared in the same manner as in Example 1 except that the amount of xylitol added was changed to 3% by mass relative to the mass of the positive electrode active material.

[0064] <Example 3>

[0065] A test cell was prepared in the same manner as in Example 1 except that mannitol having an average particle size of 1.5 μm was used instead of xylitol in the preparation of the positive electrode (the average particle size of mannitol used in other Examples and Comparative Examples was the same).

[0066] <Example 4>

[0067] A test cell was prepared in the same manner as in Example 2, except that mannitol was used instead of xylitol in the preparation of the positive electrode.

[0068] <Example 5>

[0069] A test cell was prepared in the same manner as in Example 1 except that threitol having an average particle size of 1.5 μm was used instead of xylitol in the preparation of the positive electrode (the average particle size of threitol used in other Examples and Comparative Examples was the same).

[0070] <Example 6>

[0071] A test cell was prepared in the same manner as in Example 2, except that threitol was used instead of xylitol in the preparation of the positive electrode.

[0072] <Comparative Example 1>

[0073] A test cell was produced in the same manner as in Example 1 except that sugar alcohol (xylitol) was not added in the production of the positive electrode.

[0074] <Comparative Example 2>

[0075] A test cell was prepared in the same manner as in Example 1 except that magnesium hydroxide having an average particle size of 2.9 μm (the average particle size of magnesium hydroxide in Comparative Example 3 was also the same) was used in place of xylitol in the preparation of the positive electrode.

[0076] <Comparative Example 3>

[0077] A test cell was prepared in the same manner as in Example 2, except that magnesium hydroxide was used instead of xylitol in the preparation of the positive electrode.

[0078] <Comparative Example 4>

[0079] In the preparation of the positive electrode, a test cell was prepared in the same manner as in Example 1 except that the amount of xylitol added was changed to 5% by mass relative to the mass of the positive electrode active material.

[0080] <Comparative Example 5>

[0081] In the preparation of the positive electrode, a test cell was prepared in the same manner as in Example 3 except that the amount of mannitol added was changed to 5% by mass relative to the mass of the positive electrode active material.

[0082] <Comparative Example 6>

[0083] In the preparation of the positive electrode, a test cell was prepared in the same manner as in Example 5, except that the amount of threitol added was changed to 5% by mass relative to the mass of the positive electrode active material.

[0084] The performance of each test battery of the examples and comparative examples was evaluated by the following method. The evaluation results are shown in Table 1.

[0085] [Measurement of battery capacity]

[0086] The test battery to be evaluated was charged at a constant current of 0.2 C until the battery voltage reached 4.2 V under a temperature environment of 25° C., and then discharged at a constant current of 0.5 C until the battery voltage reached 2.5 V. The discharge capacity during this charge and discharge was determined as the battery capacity.

[0087] [Determination of calorific value]

[0088] The positive electrode plate was cut into 2×2 cm, and the negative electrode plate was cut into 2.1×2.1 cm, and they were placed opposite each other to prepare a battery for evaluation, and a nail penetration test was performed according to the following procedure.

[0089] Under the environment of 25°C, the evaluation battery is charged at 0.2C until the battery voltage reaches 4.2V, and then charged at a constant voltage until the current value is equivalent to 0.05C. Then, under the environment of 25°C, the tip of a round nail (diameter 2.7mm) is brought into contact with the center of the charged battery. The round nail pierces at a speed of 1mm / second. The piercing round nail stops immediately after detecting the drop in battery voltage caused by an internal short circuit. At any time after the battery is short-circuited by the round nail, the current value I of the short-circuit current and the battery voltage V are continuously measured. Then, the heat generation at any time is calculated by accumulating the product of the current value I and the voltage V (electricity) over time.

[0090] [Table 1]

[0091]

[0092] As shown in Table 1, the test batteries of the examples all had less heat generation when abnormalities occurred than the test batteries of Comparative Examples 1 to 3 in which no sugar alcohol was added to the positive electrode, and had excellent heat suppression function. In addition, the test batteries of the examples had higher capacities than the test batteries of Comparative Examples 4 to 6 in which the addition rate of sugar alcohol to the positive electrode active material was 5% by mass or more. In the test batteries of Comparative Examples 4 to 6, the capacities were greatly reduced.

[0093] This result shows that a nonaqueous electrolyte secondary battery having a high capacity and excellent heat generation suppression function can be realized only when a positive electrode to which a sugar alcohol having 10 or less carbon atoms is added in an amount of less than 5 mass % based on the positive electrode active material is used.

[0094] Description of Reference Numerals

[0095] 10 non-aqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 16 outer can, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 groove, 23 internal terminal plate, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cover, 28 gasket, 30 positive electrode core material, 31 positive electrode mixture layer, 31a first layer, 31b second layer, 32 surface layer, 40 negative electrode core material, 41 negative electrode mixture layer

Claims

1. A positive electrode for a non-aqueous electrolyte secondary battery, comprising a positive electrode core material and a positive electrode mixture layer formed on a surface of the positive electrode core material. The positive electrode contains a sugar alcohol having 10 or less carbon atoms, The content of the sugar alcohol is less than 5% by mass relative to the mass of the positive electrode active material contained in the positive electrode mixture layer.

2. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The sugar alcohol is at least one selected from the group consisting of erythritol, threitol, pentaerythritol, xylitol, mannitol and sorbitol.

3. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The positive electrode mixture layer includes a first layer formed on the positive electrode core material side and a second layer formed on the positive electrode core material via the first layer. The content of the sugar alcohol in the second layer is higher than the content of the sugar alcohol in the first layer.

4. The positive electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The positive electrode includes a surface layer formed on the positive electrode mixture layer. The content of the sugar alcohol in the surface layer is higher than the content of the sugar alcohol in the positive electrode mixture layer.

5. The positive electrode for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein The average particle size of the sugar alcohol is smaller than the average particle size of the positive electrode active material, and the average particle size of the sugar alcohol is 0.1 to 2 μm.

6. A secondary battery comprising the positive electrode according to any one of claims 1 to 5, Negative electrode, and Non-aqueous electrolyte.