Material and device for filtering or purifying gas and liquid and preparation method

The lack of filtering or purifying gases or liquids in the prior art and the capture of volatile radionuclides in nuclear facilities is solved by using "sandwich" filter materials and stainless steel wire fiber cordierite structures formed using micron-scale fibers. The problem is that efficient filtering, purification and capture effects are achieved.

CN119015791APending Publication Date: 2024-11-26LANZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411404123.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art cannot effectively filter or purify specific components in gases or liquids, and cannot effectively capture volatile radionuclides such as Cs, Te, I, Tc, Kr generated in nuclear facilities, affecting the safety of nuclear facilities. and radiation safety.

Method used

Use a similar felt-like fiber felt formed of micron-scale polymer fibers, glass fibers or ceramic fibers, and load adsorbent materials in their voids or surfaces to form a filter material with a "sandwich" structure, which is used to filter or purify gas, Liquid; For gaseous Te, the stainless steel wire fiber felt formed by fine stainless steel wire fibers and a "sandwich" structure carrying cordierite is captured.

Benefits of technology

It realizes simple and effective filter material preparation for filtration or purification of gas and liquids, has toughness that is resistant to high temperature and high pressure and good filtration and purification effects, and can efficiently capture gaseous Te, filling the protection and purification of radioactive gaseous tellurium blank.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015791A_ABST
    Figure CN119015791A_ABST
Patent Text Reader

Abstract

The invention discloses a material and device for filtering or purifying gas and liquid and a preparation method. The filter material for filtering or purifying the gas and the liquid is composed of a felt-like fibrofelt formed by micron-scale polymer fibers or glass fibers or ceramic fibers or metal fibers and an adsorption material located in gaps of the fibrofelt or on the fiber surface of the fibrofelt. The filter material can resist high-temperature, high-pressure and high-flow impact, has good flexibility, can optimize the filtering and purifying effects, can be cut into any required shape, and can be folded into a wave-shaped wrinkle structure or stacked together, so that the filter material can be used for filtering and purifying. The device has a wide application prospect in the fields of purification of various radioactive gases in gas masks and closed spaces and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a material for filtering or purifying gas or liquid, a preparation method and a device, and a material for efficiently capturing tellurium in a gas medium, a preparation method and a device. Background Art

[0002] Devices for filtering or purifying gas or liquid can be divided into many categories, such as filter screens or certain adsorbent materials. Needle-punched filter felt is also a common technology for improving filter screens. CN114832507A discloses a filter felt formed by interlacing and weaving multiple layers of metal fibers and other materials. This filter felt composed of multiple fibers can withstand high temperatures, maintain filtering effects, and has the advantages of good purification and filtering efficiency. However, its preparation is relatively complicated, and the disclosed method cannot prepare a filter material for filtering or purifying specific components in gas or liquid.

[0003] On the other hand, long-lived actinides and volatile radionuclides (such as Cs, Te, I, Tc, Kr, etc.) are produced during the nuclear fission process in nuclear power production, and the cladding material may rupture due to overheating of the fuel rods, causing coolant loss and the release of highly toxic and volatile radionuclides. How to effectively capture, remove and separate volatile radionuclides such as Cs, Te, I, Tc, Kr from the exhaust gas stream is a problem that needs to be solved for the safety and radiation of nuclear facilities. Summary of the invention

[0004] One object of the present invention is to provide a filter material that can overcome the shortcomings of the prior art, is relatively simple to prepare and can effectively filter or purify gases and liquids. A second object of the present invention is to provide a filter material for effectively capturing gaseous Te, as well as a method for preparing such a material and a filtering device prepared using such a material.

[0005] The filter material for filtering or purifying gas or liquid of the present invention is composed of a felt-like fiber felt formed by micron-scale polymer fibers, glass fibers, ceramic fibers or metal fibers and an adsorbent material in the gaps of the fiber felt or on the fiber surface of the fiber felt.

[0006] The preparation method of the filter material of the present invention is to place a micron-sized polymer fiber, glass fiber, ceramic fiber or metal fiber in any one or a combination of at least two thereof and a dissociation liquid in a dissociator for dissociation and dispersion, and then add a powdered adsorbent material in the dissociator, and then filter out a felt-like substance with adsorbent material in its gaps after sufficient dissociation and dispersion, and then press, dry and sinter the obtained felt to obtain the filter material. The dissociation liquid described in the preparation method of the filter material of the present invention refers to a liquid that can effectively dissociate and disperse the fiber material used, such as water or viscous liquids with large molecular weights such as hydroxymethyl cellulose and polyacrylamide. The specific type of dissociation liquid used depends on the fiber type and the required fiber dispersion degree. In the preparation process of the filter material of the present invention, if the fiber material used is a polymer fiber with a low melting point, the corresponding sintering temperature should also be reduced.

[0007] The filter material for filtering or purifying gas or liquid of the present invention can also be a "sandwich" structure consisting of a fiber felt similar to a felt formed by micron-scale polymer fibers, glass fibers, ceramic fibers or metal fibers, an adsorption layer composed of adsorption materials in the gaps of the fiber felt or on the fiber surface of the fiber felt, and a protective layer composed of arbitrary fibers placed above and below the adsorption layer. The adsorption material in the adsorption layer of the filter material of the present invention is in the gap formed by the fiber material. The "sandwich" structure of the protective layers on both sides of the adsorption layer of the filter material of the present invention can effectively prevent the particles from falling during the filtration or purification operation, thereby affecting the subsequent purification or filtering effect of gas or liquid. The "sandwich" structure of the present invention is more suitable for filtering operations with large flow and / or high pressure.

[0008] The preparation method of the filter material described in the present invention is as follows: A. placing micrometer-sized polymer fibers, glass fibers, ceramic fibers, or metal fibers in any one or a combination of at least two thereof and a dissociation liquid in a dissociator for dissociation and dispersion. The dissociation liquid described herein is a liquid determined according to the different fibers used and the different dispersibility, such as polyacrylamide, deionized water, hydroxymethyl cellulose, etc., and filtering out after sufficient dissociation and dispersion to obtain a protective layer; B. placing any one or a combination of at least two of micrometer-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and a dissociation liquid in a dissociator for dissociation and dispersion, and then adding a powdered adsorption material to the dissociator, and filtering out an adsorption layer similar to a felt material having gaps therein with adsorption material after sufficient dissociation and dispersion; C. Placing the protective layers prepared in step A on both sides of the adsorption layer formed in step B to form a "sandwich" structure; D. After the "sandwich" structure prepared in step C is pressed at a pressure of 300 kPa and dried at 110 °C, the precursor is cut into an appropriate shape, calcined in a reducing atmosphere, and then washed to obtain the final filter material.

[0009] In the specific preparation process, a protective layer of fiber felt may be first formed, and then an adsorption layer consisting of a fiber layer wrapping an adsorption material may be formed on the protective layer, and then another protective layer of fiber felt may be formed on the obtained adsorption layer.

[0010] It should be noted that in specific applications of the present invention, the protective layer may also be made of other fiber materials, and even filter paper may be used as the protective layer.

[0011] The capture material of tellurium in gas medium of the present invention has a "sandwich" structure, which comprises a stainless steel wire fiber felt similar to a felt formed by fine stainless steel wire fibers, an adsorption layer of adsorption material in the gaps of the stainless steel wire fiber felt or on the surface of the stainless steel wire felt fibers, and a protective layer composed of stainless steel wire fiber felt layers similar to a felt formed by stainless steel wire fibers respectively placed on both sides of the adsorption layer, wherein the adsorption layer includes silver-loaded cordierite.

[0012] The capture material preparation method of the present invention is: A. Place the stainless steel wire fiber and the dissociation liquid in a dissociator for full dissociation and dispersion, and then filter to form a protective layer of the stainless steel fiber felt; B. Putting stainless steel wire fiber and dissociation liquid into the dissociator for dissociation and dispersion, and then adding silver-loaded cordierite into the dissociator, and filtering out the adsorption layer of the stainless steel felt with adsorption material in its gaps after sufficient dissociation and dispersion; C. Placing the protective layers prepared in step A on both sides of the adsorption layer formed in step B to form a "sandwich" structure; D. The "sandwich" structure precursor prepared in step C is pressed at a pressure of 300 kPa and dried at 110 °C, then cut into appropriate shapes, calcined in a reducing atmosphere, and then washed to obtain the final capture material.

[0013] Preferably, in the capture material preparation method of the present invention, in step B, in addition to adding silver-loaded cordierite to the dissociator, lignin is also added. The lignin in the adsorption layer is easily ashed at high temperature during sintering, and its structure can enhance the strength of the adsorption material. More preferably, the lignin in the capture material of the present invention is coniferous wood lignin, because coniferous wood lignin has the best effect.

[0014] In the capture material preparation method of the present invention, a fiber felt protective layer can be formed first, then an adsorption layer consisting of a fiber layer wrapping an adsorption material can be formed on the protective layer, and then a fiber felt protective layer can be formed on the obtained adsorption layer.

[0015] The device for capturing tellurium in a gas medium of the present invention comprises a stainless steel tubular object with an input port and an output port respectively arranged at both ends thereof and at least one layer of the aforementioned capturing material placed in the tube.

[0016] The preparation method of the silver-loaded cordierite of the present invention is: (1) Grinding a cordierite block through a sieve to obtain cordierite fine particles, washing them with tap water and deionized water in sequence, and then washing them with anhydrous ethanol, draining the liquid and drying them, and calcining the cordierite particles at 300 °C under an inert atmosphere; (2) The cordierite treated in the above step is placed in a silver solution, and then oscillated to react, and then fully washed with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven. The cordierite is then placed in an argon gas flow rate of 300 mL / min and the furnace temperature is raised to 300°C at 5°C / min. The temperature is maintained to remove residual moisture and the silver ions are reduced to elemental silver by high-temperature calcination to obtain silver-loaded cordierite.

[0017] The preparation method of the filter material of the present invention is similar to a papermaking process or a traditional felt-making process, that is, the dissociated material is separated from the dissociation liquid to obtain a "shaped" filter material, and the adsorbent material is directly retained in the gaps in the felt or deposited on the fiber surface. As long as the dissociable and dispersed material is available, it can be very conveniently loaded into the fiber felt. Therefore, the preparation method of the present invention is extremely simple and completely solves the shortcomings of the prior art. The filter material of the present invention can withstand high temperature and high pressure, and has good toughness and filtering and purification effects. It can be cut into any desired shape by cutting, and folded into a wavy pleated structure or stacked together, so as to flexibly design the structure and shape of the integral reactor. Therefore, the material of the present invention has broad application prospects in the fields of gas masks, purification of various radioactive gases in confined spaces, etc.

[0018] The highly efficient tellurium capture material in the gas medium of the present invention fills the gap in the protection and purification of radioactive gaseous tellurium in my country. The porosity of the capture material of the present invention can be adjusted by changing the amount of adsorbent material used and the pressure during the molding process. The capture material can partially or even completely eliminate the influence of internal diffusion, has low resistance, and the three-dimensional network structure can well avoid the undesirable fluid distribution phenomena such as channeling and back mixing caused by filling reasons, as well as radial diffusion limitation. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1It is a schematic diagram of the structure of the decomposed adsorption layer and the protective layer of the present invention.

[0020] Figure 2 It is a schematic diagram of an embodiment of a device for capturing tellurium in a gas medium according to the present invention.

[0021] Figure 3 It is the XPS spectrum of the Ag adsorption layer of the capture material.

[0022] Figure 4 is the XRD spectrum of the capture material adsorption layer.

[0023] Figure 5 is the XRD spectrum of the capture material protective layer.

[0024] Figure 6 It is the filtering performance of the capture material for gaseous tellurium.

[0025] Figure 7 This is the XPS spectrum of the protective layer Te after the capture material adsorbs gaseous tellurium.

[0026] Figure 8 This is the XPS spectrum of the Te adsorption layer after the capture material adsorbs gas tellurium.

[0027] Fig. 9 is the pressure drop across a single layer of capture material at different flow rates.

[0028] Fig.10 It captures the stress conditions of the material under different deformation degrees.

[0029] Figure 1 and Figure 2 Middle: 1 is an input port arranged on the tubular object, 2 is a stainless steel tubular object, 3 is a left protective layer, 4 is an adsorption layer, 5 is a right protective layer, 6 is a fixing bolt and nut connecting the tubular object and the upper tube cover, 7 is the tube cover, and 8 is an output port arranged on the tube cover. DETAILED DESCRIPTION

[0030] The present invention is explained below in conjunction with embodiments.

[0031] The filter material for filtering or purifying gas or liquid of the present invention is composed of a felt-like fiber felt formed by micron-sized polymer fibers or glass fibers or ceramic fibers or metal fibers and an adsorbent material in the gaps of the fiber felt or on the fiber surface of the fiber felt. The adsorbent material of the present invention can be any existing powdered adsorbent material, such as activated carbon powder or bentonite, or it can be some other special adsorbent material, such as cordierite described later in the present invention.

[0032] The filter material for filtering or purifying gas or liquid of the present invention may also be a "sandwich" structure consisting of a felt-like fiber felt formed of micron-scale polymer fibers, glass fibers, ceramic fibers, or metal fibers, an adsorption layer composed of adsorption materials in the gaps of the fiber felt or on the fiber surface of the fiber felt, and a protective layer composed of arbitrary fibers placed above and below the adsorption layer. The adsorption material may be any existing powdered adsorption material, such as activated carbon powder or bentonite, or may be some other special adsorption material, such as cordierite described later in the present invention. The advantages of adding protective layers on both sides of the adsorption layer of the present invention are to ensure the coverage rate of the captured material, reduce or avoid the loss of adsorbed particles, and ensure that the granular material does not fall off during use.

[0033] The capture material for tellurium in gas medium disclosed in the present invention has a "sandwich" structure, which comprises a stainless steel wire fiber felt similar to a felt formed by fine stainless steel wire fibers, an adsorption layer of adsorption material in the gaps of the stainless steel wire fiber felt or on the surface of the stainless steel wire felt fibers, and a protective layer composed of a stainless steel wire fiber felt layer similar to a felt formed by stainless steel wire fibers placed above and below the adsorption layer, wherein the adsorption material in the adsorption layer is silver-loaded cordierite.

[0034] The filter material preparation method of the present invention is to place any one or a combination of at least two of micron-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and a dissociation liquid in a dissociator for dissociation and dispersion. The dissociation liquid here refers to solutions such as polyacrylamide, deionized water, hydroxymethyl cellulose, etc. Then, a powdered adsorption material, such as a silicon-based porous material or a carbon-based porous material such as activated carbon, is added to the dissociator, and after sufficient dissociation and dispersion, a felt-like substance containing the adsorption material in its pores is filtered out, and the obtained felt-like substance is sintered to obtain the filter material.

[0035] Another filter material preparation method of the present invention is: A. placing micrometer-sized polymer fibers, glass fibers, ceramic fibers, or metal fibers in any one or a combination of at least two thereof and a dissociation liquid in a dissociator for dissociation and dispersion, wherein the dissociation liquid used is a solution of polyacrylamide, deionized water, or hydroxymethyl cellulose, and after complete dissociation, a fiber layer is obtained; B. placing any one or a combination of at least two of micrometer-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and a dissociation liquid in a dissociator for dissociation and dispersion, and filtering out a felt-like adsorption layer having adsorption materials in its gaps on the fiber layer in step A after sufficient dissociation and dispersion; C. Repeat step A and filter the fiber layer on the adsorption layer formed in step B to form a "sandwich" structure with the adsorption layer in the middle and protective layers on both sides; D. The "sandwich" structure prepared in step C is calcined in a reducing atmosphere to obtain a final product.

[0036] The capture material obtained through the aforementioned treatment retains the adsorbent material in the gaps within the fiber mat.

[0037] The preparation method of the capture material for tellurium in gas medium of the present invention is: A. placing the stainless steel wire fiber and the polyacrylamide solution in a dissociator for dissociation and dispersion, and then filtering to form a protective layer of the stainless steel fiber felt; B. placing stainless steel wire fiber and polyacrylamide in a dissociator for dissociation and dispersion, and then adding silver-loaded cordierite and lignin in a mass ratio of 16:1 in the dissociator, and filtering out an adsorption layer similar to a felt material in the gaps of the stainless steel fiber layer in step A after sufficient dissociation and dispersion; C. Repeat step A and filter the fiber layer on the adsorption layer formed in step B to form a "sandwich" structure with the adsorption layer in the middle and protective layers on both sides; D. The "sandwich" structure obtained in step C is squeezed and dried, cut into the required shape and size, and then calcined. The squeezing and drying temperature and pressure are 110°C and 300 kPa, respectively. It is then calcined at 1070°C in an atmosphere of argon:hydrogen = 4:6 to obtain a capture material with a "sandwich" structure.

[0038] The capture material prepared by the above preparation method retains silver-loaded cordierite in the gaps within the adsorption layer, see Appendix Figure 1 As shown, 3 and 5 are the left and right protective layers respectively, and 4 is the adsorption layer.

[0039] The preparation method of silver-loaded cordierite of the present invention is: (1) Pretreatment of cordierite: Grind the large piece of cordierite with an agate mortar and pass it through a sieve to separate cordierite of a specific particle size. Wash it with tap water and deionized water three times, then wash it with anhydrous ethanol three times. After draining the liquid, place it in a vacuum drying oven at 95 °C for 24 h. After the surface liquid is dry, place the cordierite in a tube furnace and calcine it for 60 min (inert atmosphere, 300 °C) to ensure that the cordierite is completely dry and store it in a dry place for future use.

[0040] (2) Preparation of silver-loaded cordierite: 10 g of the cordierite treated as described above was weighed and placed in a 10 g / L silver nitrate solution, and then shaken at 25 °C for 24 h (400 rpm). After the reaction was complete, it was washed with deionized water and anhydrous ethanol three times respectively. After draining the liquid, it was placed in a vacuum drying oven at 95 °C for 24 h. After the surface liquid was dry, the cordierite was placed in a tube furnace with an argon gas flow rate of 300 sccm. The furnace temperature was raised to 300 °C at a rate of 5 °C / min and maintained at this temperature for 240 min to remove residual moisture and reduce silver ions to elemental silver through high-temperature calcination. The silver-loaded cordierite capture material was obtained and stored in an inert atmosphere (glove box) for use in preparing the capture material.

[0041] Attached Figure 2 It is a schematic structural diagram of a specific embodiment of the capture device for tellurium in a gas medium of the present invention, which is composed of a section of stainless steel tubular object 2 and a tube cover 7 fixed to the tubular object, and at least one capture material having an adsorption layer 4 and protective layers 3 and 5 on both sides thereof is placed in the tubular object. The tubular object 2 and the tube cover 7 are fixed to each other by fixing bolts and nuts 6 on the flanges, a sealing gasket is provided between the tube 2 and the cover 7 (Note: not shown in the figure), and an input port 1 and an output port 8 are provided at both ends of the tube 2 and the cover 7, respectively. In the specific preparation, a plurality of sheets of material consisting of a protective layer and an adsorption layer are cut into suitable shapes with a tool, and are placed one by one in a stainless steel tube and pressed tightly. In the actual experiment of the present invention, 18 sheets of capture material are used, and Figure 1 The figure is an example, only three pieces are drawn.

[0042] The captured material Figure 2 The capture device shown is installed in a dynamic adsorption experimental system, and the gas generation temperature, carrier gas flow rate, adsorption temperature, and system absolute pressure are set. After a certain reaction time, the carrier gas is stopped and the temperature is cooled to room temperature. The capture material is taken out, the adsorbed tellurium is eluted with concentrated nitric acid, and tested with ICP-OES.

[0043] (1) Capture material pressure drop test The captured material is cut into a circular shape, placed directly in a stainless steel column, fixed with sealant on all sides, and loaded into a pressure testing system to detect the pressure.

[0044] (2) Capture material tensile strength test The manufactured material was cut into a rectangular structure with a length of 15 cm and a width of 2 cm, and then a tensile strength tester was used to measure the stress conditions of the capture material at different deformation distances. In order to compare the superiority of the capture material, commonly used filter materials such as glass fiber were used for comparison.

[0045] Test situation: Figure 3The XPS spectrum shows that the 3d orbital of Ag is split into two orbitals (3 / 2d and 5 / 2d orbitals), and the binding energies of the corresponding peak positions are 368.47 and 368.47 eV, which are consistent with the binding energy of elemental silver. Obviously, elemental silver is successfully loaded onto the cordierite particles.

[0046] Figure 4 The XRD spectrum of the cordierite in the adsorption layer of the capture material shows the characteristic peak of silver 111 in the XRD spectrum after loading silver, and it conforms to the standard spectrum of PDF#99-0094. Figure 5 The XRD spectrum shows that the surface of the protective layer of the capture material is stainless steel wire and complies with PDF#33-0397. This indicates that the capture material was successfully synthesized and the material is in a "sandwich" shape.

[0047] (3) Test of the adsorption performance of capture materials for gas tellurium: In order to demonstrate the superiority of silver-loaded capture materials in capturing gaseous tellurium, a capture material and a capture material without silver were used for comparison.

[0048] Figure 6 The results show that under the same experimental conditions, 14 layers can completely remove the gaseous tellurium introduced into the capture material, and the adsorption amount of the first layer can reach 74.1 mg / g. However, the capture material without silver cannot completely remove the gaseous tellurium introduced, and the adsorption amount of the first layer (25.4 mg / g) is lower than that of the capture material. The purification of gaseous tellurium is only physical filtration.

[0049] The XPS spectrum of Te revealed that ( Figure 7 and Figure 8 ) The tellurium adsorbed in the protective layer of the capture material is elemental tellurium, and the adsorption layer is Ag2Te. Therefore, the capture material's adsorption of gaseous tellurium includes not only chemical adsorption but also physical filtration.

[0050] Capture Material Pressure Drop Test: Fig. 9 It shows that the flow rate and the pressure drop of the capture material are linearly correlated, and at a flow rate of 1.6 m / s, the single-layer capture material has a pressure difference of 1.807 kPa. Compared with existing filters, the capture material has an extremely low pressure drop, which proves the feasibility of the capture material in subsequent applications.

[0051] (4) Capture material tensile strength test: Fig.10 It shows that the capture material can withstand a force of 15.1 N, while the glass fiber can only withstand a force of 11.4 N. Therefore, the capture material of the present invention for gaseous tellurium has excellent pressure-bearing capacity, and the stability of the material is guaranteed for application scenarios with higher flow rates.

[0052] Taking the above performance experiment as an example, the high-efficiency tellurium capture material in the gas medium of the present invention has the characteristics of foldable and cuttable, high temperature resistance, high pressure bearing strength, low pressure drop, physical filtration and chemical adsorption of gaseous tellurium, and exhibits good purification ability. The capture material can be used in conjunction with other system devices in a primary circuit, and can also be used as a mask protective material to protect tellurium aerosols. The capture material can be used for the specific capture of tellurium gas and tellurium aerosols in flowing high-temperature gaseous environments and natural environments at room temperature, respectively, filling the gap in the protection and purification of radioactive gaseous tellurium in my country, and has broad application prospects.

[0053] Through the experiments of the material for capturing tellurium in gas medium of the present invention, it can be known that the filter material prepared by the present invention can be fully used for filtering or purifying relevant gases or liquids.

Claims

1. A filter material for filtering or purifying gas or liquid, characterized in that The filter material is composed of a felt-like fiber felt formed by micron-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and an adsorbent material in the gaps of the fiber felt or on the fiber surface of the fiber felt.

2. A filter material for filtering or purifying gas or liquid, characterized in that The filter material is a "sandwich" structure consisting of a felt-like fiber felt formed by micron-sized polymer fibers, glass fibers, ceramic fibers or metal fibers, an adsorption layer consisting of adsorption materials in the gaps of the fiber felt or on the fiber surface of the fiber felt, and a protective layer consisting of arbitrary fiber layers above and below the adsorption layer.

3. A material for capturing tellurium in a gas medium, characterized in that The material has a "sandwich" structure of a stainless steel fiber felt formed by fine stainless steel wire fibers, an adsorption layer composed of adsorption materials in the gaps of the stainless steel fiber felt or on the surface of the stainless steel fiber felt fibers, and a protective layer composed of stainless steel fiber felt layers formed by stainless steel wire fibers respectively placed on both sides of the adsorption layer.

4. A device for capturing tellurium in a gas medium, characterized in that The capture device is a stainless steel tube with an input port and an output port at both ends thereof and at least one piece of capture material according to claim 3 placed in the tube.

5. The method for preparing the filter material according to claim 1, characterized in that: Place micron-sized polymer fiber, glass fiber, ceramic fiber or metal fiber, any one or a combination of at least two of them and a dissociation liquid in a dissociator for dissociation and dispersion, then add powdered adsorption material to the dissociator, filter out a felt-like substance with adsorption material in its gaps after sufficient dissociation and dispersion, and then sinter the obtained felt-like substance to obtain the filter material.

6. The method for preparing the filter material according to claim 2, characterized in that: A. placing any one or a combination of at least two of micrometer-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and a dissociation liquid in a dissociator for dissociation and dispersion, and filtering out after sufficient dissociation and dispersion to obtain a protective layer; B. placing any one or a combination of at least two of micrometer-sized polymer fibers, glass fibers, ceramic fibers or metal fibers and a dissociation liquid in a dissociator for dissociation and dispersion, and then adding a powdered adsorption material to the dissociator, and filtering out an adsorption layer similar to a felt material having gaps therein with adsorption material after sufficient dissociation and dispersion; C. Placing the protective layers prepared in step A on both sides of the adsorption layer formed in step B to form a "sandwich" structure; D. After the "sandwich" structure prepared in step C is squeezed and dried, the precursor is cut into an appropriate shape, calcined in a reducing atmosphere, and then washed to obtain the final filter material.

7. The method for preparing a filter material according to claim 6, characterized in that First, a protective layer of fiber felt is formed, then an adsorption layer consisting of an adsorption material wrapped by a fiber layer is formed on the protective layer, and then another protective layer of fiber felt is formed on the obtained adsorption layer.

8. The method for preparing the capture material according to claim 3, characterized in that: A. Place the stainless steel wire fiber and the dissociation liquid in a dissociator for full dissociation and dispersion, and then filter to form a protective layer of the stainless steel fiber felt; B. Putting stainless steel wire fiber and dissociation liquid into the dissociator for dissociation and dispersion, and then adding silver-loaded cordierite into the dissociator, and filtering out the adsorption layer of the stainless steel felt with adsorption material in its gaps after sufficient dissociation and dispersion; C. Placing the protective layers prepared in step A on both sides of the adsorption layer formed in step B to form a "sandwich" structure; D. After the "sandwich" structure prepared in step C is pressed at a pressure of 300 kPa and dried at 110 °C, the precursor is cut into an appropriate shape, calcined in a reducing atmosphere, and then washed to obtain the final capture material.

9. The method for preparing a capture material according to claim 8, characterized in that In addition to the silver-loaded cordierite added to the disintegrator in step B, lignin is also added.

10. The method for preparing a capture material according to claim 9, characterized in that The added lignin is softwood lignin.

11. The method for preparing a capture material according to claim 7, 8, 9 or 10, characterized in that First, a fiber felt protective layer is formed, then an adsorption layer consisting of a fiber layer wrapping an adsorption material is formed on the protective layer, and then a fiber felt protective layer is formed on the obtained adsorption layer.

12. A method for preparing silver-loaded cordierite, characterized in that: (1) Grinding a cordierite block through a sieve to obtain cordierite fine particles, washing them with tap water and deionized water in sequence, and then washing them with anhydrous ethanol, draining the liquid and drying them, and calcining the cordierite particles at 300 °C under an inert atmosphere; (2) The cordierite treated in the above step is placed in a silver solution for oscillation reaction, and then fully washed with deionized water and anhydrous ethanol, and then dried in a vacuum drying oven. The cordierite is then placed in an argon gas flow rate of 300 mL / min and the furnace temperature is raised to 300°C at 5°C / min. The temperature is maintained to remove residual moisture and the silver ions are reduced to elemental silver by high-temperature calcination to obtain silver-loaded cordierite.

Citation Information

Patent Citations

  • Preparation method of novel spherical activated carbon composite fabric

    CN104492165A

  • Preparation method of high-strength and high-precision filtering material

    CN110090494A

  • Filter material and device for filtering or purifying gas and liquid

    CN223432056U

  • Filtering member for collecting dust

    JP2005040646A