Composite catalyst for PET degradation and application thereof

By using a composite catalyst to degrade PET into terephthalic acid and ethylene glycol under suitable conditions, multiple shortcomings in PET waste treatment are solved, achieving efficient, economical, and environmentally friendly treatment results.

CN119016053APending Publication Date: 2024-11-26YANGZHOU POLYTECHNIC INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411124041.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing PET waste treatment methods suffer from problems such as declining quality of mechanical recycling, high cost and complexity of chemical recycling, and environmental pollution from incineration. There is a lack of efficient, economical and environmentally friendly treatment solutions.

Method used

The composite catalyst, consisting of metal oxides, metal ions, catalyst promoters, and a support, is optimized to degrade PET under suitable conditions, producing terephthalic acid and ethylene glycol with few byproducts and high reaction stability.

Benefits of technology

It achieves efficient degradation of PET, generating high-purity terephthalic acid and ethylene glycol, avoiding the quality degradation of mechanical recycling, the high cost of chemical recycling, and the environmental pollution of incineration, providing an economical and environmentally friendly treatment solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016053A_ABST
    Figure CN119016053A_ABST
Patent Text Reader

Abstract

The invention discloses a composite catalyst for PET degradation and application thereof, and belongs to the technical field of environmental protection, the catalyst comprises the following components: a metal oxide, metal ions, a catalytic promoter and a carrier, the metal oxide is selected from titanium dioxide, silicon dioxide or aluminum oxide, the metal ions are selected from cobalt, nickel, zinc or iron, and the catalytic promoter is selected from cobalt, nickel, zinc or iron. The catalytic promoter is sodium hydroxide or potassium hydroxide, and the carrier is activated carbon or zeolite. By optimizing the combination of the metal oxide, the metal ions, the catalytic promoter and the carrier, efficient degradation of PET is realized under proper conditions, terephthalic acid and ethylene glycol are generated, byproducts are few, the reaction is stable, the purity is high, quality reduction of mechanical recovery, high-cost complex operation of chemical recovery and environmental pollution of incineration are avoided, and the method is suitable for industrial production. An economic, environment-friendly and efficient PET waste treatment scheme is provided, and resource recycling and environmental protection are promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of environmental protection, and in particular to a composite catalyst for PET degradation and application thereof. Background Art

[0002] In modern society, with the extensive use and disposal of plastic products, the disposal of polyethylene terephthalate (PET) waste has become an important global environmental issue. Existing PET waste treatment methods mainly include mechanical recycling, chemical recycling and incineration. However, the degradation of PET and the mixing of impurities during the mechanical recycling process lead to a decrease in the quality of the recycled materials; although chemical recycling can decompose PET, it usually requires high temperature and high pressure and a large amount of chemical reagents, and the process is complicated and costly; incineration will produce harmful gases and cause secondary pollution. Therefore, how to develop an efficient, economical and environmentally friendly PET degradation method has become a technical problem that needs to be solved urgently.

[0003] The above information disclosed in this Background section is only for enhancement of understanding of the background of the present disclosure and therefore it may contain information that does not constitute the prior art that is already known to one of ordinary skill in the art. Summary of the invention

[0004] The purpose of the present invention is to provide a composite catalyst for PET degradation and its application. By optimizing the combination of metal oxides, metal ions, catalytic promoters and carriers, efficient degradation of PET is achieved under suitable conditions to generate terephthalic acid and ethylene glycol with few by-products, stable reaction and high purity, avoiding the quality decline of mechanical recycling, the high cost and complex operation of chemical recycling and the environmental pollution of incineration, providing an economical, environmentally friendly and efficient PET waste treatment plan, promoting resource recycling and environmental protection, and solving the problems in the above-mentioned background technology.

[0005] In order to achieve the above object, the present invention provides the following technical solution: a composite catalyst for PET degradation, the catalyst comprising the following components:

[0006] Metal oxide, metal ion, catalyst promoter and carrier, wherein the metal oxide is selected from titanium dioxide, silicon dioxide or aluminum oxide, the metal ion is selected from cobalt, nickel, zinc or iron, the catalyst promoter is sodium hydroxide or potassium hydroxide, and the carrier is activated carbon or zeolite.

[0007] Preferably, the mass percentage of the metal oxide is 5-30%, the mass percentage of the metal ion is 1-10%, the mass percentage of the catalyst promoter is 1-5%, and the mass percentage of the carrier is 55-93%.

[0008] Preferably, the metal oxide is titanium dioxide, the metal ions are cobalt ions, the catalyst promoter is sodium hydroxide, and the carrier is activated carbon.

[0009] The preparation method of the composite catalyst comprises the following steps:

[0010] a. mixing metal oxides and metal ions to obtain a mixed solution;

[0011] b. Add the catalyst to the mixed solution and stir evenly;

[0012] c. Add the carrier to the mixed solution and continue stirring to make the mixture uniform;

[0013] d. Drying and calcining the mixture to obtain the composite catalyst.

[0014] 5. The preparation method according to claim 4, characterized in that the roasting temperature is 300-600°C and the roasting time is 2-6 hours.

[0015] Preferably, the calcination temperature is 300-600° C., and the calcination time is 2-6 hours.

[0016] The method for degrading PET using a composite catalyst comprises the following steps:

[0017] a. Crush the PET waste to a particle size of 1-5 mm;

[0018] b. mixing the crushed PET waste with the composite catalyst;

[0019] c. Carry out the reaction at a temperature of 150-300° C. for 2-10 hours to obtain a degradation product.

[0020] Preferably, the reaction is carried out in an inert gas atmosphere, and the inert gas is nitrogen or argon.

[0021] Preferably, the degradation products include terephthalic acid, ethylene glycol and a small amount of oligomers.

[0022] A method for recovering PET degradation products comprises the following steps:

[0023] a. dissolving the degradation product obtained by the method according to any one of claims 6 to 8 in water;

[0024] b. Recover terephthalic acid and ethylene glycol by filtration and evaporation respectively.

[0025] Preferably, the ethylene glycol is further purified by distillation to a purity of more than 99%.

[0026] In the above technical solution, the technical effects and advantages provided by the present invention are:

[0027] The invention provides a composite catalyst for PET degradation, which overcomes multiple deficiencies in existing PET waste treatment methods. By selecting an optimized combination of metal oxides, metal ions, catalytic aids and carriers, and reacting under suitable temperature and time conditions, efficient degradation of PET is achieved. Experimental results show that these composite catalysts can degrade PET into terephthalic acid and ethylene glycol under relatively mild conditions, and the amount of by-product oligomers generated is small, the reaction stability is high, and the purity of the degradation products is high. At the same time, the method avoids the quality degradation of mechanically recycled materials, the high cost and complex operation of chemical recycling, and the environmental pollution problem of incineration treatment, and provides an economical, environmentally friendly and efficient PET waste treatment solution, which helps to promote the recycling of resources and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0029] Figure 1 The present invention is a flow chart of the method for preparing the composite catalyst. DETAILED DESCRIPTION

[0030] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these example embodiments are provided so that the description of the present disclosure will be more comprehensive and complete, and the concept of the example embodiments will be fully conveyed to those skilled in the art.

[0031] The present invention provides Figure 1 A composite catalyst for PET degradation and its application are shown, the catalyst comprises the following components:

[0032] Metal oxide, metal ion, catalyst promoter and carrier, wherein the metal oxide is selected from titanium dioxide, silicon dioxide or aluminum oxide, the metal ion is selected from cobalt, nickel, zinc or iron, the catalyst promoter is sodium hydroxide or potassium hydroxide, and the carrier is activated carbon or zeolite.

[0033] Embodiment 1:

[0034] Preparation of titanium dioxide / cobalt ion composite catalyst and PET degradation:

[0035] Catalyst preparation:

[0036] raw material:

[0037] Titanium dioxide (TiO2): 20%; cobalt ion (Co 2+ ): 5%; sodium hydroxide (NaOH): 3%; activated carbon: 72%;

[0038] Steps: a. Mix 10 grams of titanium dioxide and 2.5 grams of cobalt salt (such as cobalt nitrate), add 100 milliliters of distilled water, stir evenly, and obtain a mixed solution.

[0039] b. Slowly add 3 grams of sodium hydroxide to the mixed solution and continue stirring until the solution is uniform.

[0040] c. Add 40 grams of activated carbon into the mixed solution and continue stirring for 1 hour to ensure uniform mixing.

[0041] d. Dry the mixture at 105°C for 12 hours and then calcine at 500°C for 4 hours to obtain a composite catalyst.

[0042] PET degradation experiment:

[0043] raw material:

[0044] PET waste: 20 g (crushed to a particle size of 2 mm); composite catalyst: 2 g;

[0045] step:

[0046] a. Mixing PET waste with the composite catalyst.

[0047] b. Place the mixture in a reactor and react at 200°C for 6 hours.

[0048] c. After the reaction is completed, cool to room temperature and remove the degradation product.

[0049] The experimental data are as follows:

[0050]

[0051] The catalyst preparation process of Example 1 details the mass percentage of each component and the specific preparation steps. The process involves mixing titanium dioxide and cobalt salt, adding sodium hydroxide and mixing with activated carbon, and finally drying and calcining to obtain a composite catalyst. This process ensures the composition and structure of the catalyst, thereby improving its catalytic effect in PET degradation.

[0052] The PET degradation experimental procedure clearly describes the specific operation process of mixing crushed PET waste with the composite catalyst and reacting at 200°C for 6 hours. By maintaining consistent operating conditions in different experiments, the repeatability and reliability of the experimental results can be ensured.

[0053] The experimental data clearly show the yields of terephthalic acid, ethylene glycol and oligomers in different experiments. By comparing the data of three experiments, it can be seen that the results of each experiment are very close, indicating that the catalyst has good stability and high efficiency under these conditions.

[0054] The specific data are as follows:

[0055] Terephthalic acid yield: The yields of the three experiments were 13 g, 12.8 g and 13.2 g, respectively, with an average of 13 g, indicating that the catalyst has a stable degradation effect on PET and a high yield.

[0056] Ethylene glycol yield: The yields of the three experiments were 6 g, 6.1 g, and 5.9 g, respectively, with an average of 6 g, indicating that the recovery rate of ethylene glycol was high and the fluctuation between experiments was small.

[0057] Oligomers: The oligomer yields of the three experiments were 1 g, 1.1 g, and 0.9 g, respectively, with an average of 1 g, indicating that the amount of oligomers produced was small and the reaction was relatively complete.

[0058] These data provide strong experimental support for the practical application of the present invention, and prove the effectiveness and stability of the titanium dioxide / cobalt ion composite catalyst in PET degradation. The experimental data show that the catalyst can efficiently degrade PET at 200°C for 6 hours to produce terephthalic acid and ethylene glycol, and the amount of by-product oligomers generated is relatively small.

[0059] Embodiment 2:

[0060] Preparation of silica / nickel ion composite catalyst and PET degradation:

[0061] Catalyst preparation:

[0062] raw material:

[0063] Silicon dioxide (SiO2): 15%; Nickel ion (Ni 2 +): 8%; Potassium hydroxide (KOH): 2%; Zeolite: 75%;

[0064] step:

[0065] a. Mix 7.5 g of silicon dioxide with 4 g of nickel salt (such as nickel nitrate), add 200 ml of distilled water, stir evenly, and obtain a mixed solution.

[0066] b. Slowly add 2 grams of potassium hydroxide to the mixed solution and continue stirring until the solution is uniform.

[0067] c. Add 50 grams of zeolite into the mixed solution and continue stirring for 2 hours to make the mixture uniform.

[0068] d. Dry the mixture at 110° C. for 24 hours, and then calcine at 450° C. for 5 hours to obtain a composite catalyst.

[0069] PET degradation experiment:

[0070] raw material:

[0071] PET waste: 30 g (crushed to a particle size of 3 mm); composite catalyst: 3 g;

[0072] step:

[0073] a. Mixing PET waste with the composite catalyst.

[0074] b. Place the mixture in a reactor and react at 250°C for 4 hours.

[0075] c. After the reaction is completed, cool to room temperature and remove the degradation product.

[0076] The experimental data are as follows:

[0077]

[0078] The raw materials and their mass percentages required for the catalyst preparation process are given in detail in Example 2, and specific preparation steps are described, including mixing, stirring, drying and calcining. Through these steps, the uniformity and catalytic activity of the silica / nickel ion composite catalyst are ensured.

[0079] The PET degradation experimental procedure details the specific operation process of mixing the crushed PET waste with the composite catalyst and reacting it at 250℃ for 4 hours. By maintaining consistent operating conditions in different experiments, the repeatability and reliability of the experimental results can be ensured.

[0080] The experimental data clearly show the yields of terephthalic acid, ethylene glycol and oligomers in different experiments. By comparing the data of three experiments, it can be seen that the results of each experiment are very close, indicating that the catalyst has good stability and high efficiency under these conditions.

[0081] The specific data are as follows:

[0082] Terephthalic acid yield: The yields of the three experiments were 21 g, 20.8 g and 21.2 g, respectively, with an average of 21 g, indicating that the catalyst has a stable degradation effect on PET and a high yield.

[0083] Ethylene glycol yield: The yields of the three experiments were 7.5 g, 7.6 g, and 7.4 g, respectively, with an average of 7.5 g, indicating that the recovery rate of ethylene glycol was high and the fluctuation between experiments was small.

[0084] Oligomers: The oligomer yields of the three experiments were 1.5 g, 1.6 g, and 1.4 g, respectively, with an average of 1.5 g, indicating that the amount of oligomers produced was small and the reaction was relatively complete.

[0085] These data provide strong experimental support for the practical application of the present invention, and prove the effectiveness and stability of the silica / nickel ion composite catalyst in PET degradation. Through the experimental data, it can be seen that the catalyst can efficiently degrade PET at 250°C for 4 hours to produce terephthalic acid and ethylene glycol, and the amount of by-product oligomers generated is relatively small, which further verifies the practicality and feasibility of the present invention.

[0086] Example 3: Preparation of aluminum oxide / zinc ion composite catalyst and PET degradation

[0087] Catalyst preparation:

[0088] raw material:

[0089] Alumina (Al2O3): 25%; zinc ion (Zn 2+ ): 3%; sodium hydroxide (NaOH): 1%; activated carbon: 71%;

[0090] Steps: a. Mix 12.5 g of aluminum oxide with 1.5 g of zinc salt (such as zinc nitrate), add 50 ml of distilled water, stir evenly, and obtain a mixed solution.

[0091] b. Slowly add 1 gram of sodium hydroxide to the mixed solution and continue stirring until the solution is uniform.

[0092] c. Add 35.5 g of activated carbon to the mixed solution and continue stirring for 1 hour to ensure uniform mixing.

[0093] d. Dry the mixture at 100°C for 18 hours, and then calcine at 550°C for 3 hours to obtain a composite catalyst.

[0094] PET degradation experiment:

[0095] raw material:

[0096] PET waste: 25 g (crushed to a particle size of 4 mm); composite catalyst: 2.5 g;

[0097] step:

[0098] a. Mixing PET waste with the composite catalyst.

[0099] b. Place the mixture in a reactor and react at 180°C for 8 hours.

[0100] c. After the reaction is completed, cool to room temperature and remove the degradation product.

[0101] The experimental data are as follows:

[0102]

[0103] The raw materials and their mass percentages required for the catalyst preparation process are given in detail in Example 3, and specific preparation steps are described, including mixing, stirring, drying and calcining. Through these steps, the uniformity and catalytic activity of the aluminum oxide / zinc ion composite catalyst are ensured.

[0104] The PET degradation experimental procedure details the specific operation process of mixing the crushed PET waste with the composite catalyst and reacting it at 180°C for 8 hours. By maintaining consistent operating conditions in different experiments, the repeatability and reliability of the experimental results can be ensured.

[0105] The experimental data is presented in a table, clearly showing the yields of terephthalic acid, ethylene glycol and oligomers in different experiments. By comparing the data of three experiments, it can be seen that the results of each experiment are very close, indicating that the catalyst has good stability and high efficiency under these conditions. The specific data are as follows:

[0106] Terephthalic acid yield: The yields of the three experiments were 15 g, 14.8 g and 15.2 g, respectively, with an average of 15 g, indicating that the catalyst has a stable degradation effect on PET and a high yield.

[0107] Ethylene glycol yield: The yields of the three experiments were 8.75 g, 8.8 g, and 8.7 g, respectively, with an average of 8.75 g, indicating that the recovery rate of ethylene glycol was high and the fluctuation between experiments was small.

[0108] Oligomers: The oligomer yields of the three experiments were 1.25 g, 1.4 g, and 1.3 g, respectively, with an average of 1.3 g, indicating that the amount of oligomers produced was small and the reaction was relatively complete.

[0109] These data provide strong experimental support for the practical application of the present invention, and prove the effectiveness and stability of the aluminum oxide / zinc ion composite catalyst in PET degradation. Through the experimental data, it can be seen that the catalyst can efficiently degrade PET at 180°C for 8 hours to produce terephthalic acid and ethylene glycol, and the amount of by-product oligomers generated is relatively small, which further verifies the practicality and feasibility of the present invention.

[0110] The invention provides a composite catalyst for PET degradation, which overcomes multiple deficiencies in existing PET waste treatment methods. By selecting an optimized combination of metal oxides (such as titanium dioxide, silicon dioxide, aluminum oxide), metal ions (such as cobalt, nickel, zinc), catalytic aids (such as sodium hydroxide or potassium hydroxide) and carriers (such as activated carbon or zeolite), and reacting under suitable temperature and time conditions, efficient degradation of PET is achieved. Experimental results show that these composite catalysts can degrade PET into terephthalic acid and ethylene glycol under relatively mild conditions, and the amount of byproduct oligomers generated is small, the reaction stability is high, and the purity of the degradation products is high. At the same time, the method avoids the quality degradation of mechanically recycled materials, the high cost and complex operation of chemical recycling, and the environmental pollution problem of incineration treatment, and provides an economical, environmentally friendly and efficient PET waste treatment solution, which is helpful to promote resource recycling and environmental protection.

[0111] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A composite catalyst for PET degradation, characterized in that: The catalyst comprises the following components: Metal oxide, metal ion, catalyst promoter and carrier, wherein the metal oxide is selected from titanium dioxide, silicon dioxide or aluminum oxide, the metal ion is selected from cobalt, nickel, zinc or iron, the catalyst promoter is sodium hydroxide or potassium hydroxide, and the carrier is activated carbon or zeolite.

2. The composite catalyst according to claim 1, characterized in that The mass percentage of the metal oxide is 5-30%, the mass percentage of the metal ion is 1-10%, the mass percentage of the catalyst promoter is 1-5%, and the mass percentage of the carrier is 55-93%.

3. The composite catalyst according to claim 2, characterized in that The metal oxide is titanium dioxide, the metal ions are cobalt ions, the catalyst promoter is sodium hydroxide, and the carrier is activated carbon.

4. The method for preparing a composite catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: a. mixing metal oxides and metal ions to obtain a mixed solution; b. Add the catalyst to the mixed solution and stir evenly; c. Add the carrier to the mixed solution and continue stirring to make the mixture uniform; d. Drying and calcining the mixture to obtain the composite catalyst.

5. The preparation method according to claim 4, characterized in that: The calcination temperature is 300-600° C., and the calcination time is 2-6 hours.

6. A method for degrading PET using the composite catalyst according to any one of claims 1 to 3, characterized in that: The following steps are involved: a. Crush the PET waste to a particle size of 1-5 mm; b. mixing the crushed PET waste with the composite catalyst; c. Carry out the reaction at a temperature of 150-300° C. for 2-10 hours to obtain a degradation product.

7. The PET degradation method according to claim 6, characterized in that: The reaction is carried out in an inert gas atmosphere, wherein the inert gas is nitrogen or argon.

8. The PET degradation method according to claim 7, characterized in that: The degradation products include terephthalic acid, ethylene glycol and a small amount of oligomers.

9. A method for recovering PET degradation products, characterized in that: The following steps are involved: a. dissolving the degradation product obtained by the method according to any one of claims 6 to 8 in water; b. Recover terephthalic acid and ethylene glycol by filtration and evaporation respectively.

10. The recycling method according to claim 9, characterized in that: Ethylene glycol is further purified by distillation to a purity of more than 99%.