Nano fluorine-doped bismuth titanate and preparation method thereof
Through the hydrothermal synthesis of nanofluorine-doped bismuth titanate, the problem of high stability and cost of photocatalysts in the water oxidation process is solved, and the efficient degradation of organic pollutants and water oxidation reaction is achieved. It is suitable for sewage treatment and reduces maintenance Cost and extended use cycle.
Patent Information
- Application Number
- CN202310599530.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
Existing photocatalysts have poor stability, high cost and are difficult to apply on a large scale during water oxidation, especially because the high activation energy of O-O bonds limits the effective cracking of water, resulting in low energy conversion efficiency.
Nanofluoro-doped bismuth titanate is prepared by hydrothermal reaction, and is synthesized using fluoro-doped titanium dioxide and bismuth-containing compounds under closed heating conditions to form a catalyst for degradation of organic pollutants and water oxidation reaction.
It has achieved efficient degradation of organic pollutants of methyl orange and methylene blue, with a degradation rate of more than 90%, and has good stability and long life. It is suitable for actual sewage treatment and reduces maintenance costs and service cycles.
Smart Images

Figure HDA0004248346390000011 
Figure HDA0004248346390000021 
Figure HDA0004248346390000022
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysis, and in particular relates to nano fluorine-doped bismuth titanate and a preparation method thereof. Background Art
[0002] At present, the problem of energy consumption is imminent. Not only is natural resources limited, but fossil energy consumption accounts for more than 70% of global greenhouse gas emissions, which has an adverse impact on the environment and climate. Therefore, finding clean energy to replace traditional energy is the core of solving the energy problem.
[0003] Photocatalytic technology can convert solar energy into chemical energy, and has received widespread attention from scientists in recent years. Using photocatalytic technology to decompose water to produce hydrogen has the advantages of large reserves, low pollution and sustainable development, and is one of the ways to solve energy and environmental problems. Since the oxidation and reduction of water are both competitive reactions, and the generation of oxygen is a four-electron transfer process, and the activation energy barrier formed by the OO bond is high, the large-scale cracking of water to produce hydrogen is limited. Researchers have developed and manufactured various catalysts, hoping to find ones that show relatively excellent performance in water oxidation. For example, ruthenium-based catalysts and iridium-based catalysts are effective water oxidants, but they have poor stability and high cost, and it is still difficult to meet the requirements of practical applications.
[0004] In recent years, ion doping is considered to be an effective way to improve the activity of photocatalysts. Non-metallic doping generally replaces oxygen ions in oxide semiconductors, changing the chemical environment of the cations they are bonded to, which can achieve the effect of regulating the energy band structure of photocatalysts or the absorption intensity or specific surface area of visible light, thereby enhancing the redox activity of photocatalysts. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a nano fluorine-doped bismuth titanate, which is prepared by hydrothermal reaction using fluorine-doped titanium dioxide and bismuth-containing compounds as raw materials. The preparation method is simple and easy to control. The obtained nano fluorine-doped bismuth titanate has high catalytic activity and good stability, can be repeatedly used in actual organic sewage treatment, and maintains stable photocatalytic performance, thereby reducing sewage treatment costs, extending maintenance cycles, reducing maintenance costs, and facilitating application in actual sewage treatment.
[0006] The object of the present invention is to provide a nano-fluorine-doped bismuth titanate, which is prepared from fluorine-doped titanium dioxide and a bismuth-containing compound as raw materials in a water solvent under closed heating conditions. The nano-fluorine-doped bismuth titanate has a lamellar structure.
[0007] The object of the present invention is to provide a method for preparing nano fluorine-doped bismuth titanate, which uses fluorine-doped titanium dioxide and a bismuth-containing compound as raw materials and is prepared in a water solvent under closed heating conditions.
[0008] The fluorine-doped titanium dioxide is obtained by adding fluoride and titanium compound into a solvent, heating and reacting under closed conditions, and calcining.
[0009] The present invention also provides the use of the nano-fluorine-doped bismuth titanate, which is used as a photocatalyst to degrade organic pollutants, such as methyl orange and / or methylene blue. The degradation efficiency of the nano-fluorine-doped bismuth titanate on organic pollutants is higher than 90%.
[0010] The nano-fluorine-doped bismuth titanate provided by the present invention has the following beneficial effects:
[0011] (1) The nano-fluorine-doped bismuth titanate provided by the present invention has good photocatalytic performance and can effectively degrade organic dye pollutants such as methyl orange and methylene blue, with a degradation rate of more than 90%.
[0012] (2) The nano-fluorine-doped bismuth titanate provided by the present invention has good stability as a photocatalyst in the process of degrading organic pollution, can be repeatedly used in the catalytic degradation process, has a long service life, extends the maintenance cycle, reduces the amount of catalyst used and the maintenance cost, and is more conducive to the promotion and application in actual sewage treatment.
[0013] (3) The nano-fluorine-doped bismuth titanate provided by the present invention can also be used as a water oxidant, with good activity and stability, further meeting the requirements of practical use. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 (a) shows the XRD patterns of TiO2 prepared in Comparative Example 1 of the present invention and 0.25F-TiO2 prepared in Example 1; Figure 1 (b) shows an enlarged view of the 25.31° position in the XRD diagram of TiO2 prepared in Comparative Example 1 of the present invention and 0.25F-TiO2 prepared in Example 1;
[0015] Figure 2 The XRD patterns of 0.1F-BTO, 0.25F-BTO, 0.8F-BTO prepared in Example 1 of the present invention and BTO prepared in Comparative Example 1 are shown;
[0016] Figure 3 The Raman spectra of BTO prepared in Comparative Example 1 of the present invention, 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO prepared in Example 1 are shown;
[0017] Figure 4SEM images of TiO2 and BTO prepared in Comparative Example 1 of the present invention and 0.1F-TiO2 and 0.1F-BTO prepared in Example 1 are shown;
[0018] Figure 5 SEM images of 0.25F-TiO2, 0.8F-TiO2, 0.25F-BTO, and 0.8F-BTO prepared in Example 1 of the present invention are shown;
[0019] Figure 6 (a) Figure 6 (b) shows a TEM image of BTO prepared in Comparative Example 1 of the present invention; Figure 6 (c) shows a high resolution transmission scanning electron microscope (HRTEM) of BTO prepared in Comparative Example 1 of the present invention;
[0020] Figure 7 The photocatalytic degradation efficiency of BTO, 0.1F-BTO, 0.25F-BTO and 0.8F-BTO on methyl orange in the present invention is shown;
[0021] Figure 8 The photodegradation kinetics fitting curves of BTO, 0.1F-BTO, 0.25F-BTO and 0.8F-BTO to methyl orange in the present invention are shown;
[0022] Fig. 9 The degradation rate curve of methyl orange by three-cycle photocatalytic degradation of methyl orange by 0.25F-BTO in the present invention is shown;
[0023] Fig.10 (a) shows the oxygen production of pure water oxidation reaction catalyzed by BTO and 0.25F-BTO as photocatalysts in the present invention; Fig.10 (b) shows the oxygen production rate of the water oxidation reaction in which BTO and 0.25F-BTO are used as photocatalysts to add a hole sacrificial agent HLSA in the present invention;
[0024] Fig.11 The present invention shows the comparison of the changes in the cyclic oxygen production using BTO and 0.25F-BTO as photocatalysts;
[0025] Fig.12 (a) shows the transient photocurrent response spectra of BTO and 0.25F-BTO of the present invention; Fig.12 (b) shows the EIS Nyquist curves of the BTO of the present invention and 0.25F-BTO; Fig.12 (c) shows the steady-state photoluminescence spectra of BTO and 0.25F-BTO of the present invention; Fig.12 (d) shows the time-resolved transient luminescence decay spectra of BTO of the present invention and 0.25F-BTO. DETAILED DESCRIPTION
[0026] The present invention is described in detail below through specific implementation modes, and the characteristics and advantages of the present invention will become clearer and more specific with these descriptions.
[0027] The invention provides a nano fluorine-doped bismuth titanate, which is prepared using fluorine-doped titanium dioxide and a bismuth-containing compound as raw materials in a water solvent under closed heating conditions.
[0028] The present invention also provides a method for preparing the nano fluorine-doped bismuth titanate, which uses fluorine-doped titanium dioxide and a bismuth-containing compound as raw materials and is prepared in a water solvent under closed heating conditions.
[0029] The fluorine-doped titanium dioxide is obtained by adding fluoride and titanium compound into a solvent, heating and reacting under closed conditions, and calcining.
[0030] The fluoride is selected from inorganic fluorides, preferably ammonium fluoride.
[0031] The titanium compound is selected from one or more of titanate compounds and titanate ester compounds, preferably one or more of titanate ester compounds, more preferably one or more of tetrabutyl titanate, tetraisopropyl titanate and tetraethyl titanate.
[0032] The solvent is selected from one or more alcohol solvents, preferably selected from alkanols with a carbon number of 1-4, more preferably one or more of ethanol, propanol, n-butanol and isopropanol, such as anhydrous ethanol.
[0033] Preferably, dilute nitric acid is also added to facilitate dissolution of the raw materials.
[0034] The molar ratio of the fluoride to the titanium compound is (0.05-2.2):1, preferably (0.15-1.5):1, more preferably (0.25-0.75):1, such as (0.6-0.7):1. The fluoride is calculated based on the molar amount of the fluorine element, and the titanium compound is calculated based on the molar amount of the titanium element.
[0035] The volume molar ratio of the solvent to the titanium compound is (15-45) mL:0.01 mol, preferably (20-40) mL:0.01 mol, and more preferably (25-35) mL:0.01 mol. The titanium compound is calculated based on the molar amount of the titanium element therein.
[0036] During the preparation of the fluorine-doped titanium dioxide, the reaction temperature is 130-230° C., preferably 150-210° C., more preferably 170-190° C., and the reaction time is 12-32 h, preferably 15-28 h, more preferably 18-24 h.
[0037] The photocatalytic performance of the product is good when the reaction temperature is between 150 and 210°C, and the photocatalytic performance of the product is optimal at 180°C.
[0038] When the reaction temperature is 180°C, the solvent thermal reaction time is 12-15h, and the photocatalytic performance of the product is lower than that of 15-28h, among which the photocatalytic performance of 18-24h is the best.
[0039] The calcination temperature is 400-500°C, preferably 420-480°C, more preferably 440-460°C, and the calcination time is 1.5-4.5h, preferably 2-4h, more preferably 2.5-3.5h.
[0040] When the calcination temperature is 400-420° C., the photocatalytic activity of the product is lower than that of the product calcined at 420-480° C. Among them, the product synthesized at a calcination temperature of 450° C. has the best photocatalytic performance.
[0041] When the calcination temperature is 450℃, the photocatalytic activity of the product obtained by calcination time of 1.5-2h is lower than that of the product obtained by calcination time of 2-4h. Among them, the photocatalytic performance of the synthetic product obtained by calcination for 3h is the best.
[0042] The bismuth-containing compound is a water-soluble or acid-soluble bismuth-containing compound, preferably a water-soluble bismuth salt, more preferably one or more of bismuth nitrate, bismuth nitrate pentahydrate and ammonium bismuth citrate, such as bismuth nitrate and / or bismuth nitrate pentahydrate.
[0043] The mass molar ratio of the fluorine-doped titanium dioxide to the bismuth-containing compound is 1 g:(0.005-0.40) mol, preferably 1 g:(0.01-0.30) mol, and more preferably 1 g:(0.015-0.20) mol.
[0044] The mass volume ratio of the fluorine-doped titanium dioxide to water is 0.1 g:(4-28) mL, preferably 0.1 g:(6-20) mL, and more preferably 0.1 g:(8-12) mL.
[0045] In the method, a surfactant is also added, which is selected from one or more of alcohols, alkyl quaternary ammonium salts, polyethylene glycol (PEG) and polyvinyl pyrrolidone (PVP), preferably selected from one or more of ethanol, glycerol, polyethylene glycol (PEG) and polyvinyl pyrrolidone (PVP), and more preferably polyvinyl pyrrolidone (PVP).
[0046] The mass ratio of the surfactant to the fluorine-doped titanium dioxide is 0.03:(0.01-0.2), preferably 0.03:(0.05-0.15), and more preferably 0.03:(0.1-0.12).
[0047] In the method, an aqueous solution of a mineralizer is also added, which is selected from one or more alkaline substances, preferably one or more alkali metal hydroxides, and more preferably NaOH and / or KOH.
[0048] The concentration of the aqueous mineralizer solution is 2.5-7.5 mol / L, preferably 3.5-6.5 mol / L, and more preferably 4.5-5.5 mol / L.
[0049] The molar mass ratio of the mineralizer to fluorine-doped titanium dioxide is (0.1-0.4) mol:0.1 g, preferably (0.15-0.35) mol:0.1 g, and more preferably (0.2-0.3) mol:0.1 g.
[0050] The reaction temperature is 130-230°C, preferably 150-210°C, more preferably 170-190°C, and the reaction time is 12-32h, preferably 15-28h, more preferably 18-24h.
[0051] The present invention also provides the use of the nano-fluorine-doped bismuth titanate, which is used as a photocatalyst to degrade organic pollutants, such as methyl orange and / or methylene blue. The degradation efficiency of the nano-fluorine-doped bismuth titanate on organic pollutants is higher than 90%.
[0052] The preparation method of the nano-fluorine-doped bismuth titanate provided by the present invention is simple, the process method is simple in practical application, and it is easy to obtain. The obtained nano-fluorine-doped bismuth titanate has good photocatalytic performance and can be used repeatedly, which effectively prolongs the service life of the photocatalyst, reduces the maintenance cost of actual organic polluted wastewater, prolongs the maintenance cycle, and is conducive to application in actual sewage treatment.
[0053] Example
[0054] Example 1
[0055] Add 0.1g, 0.25g and 0.8g of ammonium fluoride to 30mL of anhydrous ethanol respectively. After stirring for 30 minutes, add 3.4g of tetrabutyl titanate respectively. Slowly add 1mL of nitric acid (concentration of 65wt%) and 1mL of deionized water during stirring. The mixed solution is placed in a 50mL polytetrafluoroethylene liner and sealed, heated to 180℃ in an oven, and reacted for 20h. The product after the reaction is repeatedly washed with deionized water and ethanol for 3 times, and dried at 60℃ for 15h. After cooling to room temperature, grind into powder. In a muffle furnace, heat to 450℃ at a heating rate of 5℃ / min, and calcine at 450℃ for 180min. The precursors 0.1F-TiO2, 0.25F-TiO2, and 0.8F-TiO2 are obtained respectively.
[0056] Take 0.1g of the precursors 0.1F-TiO2, 0.25F-TiO2, and 0.8F-TiO2 and add them to 10mL of deionized water, ultrasonicate for 20min, add 0.03g of polyvinyl pyrrolidone PVP and 0.84g of bismuth nitrate pentahydrate, and transfer to a 100mL polytetrafluoroethylene liner. Add 50mL of 5mol / L NaOH solution and stir continuously at room temperature for 60min. Put it in an oven and heat it at 180℃ for 18h. After cooling to room temperature, wash the samples twice with deionized water and anhydrous ethanol, respectively, and dry them at 60℃ for 12h. Nano-fluorine-doped bismuth titanate 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO were obtained respectively.
[0057] Comparative Example
[0058] Comparative Example 1
[0059] Add 3.4 g of tetrabutyl titanate to 30 mL of anhydrous ethanol. Slowly add 1 mL of nitric acid (concentration of 68 wt%) and 1 mL of deionized water during stirring. The mixed solution was placed in a 50 mL polytetrafluoroethylene liner, heated to 180 ° C in an oven, and reacted for 20 hours. The product after the reaction was repeatedly washed with deionized water and ethanol for 3 times, and dried at 60 ° C for 15 hours. After cooling to room temperature, it was ground into powder. In a muffle furnace, the temperature was raised to 450 ° C at a heating rate of 5 ° C / min, and calcined at 450 ° C for 180 minutes. The precursor TiO2 was obtained.
[0060] Take 0.1g of precursor TiO2 and ultrasonicate it in 10mL of deionized water for 20min, add 0.03g of polyvinyl pyrrolidone PVP and 0.84g of bismuth nitrate pentahydrate, and transfer it to a 100mL polytetrafluoroethylene liner. Add 50mL of 5mol / LNaOH solution and stir continuously at room temperature for 60min. Put it in an oven and heat it at 180℃ for 18h. After cooling to room temperature, wash the sample twice with deionized water and anhydrous ethanol, respectively, and dry it at 60℃ for 12h. Obtain nano bismuth titanate BTO.
[0061] Experimental example
[0062] Experimental Example 1
[0063] X-ray diffraction (XRD) tests were performed on the TiO2 prepared in Comparative Example 1 and the 0.25F-TiO2 and 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO prepared in Example 1.
[0064] The XRD spectrum of TiO2 is as follows Figure 1As shown in (a), 25.31°, 36.96°, 37.78°, 48.02°, 53.89°, 55.13°, 62.63°, 68.72°, 70.38°, and 75.01° correspond to crystal planes (101), (103), (004), (200), (105), (211), (204), (116), (220), and (215), respectively, which are consistent with the standard XRD pattern of TiO2 (PDF#71-1166), and no impurity peaks are generated, indicating that TiO2 is successfully prepared by this synthesis method.
[0065] From the XRD pattern of 0.25F-TiO2 ( Figure 1 (a)) It can be seen that the intensity of its XRD diffraction peak has decreased, which is speculated to be due to the decrease in the crystallinity of 0.25F-TiO2 caused by the doping of F. It can be seen from the local enlarged view of the XRD spectrum of 0.25F-TiO2 ( Figure 1 (b)), the diffraction peak of 0.25F-TiO2 shifts to a lower angle. - The radius is 0.133nm, O 2- The radius is 0.132nm. - Enter the TiO2 lattice and replace O 2- , causing the lattice to expand, which is manifested as a shift to a lower angle in the XRD pattern.
[0066] The obtained 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO have the same spectrum as BTO (JCPDF: 35-0795), as shown in Figure 2 As shown in the figure, there is no impurity peak, indicating that the 0.1F-BTO, 0.25F-BTO and 0.8F-BTO prepared by the present invention have high crystal phase purity. At the same time, no obvious deviation behavior of the diffraction peak of XRD was found.
[0067] Experimental Example 2
[0068] Raman tests were performed on the BTO prepared in Comparative Example 1, 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO prepared in Example 1. Figure 3 shown.
[0069] 250-300cm -1 The peak at 250-300 cm-1 belongs to the [TiO6] octahedral vibration band. Compared with BTO, 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO have a peak at 250-300 cm-1. -1 The peak at is shifted due to the change in the coordination environment of the [TiO6] octahedron. This phenomenon indicates that F -Successfully replaced the anions in the bismuth titanate lattice.
[0070] Experimental Example 3
[0071] The TiO2 and BTO prepared in Comparative Example 1 and the 0.1F-TiO2, 0.25F-TiO2, 0.8F-TiO2, 0.1F-BTO, 0.25F-BTO and 0.8F-BTO prepared in Example 1 were tested by scanning electron microscope (SEM). Figure 4 and Figure 5 shown.
[0072] from Figure 4 and Figure 5 It can be seen from the SEM images of TiO2, 0.1F-TiO2, 0.25F-TiO2, and 0.8F-TiO2 that they are composed of small particles aggregated and the size distribution is uniform. As the F doping content increases, the particle size gradually increases. This phenomenon shows that fluorine doping causes the expansion of the lattice, which in turn causes the lattice distortion, and the particles appear to be larger.
[0073] from Figure 4 and Figure 5 It can be seen from the SEM images of BTO, 0.1F-BTO, 0.25F-BTO, and 0.8F-BTO that they are formed by the aggregation of nanosheets. The influence of fluorine doping on the morphology of the precursor TiO2 is relatively large. It may be due to the secondary treatment that the Bi element participates in the bonding of bismuth titanate, thereby weakening the influence of F on the morphology of nano-bismuth titanate. From the XPS test image of 0.25F-BTO ( Figure 6 It can also be seen in (d) that the intensity of the Bi bonding diffraction peak is higher than and covers the intensity of the F1s diffraction peak.
[0074] The BTO prepared in Comparative Example 1 and the 0.25F-TiO2 prepared in Example 1 were tested by transmission scanning electron microscopy (TEM). Figure 6 (a) Figure 6 (b) is a TEM image of BTO, which shows that BTO is a microsphere composed of nanosheets. At the same time, high-resolution transmission electron microscopy (HRTEM) was used to analyze its lattice fringes (such as Figure 6 (c)), 0.27nm corresponds to Bi4Ti3O 12 (200) crystal plane.
[0075] Experimental Example 5
[0076] 50 mg of BTO prepared in Comparative Example 1 and 0.25F-BTO prepared in Example 1 were added to 50 mL of 5 mg / L methyl orange solution, and the above system was placed in the dark and stirred for 30 minutes to obtain a solution to be degraded.
[0077] 4 mL of the solution to be degraded was taken into a centrifuge tube and centrifuged for 5 min at a speed of 8000 r / min, and the supernatant was retained and centrifuged again. After the centrifugation, the supernatant was taken and the initial absorbance A0 was measured using a UV spectrophotometer.
[0078] Turn on the 300W xenon light source, then take a certain amount of the solution to be degraded at regular intervals, and measure the absorbance A of the dye according to the above centrifugation steps. t . Record the experimental data and calculate the degradation efficiency:
[0079] W=C t / C0=A t / A0,
[0080] C t is the concentration of methyl orange in the solution at time t of illumination, C0 is the initial concentration of methyl orange in the solution before the dark reaction, A t is the absorbance of the methyl orange solution at the time of illumination t, and A0 is the absorbance of the methyl orange solution before the dark reaction. The samples after the above photocatalytic test were collected by centrifugation, washed with deionized water and ethanol, and centrifuged three times. The collected catalysts were heated in an oven at 60°C for 12 hours to obtain a dry sample. The above degradation experimental steps were repeated three times.
[0081] from Figure 7 It can be seen that after 60 minutes of illumination, BTO degraded methyl orange by about 21%. With the increase of F content, the degradation efficiency of methyl orange gradually increased. Among them, the degradation efficiency of methyl orange by 0.25F-BTO catalyst reached the maximum value (91%), which was about 4 times that of BTO. However, the excessive fluorine doping content inhibited the degradation effect of photocatalyst on methyl orange.
[0082] like Figure 8 The first-order reaction formula ln(C0 / C)=kt was used to fit the photodegradation kinetics, where C, C0, k and t represent the concentration at time t (mg / L), the initial concentration of the pollutant (mg / L), the first-order kinetic reaction rate constant (min -1 ) and reaction time (min). Among them, the average apparent rate constant of 0.25F-BTO catalyst is the highest, which is 0.01166min -1 , which is 3.9 times that of BTO (0.00296min -1 ). In addition, 0.25F-BTO was recovered.
[0083] like Fig. 9 Under the same conditions, the test found that the photocatalytic activity of 0.25F-BTO did not decrease significantly after three cycles, indicating that the sample has good stability in degradation.
[0084] Experimental Example 6
[0085] The photocatalytic water oxidation reaction was carried out in a closed reactor connected to an all-glass automatic online trace gas analyzer (Lasolar-6A, Beijing Perfectlight). The temperature was maintained at about 30°C, and N2 gas was injected until the reactor was filled with N2. 50 mg of 0.25F-BTO prepared in Example 1 was dispersed in 60 mL of deionized water as a photocatalyst. After being stored in the dark for 0.5 h to allow the water on the surface of the mixture to reach adsorption-desorption equilibrium, the reactor was irradiated with a 300 W xenon lamp (λ>420 nm). During the photocatalytic reaction, the mixture in the reactor was continuously stirred with a magnetic stirrer. The light intensities on the outer surface and bottom of the reactor were 86100 μW / cm 2 and 38700μW / cm 2 At a given time interval (1 h), 1 ml of gas was extracted from the reactor and the product was analyzed using a thermal conductivity detector of a gas chromatograph (Shimadzu, GC-2014). The yield value (mL) was obtained based on the difference in oxygen concentration (the oxygen signal peak was at 490 nm).
[0086] The water oxidation performance of the catalyst was studied under visible light irradiation and without any sacrificial agent. Fig.10 As shown in a, compared with BTO, the oxygen production content of each gram of 0.25F-BTO after 6 hours of illumination reached 16 mmol, which increased the oxygen production rate of the BTO catalyst by about 2.5 times (as shown in Fig.10 b).
[0087] When the hole sacrificial agent HLSA (7.5 mL isopropanol) was added, the oxygen production rate of the system with the hole sacrificial agent decreased by 65% compared with the pure water system, indicating the importance of holes in the photocatalytic water oxidation process.
[0088] The BTO and 0.25F-BTO catalysts produced by photocatalytic hydrolysis and oxygen production were recovered. Under the same reaction conditions, after three cycles of photocatalytic oxygen production, the photocatalytic activity did not show a significant decrease. The conclusion was the same as that of the methyl orange degradation experiment, and the sample showed good cyclic stability in photocatalytic water oxidation. Fig.11 shown.
[0089] Experimental Example 7
[0090] Photoelectrochemical measurements were performed using an electrochemical workstation (CHI660E) with a standard three-electrode system. Ag / AgCl electrode and platinum wire were used as auxiliary electrode and counter electrode, respectively. BTO prepared in Comparative Example 1 and 0.25F-BTO prepared in Example 1 were used as working electrodes (10 mg of the sample was dispersed in 1 mL of ethanol, then dropped onto the ITO glass, and then dried at room temperature for 12 h to form a uniform membrane electrode). The electrolyte was 0.1 mol·L -1 Na2SO4 solution, and the visible light source is 300W Xe lamp.
[0091] Electrochemical impedance spectroscopy (EIS) was collected at an AC amplitude of 0.005 V in the frequency range of 100 kHz to 0.1 Hz. Mott-Schottky curves were collected at a frequency of 500 Hz with an AC potential amplitude of 0.005 V.
[0092] The separation efficiency of photogenerated carriers of the catalyst was studied by photoelectrochemistry (photocurrent and impedance) and surface photovoltaic response. The instantaneous photocurrent density of BTO, 0.1F-BTO, 0.8F-BTO, and 0.25F-BTO as photocatalysts under intermittent simulated sunlight is shown in Figure 2. Fig.12 As shown in (a), the order of photocurrent density is: BTO < 0.1F-BTO < 0.8F-BTO < 0.25F-BTO, among which 0.25F-BTO has the highest photocurrent density, indicating more effective photogenerated carrier separation and transmission efficiency. Fig.12 (b) The Nyquist plot radius of 0.25F-BTO is the smallest, indicating the lowest electrochemical impedance, which means that the photogenerated electron-hole pair separation and transfer resistance of the catalyst is the smallest. In summary, the enhancement of the photocatalytic performance of the sample is due to the improvement of the separation and migration efficiency of photogenerated carriers caused by fluorine doping. In addition, the photocatalyst was characterized by photoluminescence (PL) to study the effect of fluorine doping on the photogenerated electron-hole recombination of the catalyst. Fig.12 (c) When excited by light with an excitation wavelength of 350 nm, the undoped BTO nanosheets have a strong excitation peak, indicating that the photogenerated electrons and holes of BTO have a high recombination rate. However, the excitation peak of the 0.25F-BTO catalyst is reduced to a certain extent and shifted to the blue wave direction, indicating that the recombination of photogenerated carriers can be effectively suppressed by fluorine doping. And the transient fluorescence spectrum is shown in Fig.12 (d) is shown, and the corresponding carrier lifetime is shown in Table 1. The fluorescence lifetime of 0.25F-BTO is τ = 5.93ns, and the fluorescence lifetime of BTO is τ = 3.15ns. This result proves that fluorine doping can prolong the carrier lifetime of the catalyst and is beneficial to improving the photocatalytic activity of 0.25F-BTO.
[0093] The present invention is described in detail above in conjunction with specific embodiments and / or exemplary examples and drawings, but these descriptions cannot be understood as limiting the present invention. Those skilled in the art understand that, without departing from the spirit and scope of the present invention, various equivalent substitutions, modifications or improvements may be made to the technical solution of the present invention and its implementation methods, all of which fall within the scope of the present invention. The scope of protection of the present invention shall be subject to the attached claims.
Claims
1. A nano-fluorine-doped bismuth titanate, which is prepared using fluorine-doped titanium dioxide and a bismuth-containing compound as raw materials in a water solvent under closed heating conditions.
2. A method for preparing nano-fluorine-doped bismuth titanate, It is characterized in that The method uses fluorine-doped titanium dioxide and bismuth-containing compounds as raw materials, and prepares the product in a water solvent under closed heating conditions.
3. The method according to claim 2, It is characterized in that The fluorine-doped titanium dioxide is obtained by adding fluoride and titanium compound into a solvent, heating and reacting under closed conditions, and calcining.
4. The method according to claim 3, It is characterized in that The fluoride is selected from inorganic fluorides, preferably ammonium fluoride; The titanium compound is selected from one or more of titanate compounds and titanate ester compounds, preferably one or more of titanate ester compounds, more preferably one or more of tetrabutyl titanate, tetraisopropyl titanate and tetraethyl titanate.
5. The method according to claim 3, It is characterized in that The solvent is selected from one or more alcohol solvents, preferably selected from alkanols with a carbon number of 1-4, and more preferably one or more of ethanol, propanol, n-butanol and isopropanol.
6. The method according to claim 3, It is characterized in that The molar ratio of the fluoride to the titanium compound is (0.05-2.2):1, preferably (0.15-1.5):1, and more preferably (0.25-0.75):
1.
7. The method according to claim 3, It is characterized in that The reaction temperature is 130-230°C, preferably 150-210°C, more preferably 170-190°C, and the reaction time is 12-32h, preferably 15-28h, more preferably 18-24h; The calcination temperature is 400-500°C, preferably 420-480°C, more preferably 440-460°C, and the calcination time is 1.5-4.5h, preferably 2-4h, more preferably 2.5-3.5h.
8. The method according to claim 2, It is characterized in that The bismuth-containing compound is a water-soluble or acid-soluble bismuth-containing compound, preferably a water-soluble bismuth salt, more preferably one or more of bismuth nitrate, bismuth nitrate pentahydrate and ammonium bismuth citrate. The mass molar ratio of the fluorine-doped titanium dioxide to the bismuth-containing compound is 1 g:(0.005-0.40) mol, preferably 1 g:(0.01-0.30) mol, and more preferably 1 g:(0.015-0.20) mol.
9. The method according to claim 2, It is characterized in that In the method, a surfactant is further added, selected from one or more of alcohols, alkyl quaternary ammonium salts, polyethylene glycol (PEG) and polyvinyl pyrrolidone (PVP). In the method, an aqueous solution of a mineralizer is also added, which is selected from one or more alkaline substances, preferably one or more alkali metal hydroxides. The reaction temperature is 130-230°C, preferably 150-210°C, more preferably 170-190°C, and the reaction time is 12-32h, preferably 15-28h, more preferably 18-24h.
10. Use of nano-fluorine-doped bismuth titanate, It is characterized in that It is used as a photocatalyst to degrade organic pollutants, such as methyl orange and / or methylene blue. The degradation rate of nano-fluorine-doped bismuth titanate on organic pollutants is higher than 90%.